Natural graphite sodium ion battery negative electrode material as well as preparation method and application thereof

Through ball milling, intercalation and oxidation treatment technology, the spacing between graphite layers is expanded, which solves the problems of low sodium storage capacity and safety hazards of graphite in sodium-ion batteries, significantly improves the sodium storage capacity and rate performance of natural graphite, and achieves higher reversible specific capacity and stable cycle performance.

CN118754117APending Publication Date: 2024-10-11CHINA MINMETALS GRP (HEILONGJIANG) GRAPHITE IND CO LTD +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410751657.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing graphite materials have safety hazards and low sodium storage capacity problems in sodium-ion batteries, especially when alkali gold is inserted near 0V, and the insertion of sodium is unstable, resulting in poor manufacturing and performance of sodium-ion batteries.

Method used

Reduce graphite particle size through ball milling, combine intercalation reaction and oxidation layer expansion technology, use ammonium persulfate, sodium persulfate and other oxidants to carry out oxidation reaction, expand the distance between graphite layers, increase sodium storage capacity, and use intercalation agents such as sulfuric acid to Introduce large ion pre-intercalation and build a conductive surface to improve electron transfer and ion transfer efficiency.

Benefits of technology

In ester-based and ether-based electrolytes, the sodium storage capacity and rate performance of natural graphite are significantly improved, achieving higher reversible specific capacity and stable cycle performance, and overcoming the reduction of sodium storage sites and layer spacing caused by calcination treatment Narrowing down the problem.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754117A_ABST
    Figure CN118754117A_ABST
Patent Text Reader

Abstract

The invention provides a natural graphite sodium-ion battery negative electrode material as well as a preparation method and application thereof. The method comprises the following steps: S1, carrying out ball-milling treatment on natural graphite to obtain ball-milled graphite; S2, mixing the ball-milled graphite and an intercalator, and carrying out an intercalation reaction to obtain large ion pre-embedded intercalated graphite; S3, mixing the large ion pre-embedded intercalated graphite, an oxidant and a dispersion liquid to obtain a mixed liquid, and then carrying out an oxidation reaction and post-treatment to obtain the large ion pre-embedded intercalated graphite. The natural graphite sodium ion battery negative electrode material is obtained. Compared with a natural graphite body, the material prepared by the preparation method disclosed by the invention has higher sodium storage capacity and better rate capability in ester-based and ether-based electrolytes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a natural graphite sodium ion battery negative electrode material and a preparation method and application thereof. Background Art

[0002] Over the past three decades, the lithium-ion battery industry has been expanding, primarily due to the growing demand in the portable electronic device market. With the emergence of demand for hybrid electric vehicles, the focus of lithium-ion batteries has shifted to power grids and other large-scale applications, however, the abundance limitations of lithium-containing precursors have created inevitable challenges for industrialization.

[0003] As an alternative, sodium-ion batteries have attracted a great deal of attention because, unlike lithium, sodium is a ubiquitous and abundant element. Sodium-ion batteries were first developed in the late 1980s, almost the same time as lithium-ion batteries, and the recent need for large-scale energy storage for grid applications has revived interest in sodium-ion batteries.

[0004] In the search for secondary batteries to replace lithium-ion batteries, sodium-ion batteries have attracted attention for the following reasons: (i) sodium is abundant, being the fourth most abundant element in the earth's crust; (ii) sodium is low in cost compared to lithium, especially in large-scale power storage applications; and (iii) sodium and lithium have similar chemical properties.

[0005] So far, the application of graphite anode in lithium-ion batteries (LIBs) and sodium-ion batteries (SIBs) has the following problems: (i) the insertion of alkali metals between the layers near 0 V will endanger the safety of the battery; (ii) the lack of a flat platform when sodium is inserted hinders the fabrication of carbon-based commercial sodium-ion batteries.

[0006] The most common negative electrode material for commercial lithium-ion batteries is graphite, which includes artificial graphite and natural graphite, with a capacity of 372mAh / g. However, another alkali metal ion, sodium ion, cannot be inserted into graphite. This is because the sodium-carbon binary compound is unstable, so graphite cannot be used as an active material for sodium-ion batteries. Studies by Doeff et al. show that the sodium product of graphite is NaC70, with a theoretical specific capacity of 31mAh / g. The low specific capacity makes graphite almost unusable in sodium-ion batteries. In order to overcome the shortcomings of graphite, people have conducted a lot of research on alternative negative electrode materials such as amorphous carbon, expanded graphite (EG), and graphene oxide (GO). Related studies have shown that graphene oxide materials have a sufficiently large interlayer spacing (>0.37nm), and the large interlayer spacing can be used for sodium ions to insert into the graphite interlayer, achieving a high graphite sodium storage capacity. By drawing on the interlayer sodium storage mechanism of graphene oxide, the interlayer spacing of graphite materials is expanded, which helps to further improve the sodium storage capacity of graphite. At the same time, graphene oxide expands on the basis of embedding large ionic groups between graphite layers. For example, the Hummer method embeds sulfate ions between graphite layers, introducing sulfur elements. Therefore, large ion pre-embedded graphite will introduce heteroatoms. The doping of heteroatoms not only promotes electron transfer, but also reduces the ion transfer barrier, showing ultrafast discharge performance.

[0007] Hard carbon materials have abundant micropores on the surface and in the bulk phase, which provide abundant sodium storage sites and greatly increase their sodium storage capacity. By learning from the sodium storage mechanism of hard carbon pores, constructing abundant micropores on the surface of graphite may increase the sodium storage capacity of graphite. Summary of the invention

[0008] In order to solve the above-mentioned defects in the prior art, the purpose of the present invention is to provide a natural graphite sodium ion battery negative electrode material and its preparation method and application. Compared with natural graphite body, the material prepared by the present invention has a higher sodium storage capacity and better rate performance in both ester-based and ether-based electrolytes.

[0009] In order to achieve the above object, according to one aspect of the present invention, a method for preparing a natural graphite sodium ion battery negative electrode material is provided, which comprises:

[0010] S1, ball-milling natural graphite to obtain ball-milled graphite;

[0011] S2, mixing the ball-milled graphite and the intercalation agent to perform an intercalation reaction to obtain large ion pre-intercalation graphite;

[0012] S3, mixing the large ion pre-intercalated graphite, the oxidant and the dispersion to obtain a mixed solution, then performing an oxidation reaction, and performing post-treatment to obtain the natural graphite sodium ion battery negative electrode material;

[0013] The oxidant includes one or a combination of two or more of ammonium persulfate, sodium persulfate and potassium chlorate.

[0014] In the preparation method of the present invention, the graphite particle size is reduced by ball milling treatment, and the van der Waals force between graphite layers is weakened, so as to better achieve the intercalation oxidation expansion effect; the large ion pre-intercalation graphite of the graphite layer with weak interlayer van der Waals force is achieved through intercalation reaction; and the expansion of the interlayer spacing is achieved by introducing an oxidant.

[0015] The present invention only includes three main steps: ball milling, intercalation, and oxidation. The process is simple, safe, and low in cost. The preparation method of the present invention does not include a calcination process, and calcination will eliminate a portion of the closed pores formed during the milling process, thereby reducing the sodium storage sites and resulting in a reduction in the sodium storage capacity; calcination will also remove oxygen-containing functional groups during room temperature oxidation, which can effectively increase the interlayer spacing. Therefore, after calcination, the graphite interlayer spacing will be reduced, thereby reducing the sodium storage capacity. The preparation method of the present invention can overcome the above-mentioned defects.

[0016] Preferably, after the intercalation reaction, the large ion pre-intercalation graphite is washed and dried with water.

[0017] Preferably, the natural graphite sodium ion battery negative electrode material is cleaned and dried. When cleaning, preferably, the purpose is to clean the cleaned material to a neutral pH.

[0018] In S3, the dispersion liquid is preferably deionized water, and preferably, the solid content in the mixed liquid is 80%-90%.

[0019] Preferably, in S2 and S3, ultrasound is used to mix the materials, and the ultrasound time is preferably 10 to 60 minutes.

[0020] In some preferred embodiments of the present invention, the ball milling treatment is performed at a rotation speed of 100 to 500 rpm and for a time of 2 to 10 hours.

[0021] Preferably, the ball milling treatment of the present invention is carried out under a protective atmosphere, and the natural graphite and stainless steel balls are added to a ball milling jar according to a certain ball-to-material ratio for ball milling treatment. The ball-to-material ratio is preferably 5 to 15:1. The protective atmosphere is preferably composed of argon and / or nitrogen.

[0022] In some preferred embodiments of the present invention, the intercalation agent includes one or a combination of two or more of sulfuric acid, nitric acid, and perchloric acid. Preferably, the sulfuric acid is concentrated sulfuric acid with a mass concentration of 98%; the nitric acid is fuming nitric acid with a mass concentration of 98%; and the mass concentration of perchloric acid is 70%-72%. The intercalation agent diffuses in the bulk phase, and at the same time introduces non-metallic heteroatom doping, constructs a conductive surface, promotes electron transfer, and reduces the ion transfer barrier, showing good rate performance.

[0023] In some preferred embodiments of the present invention, the mass ratio of the ball-milled graphite to the intercalation agent is 1:1 to 8. According to the preferred amount of the intercalation agent, large ions can be more fully inserted into the graphite interlayer.

[0024] In some preferred embodiments of the present invention, the mass ratio of the large ion pre-intercalated graphite to the oxidant is 1:3-10.

[0025] In some preferred embodiments of the present invention, the temperature of the intercalation reaction is 15-30° C. and the time is 10-30 hours. Through the preferred experimental conditions, the large ions can be more fully inserted into the graphite layers.

[0026] In some preferred embodiments of the present invention, the oxidation reaction is carried out at a temperature of 15-30° C. and for a time of 10 to 30 hours.

[0027] Preferably, the present invention can prepare a graphite negative electrode material with a high sodium storage capacity at room temperature; the time for intercalation and oxidation is controlled to be an appropriate time, respectively. When the time is too short, the degree of intercalation or oxidation will be insufficient, and when the time is too long, the graphite will contain too many oxygen-containing functional groups, thereby reducing the conductivity and rate performance of the prepared negative electrode material.

[0028] In another aspect of the present invention, a natural graphite sodium ion battery negative electrode material obtained according to the above-mentioned preparation method is provided.

[0029] In another aspect of the present invention, a lithium ion battery is provided, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the negative electrode comprises the above-mentioned natural graphite sodium ion battery negative electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a scanning electron microscope (SEM) image of the natural graphite sodium ion battery negative electrode material in Example 1.

[0031] Figure 2 This is a scanning electron microscope (SEM) image of the natural graphite sodium ion battery negative electrode material in Example 1.

[0032] Figure 3 This is a scanning electron microscope (SEM) image of the natural graphite sodium ion battery negative electrode material in Example 1.

[0033] Figure 4 This is the EDS image of the natural graphite sodium ion battery negative electrode material in Example 1.

[0034] Figure 5This is the first week charge and discharge curve of the natural graphite sodium ion battery negative electrode material in Example 1 in an ester / ether electrolyte at a current density of 0.1C (1C=300mAh / g) in a voltage window of 0.005V to 2.5V.

[0035] Figure 6 This is the cycle data obtained by testing the natural graphite sodium ion battery negative electrode material in Example 1 at a current density of 0.1C in a voltage window of 0.005V to 2.5V.

[0036] Figure 7 This is a scanning electron microscope (SEM) image of the natural graphite sodium ion battery negative electrode material in Example 2.

[0037] Figure 8 The first week charge and discharge curve of the natural graphite sodium ion battery negative electrode material in Example 2 at a current density of 0.1C (1C=300mAh / g) in a voltage window of 0.005V to 2.5V.

[0038] Fig. 9 This is the cycle data obtained by testing the natural graphite sodium ion battery negative electrode material in Example 2 at a current density of 0.1C in a voltage window of 0.005V to 2.5V.

[0039] Fig.10 This is a scanning electron microscope (SEM) image of graphite in Comparative Example 1.

[0040] Fig.11 This is the first week charge and discharge curve of graphite in comparative example 1 at a current density of 0.1C (1C=300mAh / g) in a voltage window of 0.005V to 2.5V.

[0041] Fig.12 This is the cycle data of graphite in comparative example 1, obtained by a 0.1C current density test in a voltage window of 0.005V to 2.5V. DETAILED DESCRIPTION

[0042] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.

[0043] In the following examples, battery assembly and testing were performed according to the following method:

[0044] The final product obtained in the embodiment: Super P: polyacrylic acid mixed in a mass ratio of 8:1:1 was coated on aluminum foil to make a positive electrode sheet, a metal sodium sheet was used as the negative electrode, Whatman glass fiber was used as the diaphragm, and a 1M NaPF6 diethylene glycol dimethyl ether solution was used as the electrolyte (wherein the solvent was diethylene glycol dimethyl ether and the solute was NaPF6), and a button battery was assembled in an argon glove box. The battery was then left to stand for 8 hours and then cycled at a rate of 0.1C-10C, with a test voltage range of 0.005V-2.5V, and a 1C current density of 300mA / g.

[0045] Example 1

[0046] A method for preparing a natural graphite sodium ion battery negative electrode material.

[0047] Weigh 1 g of natural flake graphite, mix it with stainless steel balls at a ball-to-material ratio of 10:1, add it into a ball mill, pass argon for 30 minutes, and mill it in a planetary ball mill at 500 rpm for 300 minutes to collect the ball-milled graphite.

[0048] 1 g of ball-milled graphite was mixed with 98% concentrated sulfuric acid in a mass ratio of 1:5, ultrasonicated for 20 min, and stirred for 10 h to obtain sulfur-doped macroion pre-intercalated graphite.

[0049] The large ion pre-intercalated graphite was washed with deionized water until neutral and dried in vacuum at 80°C for 12 h.

[0050] The materials in the above step were mixed with ammonium persulfate in a mass ratio of 1:5, dissolved in 2 ml of deionized water, ultrasonicated for 30 min, and stirred for reaction for 24 h.

[0051] The material collected after the reaction was washed with deionized water until neutral, and then dried at 80° C. for 12 h to obtain a natural graphite sodium ion battery negative electrode material.

[0052] The SEM test results of natural graphite sodium ion battery negative electrode material are as follows Figure 1 , Figure 2 , Figure 3 As shown in Figure 2, it can be seen that the prepared natural graphite sodium ion battery negative electrode material has a loose and porous body phase and an irregular and uneven surface. From SEM, it can be seen that the graphite structure after oxidation expansion is sparse and has many sodium storage sites.

[0053] EDS test results of natural graphite sodium ion battery negative electrode materials are as follows Figure 4 As shown in the figure, it can be seen that the S element is evenly dispersed on the graphite, which indicates that the sulfate ions are successfully inserted into the graphite interlayer.

[0054] Electrochemical data of natural graphite sodium ion battery negative electrode materials such as Figure 5 , Figure 6 As shown. Compared with the theoretical specific capacity of natural graphite in ester-based electrolyte of only 34 mAh / g, the natural graphite sodium ion battery negative electrode material prepared by the present invention greatly improves the reversible specific capacity. In the first cycle of 0.1C, the charging specific capacity is as high as 220.33 mAh / g, but the first cycle coulomb efficiency is low, only 76.74%. At 1C rate, after activation, the reversible specific capacity of the prepared natural graphite sodium ion battery negative electrode material continues to rise. After 100 cycles, the specific capacity rises to 210 mAh / g, and the cycle performance is stable, and the cycle coulomb efficiency is close to 100%.

[0055] Example 2

[0056] A method for preparing a natural graphite sodium ion battery negative electrode material.

[0057] Weigh 1 g of natural flake graphite, mix it with stainless steel balls at a ball-to-material ratio of 10:1, add it into a ball mill, pass argon for 30 minutes, and mill it in a planetary ball mill at 500 rpm for 150 minutes to collect the ball-milled graphite.

[0058] 1 g of ball-milled graphite was mixed with 98% concentrated sulfuric acid in a mass ratio of 1:5, ultrasonicated for 20 min, and stirred for 10 h to obtain large ion pre-intercalated graphite.

[0059] The large ion pre-intercalated graphite was washed with deionized water until neutral and dried in vacuum at 80°C for 12 h.

[0060] The materials in the above step were mixed with sodium persulfate in a mass ratio of 1:5, dissolved in 2 ml of deionized water, ultrasonicated for 30 min, and stirred for reaction for 24 h.

[0061] The material collected after the reaction was washed with deionized water until neutral, and then dried at 80° C. for 12 h to obtain a natural graphite sodium ion battery negative electrode material.

[0062] Figure 7 This is a scanning electron microscope (SEM) image of the expanded graphite in Example 2. It can be seen that the prepared expanded graphite has a loose structure, which is conducive to sodium storage. Figure 8 , Fig. 9 The electrochemical performance data of the expanded graphite in Example 2. Its first-week reversible capacity is 191.48 mAh / g, which is greatly improved compared with natural graphite. However, due to the increase of defects caused by intercalation expansion, the first-week coulombic efficiency is very low, only 58.90%, resulting in a relatively low reversible specific capacity. Fig. 9In the 1C cycle of the expanded graphite material in Example 2, as the number of cycles increases, the electrode material is activated and the reversible specific capacity gradually increases. When the cycle reaches 165 cycles, the specific capacity increases to 198 mAh / g.

[0063] Comparative Example 1

[0064] The preparation method of the graphite material without intercalation treatment is as follows.

[0065] Weigh 1 g of natural flake graphite, mix it with stainless steel balls at a ball-to-material ratio of 10:1, add it into a ball mill, pass argon for 30 minutes, and mill it in a planetary ball mill at 500 rpm for 150 minutes to collect the ball-milled graphite.

[0066] The material collected after the reaction was washed with deionized water until neutral, and then dried at 80° C. for 12 h to obtain a ball-milled graphite material.

[0067] Fig.10 This is a scanning electron microscope (SEM) image of the ball-milled graphite of Comparative Example 1. It can be seen that compared with the intercalated oxidatively expanded graphite, its structure is not loose and its particle size distribution is not uniform. Fig.11 , Fig.12 This is a graph showing the electrochemical performance of ball-milled graphite. Fig.11 , its first-week reversible capacity is 194.19 mAh / g, but its first-week coulombic efficiency is 74.54%. Fig.12 Compared with expanded graphite, the specific capacity of ball-milled graphite does not increase during the cycle, and its 1C cycle specific capacity is significantly lower than that of expanded graphite. After 197 cycles, its specific capacity is only about 130 mAh / g, and the capacity retention rate is about 83%.

Claims

1. A method for preparing a natural graphite sodium ion battery negative electrode material, characterized in that: include: S1, ball-milling natural graphite to obtain ball-milled graphite; S2, mixing the ball-milled graphite and the intercalation agent to perform an intercalation reaction to obtain large ion pre-intercalation graphite; S3, mixing the large ion pre-intercalated graphite, the oxidant and the dispersion to obtain a mixed solution, then performing an oxidation reaction, and performing post-treatment to obtain the natural graphite sodium ion battery negative electrode material; The oxidant includes one or a combination of two or more of ammonium persulfate, sodium persulfate and potassium chlorate.

2. The preparation method according to claim 1, characterized in that: The ball milling process is performed at a rotation speed of 100 to 500 rpm and for a time of 2 to 10 hours.

3. The preparation method according to claim 1, characterized in that: The intercalant includes one or a combination of two or more of sulfuric acid, nitric acid and perchloric acid.

4. The preparation method according to claim 1, characterized in that: The ball milling treatment is performed under a protective atmosphere.

5. The preparation method according to claim 1, characterized in that: The mass ratio of the ball-milled graphite to the intercalation agent is 1:1-8.

6. The preparation method according to claim 1, characterized in that: The mass ratio of the large ion pre-intercalation graphite to the oxidant is 1:3-10.

7. The preparation method according to claim 1, characterized in that: The temperature of the intercalation reaction is 15-30° C. and the time is 10-30 hours.

8. The preparation method according to claim 1, characterized in that: The temperature of the oxidation reaction is 15-30°C and the time is 10-30h.

9. A natural graphite sodium ion battery negative electrode material obtained by the preparation method according to any one of claims 1 to 8.

10. A lithium ion battery comprising a positive electrode, a negative electrode, a separator and an electrolyte, characterized in that: The negative electrode comprises the natural graphite sodium ion battery negative electrode material according to claim 9.

Citation Information

Patent Citations

  • Preparation method of expandable graphite

    CN103145119A

  • Preparation method of expandable microcrystalline graphite

    CN107572515A

  • Preparation method of graphite oxide capable of being washed directly

    CN108640111A

  • Graphene oxide preparation method with controllable inter-layer spacing

    CN109607526A

  • Method of preparing expanded graphite from battery graphite negative electrode

    CN110797534A