Comprehensive utilization method of BOE waste liquid
By adjusting the pH value and multi-step processing of BOE waste liquid, magnesium fluoride and ammonium sulfate are prepared, which solves the problems of high BOE waste liquid treatment cost and unutilized resources in the existing technology, and achieves efficient and environmentally friendly resource recovery.
Patent Information
- Application Number
- CN202410991926.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-11
AI Technical Summary
Existing BOE waste liquid treatment methods are high in cost, pollute, and fail to effectively utilize resources, failing to maximize the use of resources.
By adjusting the first and second pH values of BOE waste liquid, combined with magnesium salts, calcium-containing fluoride removers and carbonates, magnesium fluoride and ammonium sulfate are prepared respectively to achieve resource recycling.
It reduces the cost of equipment and chemicals, improves the purity and recovery rate of the product, maximizes the utilization of resources, and the process is simple and environmentally friendly.
Smart Images

Figure CN118754172A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waste liquid recovery, and in particular to a comprehensive utilization method of BOE waste liquid. Background Art
[0002] BOE etching solution, also known as buffered oxide etching solution, is mainly composed of hydrofluoric acid and ammonium fluoride mixed in a certain proportion, such as a 49% hydrofluoric acid aqueous solution and a 40% ammonium fluoride aqueous solution mixed in a volume ratio of 1:6. It is commonly used in the etching process in the manufacturing process of semiconductors and liquid crystal displays. HF is the main etching component in BOE etching solution, and NH4F is used as a buffer component. NH4F is used to fix H + concentration to maintain a certain etching rate. + The consumption of NH4F, NHHF2 and HF results in the etching speed failing to meet the requirement, thus generating BOE waste liquid. Therefore, the main components of BOE waste liquid include NH4F, NHHF2 and HF, which are hazardous wastes and need to be harmlessly treated.
[0003] At present, the common treatment method of BOE waste liquid includes adding lime or slaked lime to react and generate calcium fluoride and ammonia water, and the calcium fluoride is landfilled harmlessly as sludge. However, this method has high disposal cost, large pollution, and does not achieve effective utilization of resources. For example, CN114132953A discloses a system and preparation method for preparing high-purity calcium fluoride using BOE waste liquid. In this preparation method, waste BOE is reacted with calcium salt. Although calcium fluoride products can be prepared, the ammonium fluoride therein is not effectively utilized, and the disposal process is complicated and the disposal cost is high.
[0004] Therefore, providing a comprehensive utilization method for BOE waste liquid, so as to harmlessly treat the BOE waste liquid and maximize resource utilization and reduce disposal costs, is a technical problem that needs to be solved in the current field. Summary of the invention
[0005] In view of the above problems, the purpose of the present invention is to provide a comprehensive utilization method of BOE waste liquid. Compared with the prior art, the comprehensive utilization method provided by the present invention can utilize BOE waste liquid to prepare products such as magnesium fluoride and ammonium sulfate, and the process is simple, which can reduce the equipment investment cost and the reagent cost, is environmentally friendly, and is conducive to industrial application.
[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0007] The present invention provides a comprehensive utilization method of BOE waste liquid, which comprises the following steps:
[0008] (1) adjusting the BOE waste liquid to a first pH value to obtain a first pH-adjusted liquid, then adding a magnesium salt to the first pH-adjusted liquid until no precipitation is precipitated, then performing solid-liquid separation to obtain a filter cake and a filtrate, the filter cake is sequentially washed and dried to obtain a magnesium fluoride product, and the filtrate is mixed with the washed liquid obtained by washing to obtain a precipitated liquid;
[0009] (2) adding a calcium-containing defluorinating agent to the precipitated liquid obtained in step (1) to perform defluorination treatment, and then performing solid-liquid separation to obtain a defluorinated liquid;
[0010] (3) adding carbonate to the defluorinated liquid obtained in step (2) to perform decalcification treatment, and then performing solid-liquid separation to obtain a decalcified liquid;
[0011] (4) The decalcified liquid obtained in step (3) is subjected to a second pH adjustment, and then concentrated, cooled, and solid-liquid separated in sequence to obtain an ammonium sulfate product.
[0012] In the comprehensive utilization method provided by the present invention, components such as hydrogen fluoride, ammonium fluoride and ammonium bifluoride in BOE waste liquid are recycled and utilized as resources, and products such as magnesium fluoride and ammonium sulfate can be prepared. Magnesium fluoride is a flux for manufacturing ceramics, glass and smelting metals such as magnesium and aluminum, and a coating for lenses and filters in optical instruments. Ammonium sulfate is an excellent nitrogen fertilizer and can also be used as an auxiliary agent for extracting rare earths and an electroplating auxiliary agent, both of which have wide applications. In the comprehensive utilization method provided by the present invention, firstly, according to the hydrogen ion concentration in the BOE waste liquid, a regulator is added to adjust the first pH value to meet the requirements of magnesium fluoride precipitation, and a magnesium salt is added to obtain a filter cake containing magnesium fluoride, and then a magnesium fluoride product is obtained, and a small amount of unprecipitated fluoride ions and ammonium ions are recovered by mixing the filtrate and the washing liquid of the filter cake; then, by adding a calcium-containing defluorinating agent to the precipitated liquid, the remaining fluoride ions can be precipitated in the form of calcium fluoride to obtain a defluorinated liquid; then, carbonate is used to remove the calcium ions contained in the defluorinated liquid, and then a second pH value is adjusted to facilitate the subsequent precipitation of ammonium sulfate to obtain an ammonium sulfate product, thereby realizing the maximum recycling of BOE waste liquid resources, and the obtained product has a high purity and recovery rate.
[0013] In the present invention, the washing liquid used in the washing is generally water. For example, the water removed by concentration in step (4) can be used to achieve the recycling of water resources.
[0014] Preferably, the BOE waste liquid in step (1) contains 0.1-5% hydrogen fluoride, for example, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, but is not limited to the listed values, and other values not listed in the numerical range are also applicable; 5-25% ammonium fluoride, for example, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13% , 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24% or 25%, but not limited to the listed values, and other values not listed in the numerical range are also applicable; 1-15% ammonium bifluoride, for example, can be 1%, 2%, 4%, 6%, 8%, 10%, 12%, 14% or 15%, but not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0015] Preferably, the pH value of the BOE waste liquid is less than 2, for example, it may be 1.9, 1.8, 1.7, 1.6 or 1.5, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0016] Preferably, the regulator used for adjusting the first pH value in step (1) comprises magnesium hydroxide.
[0017] Preferably, the endpoint pH value of the first pH adjustment is 6-7, for example, 6, 6.1, 6.2, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9 or 7, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0018] Preferably, the magnesium salt in step (1) comprises magnesium sulfate.
[0019] Preferably, the molar ratio of the fluorine element in the liquid to the magnesium element in the magnesium salt after the first pH value is adjusted is 2:(1-1.5), for example, it can be 2:1, 2:1.1, 2:1.2, 2:1.3, 2:1.4 or 2:1.5, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] In the present invention, by preferably controlling the molar ratio of the fluorine element in the liquid after the first pH value adjustment to the magnesium element in the magnesium salt, it is possible to ensure that the fluorine element and the magnesium element are fully combined, thereby ensuring the fluorine removal effect while not wasting reagents.
[0021] Preferably, the magnesium salt is added in the form of a solution.
[0022] In the present invention, the water used to prepare the magnesium salt solution can be the water removed by concentration in step (4), thereby realizing the recycling of water resources.
[0023] Preferably, the concentration of magnesium ions in the solution is 2.5-4.5 mol / L, for example, it can be 2.5 mol / L, 2.6 mol / L, 2.8 mol / L, 3 mol / L, 3.2 mol / L, 3.4 mol / L, 3.6 mol / L, 3.8 mol / L, 4 mol / L, 4.2 mol / L, 4.4 mol / L or 4.5 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0024] Preferably, the magnesium salt is stirred after being added.
[0025] Preferably, the stirring time after the addition of the magnesium salt is 0.5-1 h, for example, 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h or 1 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] Preferably, the calcium-containing defluoridating agent in step (2) comprises calcium hydroxide.
[0027] Preferably, the molar ratio of the fluorine element in the post-precipitation liquid to the calcium element in the calcium-containing defluorinating agent is 2:(1-1.2), for example, it can be 2:1, 2:1.02, 2:1.04, 2:1.06, 2:1.08, 2:1.1, 2:1.12, 2:1.14, 2:1.16, 2:1.18 or 2:1.2, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] In the present invention, by preferably controlling the molar ratio of fluorine in the post-precipitation liquid to calcium in the calcium-containing defluorinating agent, it is possible to ensure that fluorine and magnesium are fully combined, thereby ensuring the fluorine removal effect while not wasting the agent.
[0029] Preferably, the calcium-containing defluoridating agent is stirred after being added.
[0030] Preferably, the stirring time after the calcium-containing defluoridating agent is added is 10-30 min, for example, it can be 10 min, 12 min, 14 min, 16 min, 18 min, 20 min, 22 min, 24 min, 26 min, 28 min or 30 min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0031] Preferably, the carbonate in step (3) comprises sodium carbonate.
[0032] Preferably, the molar ratio of calcium element in the defluorinated liquid to carbonate ion in carbonate is 1:(1-1.5), for example, it can be 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4 or 1:1.5, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] In the present invention, by preferably controlling the molar ratio of calcium element in the defluorinated liquid to carbonate ion in carbonate, it is possible to ensure that calcium element and carbonate ion are fully combined, thereby ensuring the calcium ion removal effect without wasting reagents and ensuring that too much sodium carbonate remains, otherwise the quality of the ammonium sulfate product will be affected.
[0034] Preferably, the carbonate is stirred after being added.
[0035] Preferably, the stirring time after the addition of the carbonate is 0.2-1h, for example, it can be 0.2h, 0.3h, 0.4h, 0.5h, 0.6h, 0.7h, 0.8h, 0.9h or 1h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0036] Preferably, the regulator used for adjusting the second pH value in step (4) includes sulfuric acid.
[0037] In the present invention, the source of the sulfuric acid used for the second pH value adjustment is not particularly limited, for example, it can be relatively pure waste sulfuric acid produced by semiconductor manufacturers, wherein the mass concentration of the sulfuric acid is 48-55%, TOC is less than 100ppm, and there is no heavy metal.
[0038] Preferably, the endpoint pH value of the second pH adjustment is 4.5-5.5, for example, it can be 4.5, 4.6, 4.7, 4.8, 4.9, 5, 5.1, 5.2, 5.3, 5.4 or 5.5, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0039] In the present invention, the endpoint pH value of the second pH value adjustment is preferably controlled to ensure that the ammonium sulfate product stably reaches the standard.
[0040] Preferably, the concentration method in step (4) includes distillation concentration.
[0041] Preferably, the pressure of the distillation and concentration is -0.05 to -0.1 MPa, for example, it can be -0.05 MPa, -0.06 MPa, -0.07 MPa, -0.08 MPa, -0.09 MPa or -0.1 MPa, but is not limited to the listed values. Other unlisted values within the numerical range are also applicable. The above pressure range refers to absolute pressure.
[0042] Preferably, the temperature of the distillation and concentration is 80-95°C, for example, it can be 80°C, 82°C, 84°C, 86°C, 88°C, 90°C, 92°C, 94°C or 95°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0043] Preferably, the endpoint of the concentration is that the volume of the crystalline solid accounts for 1 / 3 to 1 / 2 of the total volume, for example, it can be 0.34, 0.36, 0.38, 0.40, 0.42, 0.44, 0.46, 0.48 or 0.5, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0044] Preferably, the terminal temperature of the cooling is 25-45°C, for example, it can be 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, 32°C, 34°C, 36°C, 38°C, 40°C, 42°C, 44°C or 45°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0045] Preferably, the solid-liquid separation method includes filtration or centrifugation.
[0046] Preferably, the filtering method includes pressure filtration or suction filtration.
[0047] In the present invention, the solid-liquid separation method in steps (1) to (3) can be, for example, filter press separation or suction filtration separation, and the solid-liquid separation method in step (4) can be, for example, centrifugal separation. The centrifugal water after centrifugal separation in step (4) can be returned to the concentration step for further concentration, thereby forming a material cycle.
[0048] As a preferred technical solution of the present invention, the comprehensive utilization method comprises the following steps:
[0049] (1) The BOE waste liquid is subjected to a first pH adjustment using magnesium hydroxide to an end point pH value of 6-7 to obtain a first pH adjusted liquid, and then magnesium sulfate is added to the first pH adjusted liquid until no precipitation is precipitated, the molar ratio of the fluorine element in the first pH adjusted liquid to the magnesium element in the magnesium sulfate is 2:(1-1.5), the magnesium sulfate is added in the form of a solution, the concentration of magnesium ions in the solution is 2.5-4.5 mol / L, the magnesium sulfate is stirred for 0.5-1h after being added, and then the solid-liquid separation is performed to obtain a filter cake and a filtrate, the filter cake is sequentially washed and dried to obtain a magnesium fluoride product, the filtrate is mixed with the washed liquid obtained by washing to obtain a precipitated liquid, the BOE waste liquid contains 0.1-5% hydrogen fluoride, 5-25% ammonium fluoride, and 1-15% ammonium bifluoride, and the pH value of the BOE waste liquid is less than 2;
[0050] (2) adding calcium hydroxide to the precipitated liquid obtained in step (1) for defluorination treatment, wherein the molar ratio of the fluorine element in the precipitated liquid to the calcium element in the calcium hydroxide is 2:(1-1.2), stirring for 10-30 minutes after the calcium hydroxide is added, and then solid-liquid separation is performed to obtain a defluorinated liquid;
[0051] (3) adding sodium carbonate to the defluorinated liquid obtained in step (2) for decalcification, wherein the molar ratio of calcium element in the defluorinated liquid to carbonate ion in sodium carbonate is 1:(1-1.5), stirring for 0.2-1h after adding sodium carbonate, and then separating the solid and liquid to obtain a decalcified liquid;
[0052] (4) The decalcified liquid obtained in step (3) is adjusted to a second pH value of 4.5-5.5 using sulfuric acid, and then distilled and concentrated at a pressure of -0.05 to -0.1 MPa and a temperature of 80-95° C. until the volume of the crystalline solid accounts for 1 / 3 to 1 / 2 of the total volume, and then cooled to 25-45° C., followed by solid-liquid separation to obtain an ammonium sulfate product.
[0053] Compared with the prior art, the present invention has the following beneficial effects:
[0054] (1) In the comprehensive utilization method provided by the present invention, the main components such as hydrogen fluoride, ammonium fluoride and ammonium bifluoride in BOE waste liquid are recycled to obtain products such as magnesium fluoride and ammonium sulfate. The obtained products have high purity and yield. Under optimal conditions, the purity of the magnesium fluoride product can reach more than 97%, the recovery rate of the F element can reach more than 98%, the nitrogen content of the ammonium sulfate can reach more than 21%, and the recovery rate of the N element can reach more than 99%, so as to maximize the utilization of resources.
[0055] (2) In the comprehensive utilization method provided by the present invention, no highly toxic chemicals are added during the recovery process, the operation is simple, the skill requirements for workers are reduced, the cost of adding reagents, the filling cost of solid waste and the equipment investment cost are reduced, and the waste discharge to the environment is reduced, which has economic and environmental benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 It is a schematic flow chart of the comprehensive utilization method described in Example 1 of the present invention. DETAILED DESCRIPTION
[0057] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0058] Example 1
[0059] This embodiment provides a comprehensive utilization method of BOE waste liquid, such as Figure 1 As shown, the comprehensive utilization method comprises the following steps:
[0060] (1) 500 mL of BOE waste liquid (containing 1% hydrogen fluoride, 5% ammonium fluoride, 1% ammonium bifluoride, and a pH value of 1) is subjected to a first pH adjustment using magnesium hydroxide to an end point pH value of 6.5 to obtain a first pH-adjusted liquid, and then a 3 mol / L magnesium sulfate solution (added according to a molar ratio of fluorine element to magnesium element of 2:1.2) is added to the first pH-adjusted liquid until no precipitation is precipitated, and the magnesium sulfate is stirred for 0.6 h after being added, and then filtered to obtain a filter cake and a filtrate, and the filter cake is washed and dried in turn to obtain a magnesium fluoride product, and the filtrate is mixed with the washed liquid obtained by washing to obtain 500 mL of precipitated liquid;
[0061] (2) adding calcium hydroxide (added at a molar ratio of fluorine to calcium of 2:1.1) to the precipitated liquid obtained in step (1) for defluorination treatment, stirring for 20 minutes after the addition of calcium hydroxide, and then filtering to obtain a defluorinated liquid;
[0062] (3) adding sodium carbonate (added at a molar ratio of calcium element to carbonate ion of 1:1.2) to the defluorinated liquid obtained in step (2) for decalcification, stirring for 0.5 h after the addition of sodium carbonate, and then filtering to obtain a decalcified liquid;
[0063] (4) The decalcified liquid obtained in step (3) is subjected to a second pH adjustment to 5.5 using sulfuric acid having a mass concentration of 50%, and then distilled and concentrated at a pressure of -0.07 MPa and a temperature of 85° C. until the volume of the crystalline solid accounts for 1 / 3 of the total volume, and then cooled to 40° C., followed by centrifugation to obtain an ammonium sulfate product.
[0064] Example 2
[0065] This embodiment provides a comprehensive utilization method of BOE waste liquid, which comprises the following steps:
[0066] (1) 500 mL of BOE waste liquid (containing 2% hydrogen fluoride, 8% ammonium fluoride, 2% ammonium bifluoride, and a pH value of 1) is subjected to a first pH adjustment using magnesium hydroxide to an end point pH value of 6 to obtain a first pH-adjusted liquid, and then a 2.5 mol / L magnesium sulfate solution (added according to a molar ratio of fluorine element to magnesium element of 2:1) is added to the first pH-adjusted liquid until no precipitation is precipitated, and the magnesium sulfate is stirred for 0.5 h after addition, and then filtered to obtain a filter cake and a filtrate, and the filter cake is washed and dried in turn to obtain a magnesium fluoride product, and the filtrate is mixed with the washed liquid obtained by washing to obtain 500 mL of precipitated liquid;
[0067] (2) adding calcium hydroxide (added at a molar ratio of fluorine to calcium of 2:1.2) to the precipitated liquid obtained in step (1) for defluorination treatment, stirring for 30 minutes after the addition of calcium hydroxide, and then filtering to obtain a defluorinated liquid;
[0068] (3) adding sodium carbonate (added at a molar ratio of calcium element to carbonate ion of 1:1) to the defluorinated liquid obtained in step (2) for decalcification, stirring for 0.2 h after the addition of sodium carbonate, and then filtering to obtain a decalcified liquid;
[0069] (4) The decalcified liquid obtained in step (3) is subjected to a second pH adjustment to 5 using sulfuric acid having a mass concentration of 50%, and then distilled and concentrated at a pressure of -0.05 MPa and a temperature of 95° C. until the volume of the crystalline solid accounts for 1 / 3 of the total volume, and then cooled to 25° C., followed by centrifugation to obtain an ammonium sulfate product.
[0070] Example 3
[0071] This embodiment provides a comprehensive utilization method of BOE waste liquid, which comprises the following steps:
[0072] (1) 500 mL of BOE waste liquid (containing 1.5% hydrogen fluoride, 15% ammonium fluoride, 2% ammonium bifluoride, and a pH value of 1) is subjected to a first pH adjustment using magnesium hydroxide to an end point pH value of 7 to obtain a first pH-adjusted liquid, and then a 4.5 mol / L magnesium sulfate solution (added according to a molar ratio of fluorine element to magnesium element of 2:1.5) is added to the first pH-adjusted liquid until no precipitation is produced, and the magnesium sulfate is stirred for 1 hour after being added, and then filtered to obtain a filter cake and a filtrate, and the filter cake is washed and dried in turn to obtain a magnesium fluoride product, and the filtrate is mixed with the washed liquid obtained by washing to obtain 500 mL of precipitated liquid;
[0073] (2) adding calcium hydroxide (added at a molar ratio of fluorine to calcium of 2:1) to the precipitated liquid obtained in step (1) for defluorination treatment, stirring for 10 minutes after the addition of calcium hydroxide, and then filtering to obtain a defluorinated liquid;
[0074] (3) adding sodium carbonate (added at a molar ratio of calcium element to carbonate ion of 1:1.5) to the defluorinated liquid obtained in step (2) for decalcification, stirring for 1 hour after the addition of sodium carbonate, and then filtering to obtain a decalcified liquid;
[0075] (4) The decalcified liquid obtained in step (3) is subjected to a second pH adjustment to 4.5 using sulfuric acid having a mass concentration of 50%, and then distilled and concentrated at a pressure of -0.1 MPa and a temperature of 80° C. until the volume of the crystalline solid accounts for 1 / 2 of the total volume, and then cooled to 45° C., followed by centrifugation to obtain an ammonium sulfate product.
[0076] Example 4
[0077] This embodiment provides a method for comprehensive utilization of BOE waste liquid. The difference between the comprehensive utilization method and that of Embodiment 1 is that after the first pH value is adjusted, the molar ratio of the fluorine element in the liquid to the magnesium element in the magnesium salt is 2:0.8.
[0078] Example 5
[0079] This embodiment provides a method for comprehensive utilization of BOE waste liquid. The difference between the comprehensive utilization method and that of Embodiment 1 is that after the first pH value is adjusted, the molar ratio of the fluorine element in the liquid to the magnesium element in the magnesium salt is 2:1.8.
[0080] Example 6
[0081] This embodiment provides a comprehensive utilization method of BOE waste liquid. The difference between the comprehensive utilization method and that of Embodiment 1 is that the molar ratio of fluorine element in the liquid after precipitation to calcium element in the calcium-containing defluorination agent is 2:0.7.
[0082] Example 7
[0083] This embodiment provides a method for comprehensive utilization of BOE waste liquid. The difference between the comprehensive utilization method and that of Embodiment 1 is that the molar ratio of calcium element in the defluorinated liquid to carbonate ion in carbonate is 1:0.6.
[0084] Comparative Example 1
[0085] This comparative example provides a method for comprehensive utilization of BOE waste liquid. The difference between the comprehensive utilization method and Example 1 is that step (2) and step (3) are not performed, and the precipitated liquid is used as the decalcified liquid to directly perform the second pH value adjustment, concentration, cooling and solid-liquid separation in step (4).
[0086] The purity of the magnesium fluoride products prepared in Examples 1-7 and Comparative Example 1 was tested by ion chromatography, and the results are shown in Table 1.
[0087] The nitrogen content of the ammonium sulfate products prepared in Examples 1-7 and Comparative Example 1 was detected by a nitrogen content titration method. The results are shown in Table 1.
[0088] The recoveries of the F element and the N element in Examples 1-7 and Comparative Example 1 were calculated, and the results are shown in Table 1, wherein the calculation method for the recovery of the F element is: the mass of the fluorine element in the magnesium fluoride product / the mass of the fluorine element in the BOE waste liquid × 100%; the calculation method for the recovery of the N element is: the mass of the nitrogen element in the ammonium sulfate / the mass of the fluorine element in the BOE waste liquid × 100%.
[0089] Table 1
[0090]
[0091] From the data in Table 1, we can see the following points:
[0092] (1) Under optimal conditions, the comprehensive utilization method provided by the present invention can make the purity of the magnesium fluoride product reach more than 97%, the recovery rate of the F element reach more than 98%, the nitrogen content of ammonium sulfate reach more than 21%, and the recovery rate of the N element reach more than 99%.
[0093] (2) Comprehensively comparing the data of Example 1 and Examples 4-5, it can be seen that the difference between Example 4-5 and Example 1 is that the molar ratio of the fluorine element in the liquid after the first pH value is adjusted to the magnesium element in the magnesium salt is not within the preferred range of the present invention. In Example 4, too little magnesium is added, resulting in a significantly lower recovery rate of the fluorine element than in Example 1. In Example 5, too much magnesium is added, resulting in a decrease in the nitrogen content of ammonium sulfate. It can be seen that the present invention can ensure that the fluorine element and the magnesium element are fully combined by preferably controlling the molar ratio of the fluorine element in the liquid after the first pH value is adjusted to the magnesium element in the magnesium salt, thereby ensuring the fluorine removal effect without wasting reagents and ensuring the quality of ammonium sulfate.
[0094] (3) A comprehensive comparison of the data of Example 1 and Example 6 shows that the only difference between Example 6 and Example 1 is that the molar ratio of the fluorine element in the liquid after precipitation to the calcium element in the calcium-containing defluorinating agent is not within the preferred range of the present invention. In Example 6, too little calcium is added, resulting in the inability to effectively remove the fluorine element, and the nitrogen content of the ammonium sulfate is reduced. It can be seen that the present invention can ensure the fluorine removal effect without wasting the agent by preferably controlling the molar ratio of the fluorine element in the liquid after precipitation to the calcium-containing defluorinating agent, thereby ensuring the quality of the ammonium sulfate.
[0095] (4) A comprehensive comparison of the data of Example 1 and Example 7 shows that the only difference between Example 7 and Example 1 is that the molar ratio of calcium element in the defluorinated liquid to carbonate ion in carbonate is not within the preferred range of the present invention. Too little carbonate is added in Example 7, resulting in an inability to effectively remove calcium ions and a decrease in the nitrogen content of ammonium sulfate. It can be seen that the present invention can ensure the calcium ion removal effect without wasting reagents by preferably controlling the molar ratio of calcium element in the defluorinated liquid to carbonate ion in carbonate, and ensure that no excessive sodium carbonate remains, otherwise the quality of the ammonium sulfate product will be affected.
[0096] (5) A comprehensive comparison of the data of Example 1 and Comparative Example 1 shows that the only difference between Comparative Example 1 and Example 1 is that step (2) and step (3) are not performed. The nitrogen content of ammonium sulfate and the recovery rate of N element in Comparative Example 1 are significantly lower than those in Example 1. It can be seen that the present invention can improve the quality and recovery rate of ammonium sulfate through the combined operation of defluorination treatment and decalcification treatment.
[0097] In summary, the comprehensive utilization method provided by the present invention can utilize BOE waste liquid to prepare products such as magnesium fluoride and ammonium sulfate, and the process is simple, which can reduce the equipment investment cost and the reagent cost, is environmentally friendly, and is conducive to industrial application.
[0098] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for comprehensive utilization of BOE waste liquid, characterized in that: The comprehensive utilization method comprises the following steps: (1) adjusting the BOE waste liquid to a first pH value to obtain a first pH-adjusted liquid, then adding a magnesium salt to the first pH-adjusted liquid until no precipitation is precipitated, then performing solid-liquid separation to obtain a filter cake and a filtrate, the filter cake is sequentially washed and dried to obtain a magnesium fluoride product, and the filtrate is mixed with the washed liquid obtained by washing to obtain a precipitated liquid; (2) adding a calcium-containing defluorinating agent to the precipitated liquid obtained in step (1) to perform defluorination treatment, and then performing solid-liquid separation to obtain a defluorinated liquid; (3) adding carbonate to the defluorinated liquid obtained in step (2) to perform decalcification treatment, and then performing solid-liquid separation to obtain a decalcified liquid; (4) The decalcified liquid obtained in step (3) is subjected to a second pH adjustment, and then concentrated, cooled, and solid-liquid separated in sequence to obtain an ammonium sulfate product.
2. The comprehensive utilization method according to claim 1, characterized in that: The BOE waste liquid in step (1) contains 0.1-5% hydrogen fluoride, 5-25% ammonium fluoride, and 1-15% ammonium hydrogen fluoride; Preferably, the pH value of the BOE waste liquid is less than 2.
3. The comprehensive utilization method according to claim 1 or 2, characterized in that: The first pH value adjustment agent used in step (1) includes magnesium hydroxide; Preferably, the endpoint pH value of the first pH adjustment is 6-7.
4. The comprehensive utilization method according to any one of claims 1 to 3, characterized in that: The magnesium salt in step (1) comprises magnesium sulfate; Preferably, the molar ratio of the fluorine element in the liquid to the magnesium element in the magnesium salt after the first pH value is adjusted is 2:(1-1.5); Preferably, the magnesium salt is added in the form of a solution; Preferably, the concentration of magnesium ions in the solution is 2.5-4.5 mol / L; Preferably, the magnesium salt is stirred after being added; Preferably, the stirring time after the magnesium salt is added is 0.5-1h.
5. The comprehensive utilization method according to any one of claims 1 to 4, characterized in that: The calcium-containing defluoridating agent in step (2) comprises calcium hydroxide; Preferably, the molar ratio of the fluorine element in the precipitated liquid to the calcium element in the calcium-containing defluoridation agent is 2:(1-1.2); Preferably, the calcium-containing defluoridating agent is stirred after being added; Preferably, the stirring time after the calcium-containing defluoridating agent is added is 10-30 minutes.
6. The comprehensive utilization method according to any one of claims 1 to 5, characterized in that: The carbonate in step (3) comprises sodium carbonate; Preferably, the molar ratio of calcium element in the defluorinated liquid to carbonate ion in the carbonate is 1:(1-1.5); Preferably, the carbonate is stirred after being added; Preferably, the stirring time after the carbonate is added is 0.2-1 h.
7. The comprehensive utilization method according to any one of claims 1 to 6, characterized in that: Step (4) the second pH value adjustment agent used comprises sulfuric acid; Preferably, the endpoint pH value of the second pH adjustment is 4.5-5.
5.
8. The comprehensive utilization method according to any one of claims 1 to 7, characterized in that: The concentration method in step (4) includes distillation concentration; Preferably, the pressure of the distillation concentration is -0.05 to -0.1 MPa; Preferably, the distillation and concentration temperature is 80-95°C; Preferably, the end point of the concentration is that the volume of the crystalline solid accounts for 1 / 3 to 1 / 2 of the total volume; Preferably, the cooling end point temperature is 25-45°C.
9. The comprehensive utilization method according to any one of claims 1 to 8, characterized in that: The solid-liquid separation method includes filtration or centrifugation.
10. The comprehensive utilization method according to any one of claims 1 to 9, characterized in that: The comprehensive utilization method comprises the following steps: (1) The BOE waste liquid is subjected to a first pH adjustment using magnesium hydroxide to an end point pH value of 6-7 to obtain a first pH adjusted liquid, and then magnesium sulfate is added to the first pH adjusted liquid until no precipitation is precipitated, the molar ratio of the fluorine element in the first pH adjusted liquid to the magnesium element in the magnesium sulfate is 2:(1-1.5), the magnesium sulfate is added in the form of a solution, the concentration of magnesium ions in the solution is 2.5-4.5 mol / L, the magnesium sulfate is stirred for 0.5-1h after being added, and then the solid-liquid separation is performed to obtain a filter cake and a filtrate, the filter cake is sequentially washed and dried to obtain a magnesium fluoride product, the filtrate is mixed with the washed liquid obtained by washing to obtain a precipitated liquid, the BOE waste liquid contains 0.1-5% hydrogen fluoride, 5-25% ammonium fluoride, and 1-15% ammonium bifluoride, and the pH value of the BOE waste liquid is less than 2; (2) adding calcium hydroxide to the precipitated liquid obtained in step (1) for defluorination treatment, wherein the molar ratio of the fluorine element in the precipitated liquid to the calcium element in the calcium hydroxide is 2:(1-1.2), stirring for 10-30 minutes after the calcium hydroxide is added, and then solid-liquid separation is performed to obtain a defluorinated liquid; (3) adding sodium carbonate to the defluorinated liquid obtained in step (2) for decalcification, wherein the molar ratio of calcium element in the defluorinated liquid to carbonate ion in sodium carbonate is 1:(1-1.5), stirring for 0.2-1h after adding sodium carbonate, and then separating the solid and liquid to obtain a decalcified liquid; (4) The decalcified liquid obtained in step (3) is adjusted to a second pH value of 4.5-5.5 using sulfuric acid, and then distilled and concentrated at a pressure of -0.05 to -0.1 MPa and a temperature of 80-95° C. until the volume of the crystalline solid accounts for 1 / 3 to 1 / 2 of the total volume, and then cooled to 25-45° C., followed by solid-liquid separation to obtain an ammonium sulfate product.