Active electrode material
By modifying mixed niobium oxide materials, the problems of safety limitations of graphite anodes and insufficient performance of lithium titanate materials in lithium-ion batteries have been solved, and efficient and safe lithium-ion battery performance improvements have been achieved.
Patent Information
- Application Number
- CN202410736930.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2021-04-09
- Filing Date
- 2021-08-27
- Publication Date
- 2024-10-11
AI Technical Summary
There are safety limitations of graphite anodes in existing lithium-ion batteries during high-power charging, resulting in lithium dendrite plating, resulting in battery cell short circuits, fire or explosion risks, and lithium titanate and mixed niobium oxide materials maintain capacity at high rates. Rate and power performance are limited and need improvement.
Modified mixed niobium oxide materials are used to improve their electronic conductivity and Coulombic efficiency by introducing different cations, oxygen deficiency or oxygen excess, and forming mixed anions, and are used as anode materials for lithium-ion batteries, combined with conductive additives and bonding agent to improve electrode performance.
Improved delithiation voltage and electronic conductivity at high C rates are achieved, improving the fast charging and discharging capabilities and safety of lithium-ion batteries, and reducing the resistance and cost of battery cells.
Smart Images

Figure BDA0004882059900000281 
Figure BDA0004882059900000291 
Figure BDA0004882059900000311
Abstract
Description
[0001] This application is a divisional application of the Chinese invention application with an international application date of August 27, 2021, an international application number of PCT / GB2021 / 052228, an application number of 202180051259.7 entering the Chinese national phase, and the invention name of “Active Electrode Material”. Field of the Invention
[0002] The present invention relates to active electrode materials and to methods for producing active electrode materials. Such materials are of interest as active electrode materials in lithium-ion or sodium-ion batteries, for example as anode materials for lithium-ion batteries. Background Art
[0003] Lithium-ion (Li-ion) batteries are a commonly used type of rechargeable battery, and their global market is expected to grow to $200 billion by 2030. Li-ion batteries are the technology of choice for electric vehicles with multiple requirements from technical performance to environmental impact, thus providing a viable path for a green automotive industry.
[0004] A typical lithium-ion battery consists of multiple battery cells connected in series or parallel. Each individual battery cell is usually composed of an anode (negative electrode) and a cathode (positive electrode), which are separated by a porous electrical insulating membrane (called a separator) and immersed in a liquid (called an electrolyte) that can transport lithium ions.
[0005] In most systems, the electrode consists of an electrochemically active material - meaning it is able to chemically react with lithium ions, thereby reversibly storing and releasing them in a controlled manner - mixed with conductive additives (such as carbon) and polymer binders, if necessary. A slurry of these components is applied in the form of a film on a current collector (usually a thin foil of copper or aluminum), forming an electrode after drying.
[0006] In known Li-ion battery technology, the safety limitations of graphite anodes during battery charging have severely hampered their use in high-power electronics, automotive and industrial applications. Among a wide range of potential alternatives recently proposed, lithium titanate (LTO) and mixed niobium oxides are the main contenders to replace graphite as the active material of choice for high-power fast-charging applications.
[0007] Batteries that rely on graphite anodes are fundamentally limited in terms of charge rate. Under nominal conditions, lithium ions are inserted into the anode active material during charging. As the charge rate increases, the typical graphite voltage characteristics are such that there is a high risk that the overpotential causes the potential of the sites on the anode to become <0V relative to Li / Li+, which leads to a phenomenon called lithium dendrite plating, whereby lithium ions are deposited on the surface of the graphite electrode in the form of lithium metal instead. This leads to an irreversible loss of active lithium and, therefore, rapid decay of the battery cell capacity. In some cases, such dendritic deposits can grow to such a large size that they pierce the battery separator and cause the battery cell to short-circuit. This can trigger a catastrophic failure of the battery cell, resulting in a fire or explosion. Therefore, the fastest charging batteries with graphite anodes are limited to charge rates of 5-7C, but usually lower.
[0008] Lithium titanate (LTO) anodes do not suffer from dendrite plating at high charge rates due to their high potential (1.6 V vs. Li / Li+) and have excellent cycle life because they do not suffer from significant volume expansion of the active material upon Li ion insertion due to their adaptable 3D crystal structure. For these two reasons, LTO batteries are generally considered to be high-safety battery cells. However, LTO is a relatively poor electronic and ionic conductor, which leads to limited capacity retention and resulting power performance at high rates unless the material is nanosized to increase the specific surface area and is carbon-coated to increase electronic conductivity. This particle-level material engineering increases the porosity and specific surface area of the active material and leads to a significant reduction in the achievable packing density in the electrode. This is important because it results in low-density electrodes and a higher fraction of electrochemically inactive materials (e.g., binders, carbon additives), resulting in much lower gravimetric energy density and volumetric energy density.
[0009] The key measure of anode performance is the electrode volume capacity (mAh / cm 3 ), which is the amount of charge (i.e., lithium ions) that can be stored per unit volume of the anode. This is an important factor in determining the overall battery energy density (Wh / L) on a volume basis when combined with the cathode and appropriate cell design parameters. The electrode volume capacity can be approximated by the electrode density (g / cm 3 ), the product of the active material specific capacity (mAh / g) and the fraction of active material in the electrode. LTO anodes typically have a relatively low specific capacity (c.165 mAh / g, compared to c.330 mAh / g for graphite), which is consistent with the low electrode density discussed above (typically 2.0 g / cm 3 ) and low active material fraction (<90%) result in very low volumetric capacity (<300 mAh / cm 3), and thus result in low battery energy density and high $ / kWh cost in various applications. Therefore, LTO batteries / battery cells are usually limited to specific niche applications despite their long cycle life, fast charging capability and high safety.
[0010] The use of mixed niobium oxide structures in Li-ion battery cells has recently attracted interest. Zhu et al., J. Mater. Chem. A, 2019, 7, 25537 and Zhu et al., Chem. Commun., 2020, 56, 7321-7324 disclose Zn2Nb as a possible active electrode material. 34 O 87 and Cu2Nb 34 O 87 . These papers rely on complex particle-scale engineering to purportedly achieve good properties, such as attempts to control particle porosity and morphology. It is believed that the properties of these materials can be improved. For example, these materials may not have sufficient electronic conductivity to allow efficient charging and discharging in Li-ion battery cells for commercial use, resulting in excessive impedance. In addition, improvements can still be made in Li-ion capacity, Coulombic efficiency, and tuning the voltage characteristics of charging and discharging. Making these improvements as described herein without the need for extensive nanoscale or particle-scale engineering and without the need for coatings is an important step towards low-cost battery materials to achieve mass market penetration. If these improvements are not addressed, the resistance in the resulting device is too large and the energy density is low, resulting in increased polarization, reduced power density, lower energy efficiency, and increased cost. Therefore, there is still a need for improved Zn2Nb for lithium-ion batteries. 34 O 87 and Cu2Nb 34 O 87 nature. Summary of the invention
[0011] In a first aspect, the present invention provides an active electrode material comprising a mixed niobium oxide, wherein the mixed niobium oxide has a composition M1 a M2 2-a M3 b Nb 34-b O 87-c-d Q d ,in:
[0012] M1 and M2 are different;
[0013] M1 is selected from the group consisting of Mg, Ca, Sr, Y, La, Ce, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, In, Si, Ge, Sn, Pb, P, Sb, Bi, and mixtures thereof;
[0014] M2 is Zn or Cu;
[0015] M3 is selected from the group consisting of Mg, Ca, Sr, Y, La, Ce, Ti, Zr, Hf, V, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, In, Si, Ge, Sn, Pb, P, Sb, Bi, and mixtures thereof;
[0016] Q is selected from F, Cl, Br, I, N, S, Se and mixtures thereof;
[0017] 0≤a<1.0; 0≤b≤3.4; -0.5≤c≤4.35; 0≤d≤4.35;
[0018] One or more of a, b, c, and d is not equal to 0; and
[0019] When a, b, and d are equal to zero, c is greater than zero.
[0020] It should be understood that the composition of the mixed niobium oxide does not correspond to the stoichiometric Zn2Nb 34 O 87 Cu2Nb 34 O 87 The inventors have found that by incorporating additional cations (M1 and / or M3), and / or by generating induced oxygen deficiency or oxygen excess, and / or by forming mixed anionic materials (comprising O and Q) to Zn2Nb 34 O 87 Cu2Nb 34 O 87 The modified niobium oxide has improved electrochemical properties, and in particular improved electrochemical properties when used as an anode material. When a>0, the mixed niobium oxide is modified by partially replacing M2 (Zn or Cu) with M1. When b>0, the mixed niobium oxide is modified by partially replacing Nb with M3. When c≠0, the mixed niobium oxide is modified by oxygen deficiency or oxygen excess. When d>0, the mixed niobium oxide is modified by partially replacing O with Q. The inventors have found that compared to the unmodified 'basic' Zn2Nb 34 O 87 In contrast, the materials according to the invention have improved electronic conductivity and improved coulombic efficiency as well as improved delithiation voltage at high C-rates, as shown in the examples of the invention. These are important results demonstrating the advantages of the materials of the invention for use in high-power batteries designed for fast charge / discharge.
[0021] The active electrode material of the present invention is particularly useful for electrodes, preferably for anodes of lithium-ion or sodium-ion batteries. Therefore, in another embodiment of the present invention, the active electrode material of the first aspect comprises mixed niobium oxide and at least one other component; optionally wherein the at least one other component is selected from a binder, a solvent, a conductive additive, a different active electrode material and a mixture thereof. This composition can be used to manufacture an electrode. Another embodiment of the present invention is an electrode comprising the active electrode material of the first aspect in electrical contact with a current collector. Another embodiment of the present invention is an electrochemical device comprising an anode, a cathode and an electrolyte disposed between the anode and the cathode, wherein the anode comprises an active electrode material according to the first aspect; optionally wherein the electrochemical device is a lithium-ion battery or a sodium-ion battery.
[0022] In a second aspect, the present invention provides a method for preparing a mixed niobium oxide as defined by the first aspect, the method comprising the steps of: providing one or more precursor materials; mixing the precursor materials to form a precursor material mixture; and heat treating the precursor material mixture at a temperature in the range of 400° C. to 1350° C. or 800° C. to 1350° C., thereby providing the mixed niobium oxide. This represents a convenient and efficient method for preparing the active electrode material of the first aspect.
[0023] The present invention includes any combination of aspects and features described herein unless such combination is expressly impermissible or explicitly avoided. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The principles of the present invention will now be discussed with reference to the accompanying drawings.
[0025] Figure 1 : Powder XRD of samples 1-4
[0026] Figure 2 : Powder XRD of samples 5-12. DETAILED DESCRIPTION
[0027] Aspects and embodiments of the present invention will now be discussed with reference to the accompanying drawings. Other aspects and embodiments will be apparent to those skilled in the art. All documents mentioned herein are incorporated herein by reference.
[0028] The term "mixed niobium oxide" (MNO) may refer to an oxide comprising niobium and at least one other cation. MNO materials have a high redox voltage (>0.8 V vs. lithium), enabling safe and long-life operation, which is critical for battery cells for fast-charging batteries. In addition, each atom of the niobium cation can have two redox reactions, resulting in a higher theoretical capacity than, for example, LTO. The mixed niobium oxide described herein is derived from the basic structure Zn2Nb34 O 87 Cu2Nb 34 O 87 .
[0029] Zn2Nb 34 O 87 Cu2Nb 34 O 87 It can be considered to have ReO3-derived MO 3-x Crystal structure. Preferably, the mixed niobium oxide has a Wadsley-Roth crystal structure. The Wadsley-Roth crystal structure is considered to be a crystallographically non-stoichiometric MO3(ReO3) crystal structure containing crystallographic shear, and the simplified formula is MO 3-x Therefore, these structures usually contain [MO6] octahedral subunits in their crystal structure. MNO materials with these structures are believed to have favorable properties for use as active electrode materials, such as in lithium-ion batteries.
[0030] The open tunnel-like MO3 crystal structure of MNO materials also makes them ideal candidates for high Li-ion storage capacity and high-rate intercalation / deintercalation. The crystallographic non-stoichiometry present in the MNO structure gives rise to Wadsley-Roth crystallographic superstructures. These superstructures, combined with other properties such as the Jahn-Teller effect and crystallographic disorder enhanced by the use of multiple mixed cations, stabilize the crystals during intercalation and keep the tunnels open and stable, thereby facilitating the storage of Li-ion ions due to the high Li-ion diffusion rate (reported to be about 10 -13 cm 2 s -1 ) to achieve extremely high rate performance.
[0031] Zn2Nb 34 O 87 Cu2Nb 34 O 87 The crystal formula of can be described as having a 3x4x∞ crystallographic block structure consisting of [MO6] octahedra, where M is Cu, Zn, or Nb. The Cu and Zn octahedra may be randomly distributed in the structure, or may prefer specific sites, such as at the edges or corners of the blocks. This is equivalent to 2 / 3 of each block being a Zn or Cu cation. Zn2Nb 34 O 87 The crystal formula can be described as Cu2Nb 34 O 87 isostructural phases of 2,4-dimethyl-1,2 ...
[0032] The overall crystal composition of the materials described herein is preferably charge neutral and thermodynamically favorable to follow the above description. When reducing the resistance of the material, a structure lacking oxygen, such as by introducing oxygen vacancy site defects, is preferred, so that M x O y Change to M x O y-δ . Oxygen-deficient structures may contain shear defects. Structures in which cations (i.e., Zn, Cu, and Nb) or anions (i.e., O) have been substituted may have matching valences (i.e., 5+ cations for equal proportions of 4+ and 6+ cations) or mismatched valences, which may induce oxygen deficiency or oxygen excess if the substitution occurs at equivalent crystal sites. Substitution may also occur at different crystal sites, such as interstitial sites.
[0033] As is well known, the crystal structure of a material can be determined by analyzing an X-ray diffraction (XRD) pattern. For example, an XRD pattern obtained from a given material can be compared to a known XRD pattern to confirm the crystal structure, for example, via a public database such as the ICDD crystallographic database. Rietveld analysis can also be used to determine the crystal structure of a material, particularly with respect to unit cell parameters. Thus, the active electrode material may have a Wadsley-Roth crystal structure, as determined by X-ray diffraction.
[0034] Preferably, the crystal structure of the mixed niobium oxide as determined by X-ray diffraction corresponds to Zn2Nb 34 O 87 Cu2Nb 34 O 87 ; Most preferably Zn2Nb 34 O 87 In this way, it was confirmed that the 'base' material had been modified without significantly affecting the crystal structure, which is believed to have advantageous properties for use as an active electrode material. 34 O 87 The crystal structure of can be found in the ICDD Crystallographic Database entry JCPDS28-1478.
[0035] The mixed niobium oxide with cation / anion exchange may have unit cell parameters a, b and c, where a is Preferably Preferably and Preferably The mixed niobium oxide may have unit cell parameters α and γ, each about 90°, preferably wherein α=γ=90°; and β in the range of 113.05-113.75°, preferably 113.08-113.69° and a unit cell volume of Preferably The unit cell parameters can be determined by X-ray diffraction.The mixed niobium oxide can have a crystallite size of 5-150 nm, preferably 30-60 nm, as determined according to the Scherrer equation.
[0036] Here, the term 'corresponding' is intended to reflect that the peaks in the X-ray diffraction pattern may be offset by no more than 0.5 degrees (preferably no more than 0.25 degrees, more preferably no more than 0.1 degrees) from the corresponding peaks in the X-ray diffraction patterns of the materials listed above.
[0037] Mixed niobium oxide having composition M1 a M2 2-a M3 b Nb 34-b O 87-c-d Q d ,in:
[0038] M1 and M2 are different;
[0039] M1 is selected from the group consisting of Mg, Ca, Sr, Y, La, Ce, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, In, Si, Ge, Sn, Pb, P, Sb, Bi, and mixtures thereof;
[0040] M2 is Zn or Cu;
[0041] M3 is selected from the group consisting of Mg, Ca, Sr, Y, La, Ce, Ti, Zr, Hf, V, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, In, Si, Ge, Sn, Pb, P, Sb, Bi, and mixtures thereof;
[0042] Q is selected from F, Cl, Br, I, N, S, Se and mixtures thereof;
[0043] 0≤a<1.0; 0≤b≤3.4; -0.5≤c≤4.35; 0≤d≤4.35;
[0044] One or more of a, b, c, and d is not equal to 0; and
[0045] When a, b, and d are equal to zero, c is greater than zero.
[0046] By 'and mixtures thereof', it is intended that M1, M3 and Q may each represent two or more elements from their corresponding lists. An example of such a material is Mg 0.1 Ge 0.1 Zn 1.8 Nb 34 O 87.1Here, M1 is Mg a’ Ge a” (where a'+a"=a), M2 is Zn, a=0.2, b=0, c=-0.1, d=0. Here, it is assumed that each cation adopts its typical oxidation state, i.e., Mg 2+ ,Ge 4+ 、Zn 2+ and Nb 5+ , c was calculated.
[0047] The exact values of a, b, c, d within the defined ranges can be selected to provide a charge-balanced or substantially charge-balanced crystal structure. Additionally or alternatively, the exact values of a, b, c, d within the defined ranges can be selected to provide a thermodynamically stable or thermodynamically metastable crystal structure.
[0048] When the exchange of cations or anions (i.e., Zn, Cu, Nb, O) in the structure occurs without retaining the initial valence, this can lead to both oxygen deficiency and oxygen excess. 4+ Replace Zn 2+ The materials with Al 3+ Replace Nb 5+ A slight oxygen deficiency is shown (ie, Nb2O5 vs. Al2O3). Oxygen deficiency can also be induced by heat treatment under inert or reducing conditions, which results in induced oxygen vacancy defects in the structure.
[0049] There may be partial oxidation or partial reduction to compensate for the exchange without retaining the initial valence. 4+ Replace Zn 2+ This can be achieved at least in part by removing some of the Nb 5+ Reduction to Nb 4+ to compensate.
[0050] M2 is Zn or Cu. Preferably, M2 is Zn, in which case the material is based on Zn2Nb 34 O 87 .
[0051] M1 is a cation that replaces M2 in the crystal structure. M1 can be selected from Mg, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, Si, Ge, Sn, P and mixtures thereof; preferably Mg, Ti, Zr, V, Nb, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, B, Al, Si, Ge, P and mixtures thereof; most preferably Mg, Zr, V, Cr, Mo, W, Fe, Cu, Zn, Al, Ge, P and mixtures thereof. M1 may have a cation that is similar to M2. 2+ Different valence. This can lead to hypoxia or excess oxygen. Optionally, M1 has a value equal to or higher than M2 2+ valence, preferably a higher valence.
[0052] M1 may also be selected from each specific element so used in the embodiments.
[0053] When more than one element is present as M1 or M3, it is understood that the valence refers to M1 or M3 as a whole. For example, if 25 at% of M1 is Ti and 75 at% of M1 is W, the valence of M1 is 0.25×4 (contribution of Ti)+0.75×6 (contribution of W).
[0054] M1 preferably has the same 2+ Different ionic radii, most preferably smaller ionic radii. This results in changes in the unit cell size and local deformations in the crystal structure, thereby providing the advantages discussed herein. The ionic radius referred to herein is the Shannon ionic radius (available from RD Shannon, Acta Cryst., A32, 1976, 751-767) under the coordination and valence that the ions are expected to adopt in the crystal structure of the mixed niobium oxide. For example, Zn2Nb 34 O 87 The crystal structure includes Nb 5+ O6 octahedron and Zn 2+ O6 octahedron. Therefore, when M3 is Zr, the ionic radius is taken as 6-coordinated Zr 4+ The ionic radius is because this is the substitution of Zn2Nb 34 O 87 The typical valence and coordination of Zr in Nb.
[0055] The amount of M1 is defined by a, satisfying the criterion 0≤a<1.0. a may be 0≤a≤0.6, preferably 0≤a≤0.2. Most preferably, a>0, for example a≥0.01. When M1 has the same valence as M2, it may be easier to achieve higher values of a. When M1 contains a cation with a valence of 2+ (e.g., Mg), a may be 0≤a<1.0. When M1 does not contain a cation with a valence of 2+, a may be 0≤a≤0.15.
[0056] M3 is a cation that replaces Nb in the crystal structure. M3 can be selected from Mg, Ti, Zr, Hf, V, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, Si, Sn, P and mixtures thereof; preferably Mg, Ti, Zr, V, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Si, P and mixtures thereof; most preferably Ti, Zr, V, Cr, Mo, W, Fe, Cu, Zn, Al, P and mixtures thereof. M3 may have a relative position to Nb 5+ Different valence. This can lead to oxygen deficiency or oxygen excess. Preferably, M3 has a lower 5+ This results in oxygen deficiency, i.e. the presence of oxygen vacancies provides the advantages discussed in this paper.
[0057] M3 may also be selected from each specific element so used in the embodiments.
[0058] M3 preferably has 5+ Different ionic radii, most preferably larger ionic radii. This results in altered unit cell dimensions and local deformations in the crystal structure, providing the advantages discussed herein.
[0059] The amount of M3 is defined by b, satisfying the criterion 0≤b≤3.4. b may be 0≤b≤1.5, preferably 0≤b≤0.3. In each of these cases, b may be >0, for example b≥0.01. When M3 has a relative humidity of Nb 5+ When the valence is the same, it may be easier to achieve a higher b value. When M3 includes a cation with a valence of 5+ (e.g., Ta), b may be 0≤b≤3.4. When M3 does not include a cation with a valence of 5+, b may be 0≤b≤0.2.
[0060] Surprisingly, it has been found that the cationic substitution process according to the present invention can produce a mixed niobium oxide that is more economical to synthesize than the unmodified 'base' material. Optionally, both a and b are > 0. When both a and b are > 0, the 'base' material has been substituted both at the M2 site and at the Nb site.
[0061] c reflects the oxygen content of the mixed niobium oxide. When c is greater than 0, it forms an oxygen-deficient material, i.e., the material has oxygen vacancies. Such a material will not have an exact charge balance without changing the state of the cationic oxygen, but is considered to be "substantially charge balanced" as described above. Alternatively, c may be equal to 0, in which case it is not an oxygen-deficient material. c may be less than 0, which is an oxygen-excess material. c may be -0.25≤c≤4.35.
[0062] When c is 4.35, the number of oxygen vacancies is equal to 5% of the total oxygen in the crystal structure. c may be greater than 0.0435, greater than 0.087, greater than 0.174, or greater than 0.435. c may be between 0 and 2, between 0 and 0.75, between 0 and 0.5, or between 0 and 0.25. For example, c may satisfy 0.01≤c≤4.35. When a material is deficient in oxygen, such as in the case of induced hypoxia, the electrochemical properties of the material may be improved, for example, resistance measurements may show increased conductivity compared to an equivalent non-deficient material. As will be understood, the percentage values expressed herein are atomic percentages.
[0063] The present invention relates to mixed niobium oxides which may contain oxygen vacancies (oxygen-deficient mixed niobium oxides), or may have excess oxygen. Oxygen vacancies in mixed niobium oxides may be formed by under-substitution of the base material as described above, and oxygen excess in mixed niobium oxides may be formed by substitution to increased valence. Oxygen vacancies may also be formed by heating the mixed niobium oxide under reducing conditions, which may be referred to as formation-induced oxygen deficiency. The amount of oxygen vacancies and oxygen excess may be relative to the total amount of oxygen in the base material, i.e., the unsubstituted material (e.g., Zn2Nb 34 O 87 ) is expressed as the amount of oxygen in the
[0064] There are a variety of methods to determine whether deficiencies in oxygen, such as oxygen vacancies, are present in a material. For example, thermogravimetric analysis (TGA) can be performed to measure the change in mass of a material when it is heated in an air atmosphere. When heated in air, the mass of a material containing oxygen vacancies increases as the material "reoxidizes" and the oxygen vacancies are filled with oxide anions. The magnitude of the mass increase can be used to quantify the concentration of oxygen vacancies in the material, assuming that the mass increase occurs entirely due to the oxygen vacancies being filled. It should be noted that a material containing oxygen vacancies may show an initial mass increase when the oxygen vacancies are filled, followed by a mass decrease at higher temperatures if the material undergoes thermal decomposition. In addition, there may be overlapping mass loss and mass gain processes, meaning that some materials containing oxygen vacancies may not show mass gain (and sometimes may not show mass loss or gain) during TGA analysis.
[0065] Other methods for determining the presence of deficient oxygen (e.g., oxygen vacancies) include Raman spectroscopy, electron paramagnetic resonance (EPR), X-ray photoelectron spectroscopy (e.g., XPS of oxygen 1s and / or XPS of cations in mixed oxides), X-ray absorption near edge structure (XANES, e.g., XANES of cations in mixed metal oxides), and TEM (e.g., scanning TEM (STEM) equipped with high angle annular dark field (HAADF) and annular bright field (ABF) detectors). The presence of deficient oxygen can be qualitatively determined by evaluating the color of the material relative to a non-deficient sample of the same material, the color being indicative of changes in the electronic band structure of the material through interaction with light. For example, the non-deficient stoichiometric Zn2Nb 34 O 87 White. Zn2Nb with induced hypoxia 34 O <87 With grey / black color. The presence of vacancies can also be inferred from comparison of the properties of the stoichiometric material (eg, conductivity) with the properties of the oxygen-deficient material.
[0066] When d>0, additional anions Q are introduced into the mixed niobium oxide. Due to their different electronic structures (i.e., F- and O 2- ) and different ionic radii (6-coordinate 6-Coordination ), they can improve the electrochemical performance of the active material. This is because the different ionic radii change the unit cell characteristics, thereby allowing an increase in Li ion capacity, or an increase in Coulombic efficiency by increasing reversibility. They can also increase the conductivity by changing the electronic structure of the crystal (i.e., doping effect), as in the case of oxygen vacancy defects or low-valent cation substitution. d can be 0≤d≤3.0, or 0≤d≤2.17. In each of these cases, d can be>0. Q is selected from F, Cl, N, S and mixtures thereof; or F, N and mixtures thereof; or Q is F.
[0067] Optionally, d=0, in which case the material has composition M1 a M2 2-a M3 b Nb 34-b O 87-c , wherein M1, M2, M3, a, b and c are as defined herein. Advantageously, the material with d=0 does not contain anion Q and may be easier to synthesize.
[0068] When a>0 and b=d=0, the material has composition M1 a M2 2-a Nb 34 O 87-c, wherein M1, M2, a and c are as defined herein, e.g. 0≤c≤4.35. This represents a material that has been modified at the M2 site and optionally modified by induced oxygen deficiency. Such materials represent an improvement of the 'base' oxide M22Nb by simple synthetic means. 34 O 87 Here, M1 may represent Ti, Mg, V, Cr, W, Zr, Mo, Cu, Ga, Ge, Ni, Al, Hf, Ta, Zn and mixtures thereof; preferably Ti, Mg, V, Cr, W, Zr, Mo, Ga, Ge, Al, Zn and mixtures thereof.
[0069] When a=b=d=0 and c>0, the material has the composition M22Nb 34 O 87-c , wherein M2 and c are as defined herein. This indicates that the modification is made only by inducing oxygen deficiency, thereby providing materials with improved properties as shown in the examples. For example, it has been found that materials with a=b=d=0 and c>0 unexpectedly improve electronic conductivity.
[0070] It should be understood that the discussion of the variables of composition (M1, M2, M3, Q, a, b, c and d) is intended to be understood in combination. For example, preferably, M1 is selected from Mg, Ti, Zr, V, Nb, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, B, Al, Si, Ge, P and mixtures thereof, and M3 is selected from Mg, Ti, Zr, V, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Si, P and mixtures thereof, and Q is selected from F, Cl, N, S and mixtures thereof. Preferably, 0≤a≤0.6, 0≤b≤1.5, 0≤c≤4.35 and 0≤d≤3.0.
[0071] For example, the mixed niobium oxide may have a composition M1 a M2 2-a M3 b Nb 34-b O 87-c-d Q d ,in:
[0072] M1 and M2 are different;
[0073] M1 is selected from the group consisting of Mg, Ti, Zr, V, Nb, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, B, Al, Si, Ge, P and mixtures thereof;
[0074] M2 is Zn or Cu;
[0075] M3 is selected from the group consisting of Mg, Ti, Zr, V, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Si, P, and mixtures thereof;
[0076] Q is selected from F, N and mixtures thereof;
[0077] 0≤a≤0.6; 0≤b≤1.5; -0.5≤c≤4.35; 0≤d≤4.35;
[0078] One or more of a, b, c, and d is not equal to 0; and
[0079] When a, b, and d are equal to zero, c is greater than zero.
[0080] For example, the mixed niobium oxide may have a composition M1 a Zn 2-a M3 b Nb 34-b O 87-c-d Q d ,in:
[0081] M1 is selected from Mg, Zr, V, Cr, Mo, W, Fe, Cu, Al, Ge, P and mixtures thereof;
[0082] M3 is selected from Ti, Zr, V, Cr, Mo, W, Fe, Cu, Zn, Al, P and mixtures thereof;
[0083] Q is selected from F, N and mixtures thereof;
[0084] 0 <a≤0.2;0≤b≤0.3;0≤c≤4.35;0≤d≤3.0。
[0085] M1, M3 and Q may also be selected from each specific element used as these dopants in the embodiments.
[0086] Optionally, the mixed niobium oxide is free of titanium.
[0087] The mixed niobium oxide may have a composition M1 a M2 2-a M3 b Nb 34-b O 87-c ,in:
[0088] M1 is selected from Cr, Al, Ge and mixtures thereof, preferably wherein M1 is Cr;
[0089] M2 is Zn or Cu, preferably wherein M2 is Zn;
[0090] M3 is selected from Ti, Zr, Fe and mixtures thereof and optionally contains Ti, preferably where M3 is selected from Ti, Zr and mixtures thereof and optionally contains Ti, and most preferably where M3 is Ti;
[0091] 0 < a < 1.0, preferably 0.01 < a < 1.0;
[0092] 0 < b ≤ 1.5, preferably 0.01 < b < 1.0;
[0093] -0.5 ≤ c ≤ 4.35, preferably -0.5 ≤ c ≤ 2, and most preferably c = 0.
[0094] The mixed niobium oxide may have the composition Cr a Zn 2-a M3 b Nb 34-b O 87-c , where:
[0095] M3 is selected from Ti, Zr and mixtures thereof and optionally contains Ti, preferably where M3 is Ti;
[0096] 0.01 < a < 1.0, preferably 0.1 < a < 1.0;
[0097] 0.01 < b < 1.0, preferably 0.1 < b < 1.0;
[0098] -0.5 ≤ c ≤ 2, preferably c = 0.
[0099] The mixed niobium oxide may also contain Li and / or Na. For example, when the mixed niobium oxide is used in a metal ion battery electrode, Li and / or Na may enter the crystal structure.
[0100] The mixed niobium oxide is preferably in particulate form. The material may have a D 50 particle size in the range of 0.1 - 100 μm, or 0.5 - 50 μm, or 1 - 20 μm. These particle sizes are advantageous because they are easy to handle and form into electrodes. In addition, these particle sizes avoid the need to use complex and / or expensive methods to provide nanoparticles. Nanoparticles (e.g., particles with a D 50 particle size of 100 nm or less) are generally more complex to synthesize and require additional safety considerations.
[0101] The mixed niobium oxide may have a D 10 particle size of at least 0.05 μm, or at least 0.1 μm, or at least 0.5 μm, or at least 1 μm. By maintaining the D 10 particle size within these ranges, the likelihood of parasitic reactions in a Li-ion battery cell is reduced due to the reduced surface area, and it is easier to handle with less binder in the electrode slurry.
[0102] The mixed niobium oxide may have a D of no more than 200 μm, no more than 100 μm, no more than 50 μm, or no more than 20 μm. 90 Particle size. 90 By maintaining the particle size within these ranges, the proportion of the particle size distribution with large particle sizes is minimized, thereby making the material easier to manufacture into a homogeneous electrode.
[0103] The term "particle size" refers to the equivalent spherical diameter (esd), which is the diameter of a sphere having the same volume as a given particle, wherein the particle volume is understood to include the volume of any intraparticle pores. n ” and “D n The term "D" refers to the diameter below which n% of the volume of the particle population exists. 50 ” and “D 50 "Particle size" refers to the median particle size based on volume, below which 50% of the volume of the particle population exists. In the case where the material comprises primary crystallites agglomerated into secondary particles, it is understood that the particle size refers to the diameter of the secondary particles. The particle size can be determined by laser diffraction. The particle size can be determined according to ISO 13320:2009, for example using Mie theory.
[0104] The mixed niobium oxide may have a range of 0.1-100 m 2 / g, or 0.5-50m 2 / g, or 1-20m 2 In general, a low BET surface area is preferred in order to minimize the reaction of the mixed niobium oxide with the electrolyte, for example, to minimize the formation of a solid electrolyte interphase (SEI) layer during the first charge-discharge cycle of an electrode comprising the material. However, too low a BET surface area can result in unacceptably low charge rates and capacities because the bulk of the mixed niobium oxide is poorly accessible to metal ions in the surrounding electrolyte.
[0105] The term "BET surface area" refers to the surface area per unit mass calculated by measuring the physical adsorption of gas molecules on a solid surface using the Brunauer-Emmett-Teller theory. For example, the BET surface area can be determined according to ISO 9277:2010.
[0106] The specific capacity / reversible delithiation capacity of the mixed niobium oxide may be 180 mAh / g or greater, 190 mAh / g or greater, or 197 mAh / g or greater. Here, the specific capacity is defined as the specific capacity measured in the second cycle of a half-cell constant current cycle test at a 0.1C rate, wherein in the half-cell, the voltage window is 1.1-3.0 V relative to Li / Li+. Providing a material with a high specific capacity may be advantageous because it may provide improved performance in an electrochemical device comprising the mixed niobium oxide.
[0107] When formulated or coated as an electrode (optionally with a conductive carbon additive and a binder material) as described below, the active electrode material may have a sheet resistance of 2.5 kΩ / sq or less, more preferably 1.2 kΩ / sq or less, which may be measured as defined in the Examples. Sheet resistance may be a useful surrogate measure of the electronic conductivity of such materials. Providing materials with suitably low sheet resistance may be advantageous, as this may provide improved performance in electrochemical devices comprising mixed niobium oxides.
[0108] The mixed niobium oxide may have a value greater than 10 -15 cm 2 s -1 , or more preferably greater than 10 -13 cm 2 s -1 It would be advantageous to provide a material having a suitably high lithium diffusion rate, as this could provide enhanced performance in an electrochemical device including mixed niobium oxide.
[0109] The mixed niobium oxide can be formed into a composite electrode with a suitable binder and conductive additives as described below to provide 2.5 g / cm 3 This enables the composite electrode to have an electrode porosity (calculated by the average of the measured electrode density / true density of each component) in the range of 30% to 40%, meeting the industrial requirements for high energy and high power battery cells. For example, a porosity of up to 2.9 g / cm 3 Electrode density. Providing materials with such electrode density may be advantageous because it may provide improved performance in electrochemical devices including mixed niobium oxide. Specifically, when the electrode density is high, high volumetric capacity may be achieved, such as gravimetric capacity x electrode density x mixed niobium oxide fraction = volumetric capacity.
[0110] The initial coulombic efficiency has been measured as the difference between the lithiation and delithiation capacities in the first charge / discharge cycle at C / 10 in a half-cell. The initial coulombic efficiency of the active electrode material may be greater than 97.9%, or greater than 98.8%. Providing a material with a suitably high initial coulombic efficiency may be advantageous, as this may provide improved performance in an electrochemical device comprising mixed niobium oxide.
[0111] The active electrode material of the first aspect of the invention may comprise mixed niobium oxide and at least one other component, optionally wherein at least one other component is selected from a binder, a solvent, a conductive additive, a different active electrode material and a mixture thereof. Such a composition can be used to prepare an electrode, such as an anode of a lithium ion battery. Preferably, the different active electrode materials are selected from different mixed niobium oxides, lithium titanium oxides, niobium oxides and mixtures thereof having a composition as defined in the first aspect. Alternatively, the active electrode material may consist of mixed niobium oxide.
[0112] The active electrode material may comprise mixed niobium oxide and lithium titanium oxide, preferably a mixture of mixed niobium oxide and lithium titanium oxide.
[0113] The lithium titanium oxide preferably has a spinel or ramsdellite crystal structure, for example, as determined by X-ray diffraction. Examples of lithium titanium oxides having a spinel crystal structure are Li4Ti5O 12 An example of a lithium titanium oxide having a ramsdellite crystal structure is Li2Ti3O7. These materials have been shown to have good properties for use as active electrode materials. Thus, the lithium titanium oxide may have a structure corresponding to Li4Ti5O as determined by X-ray diffraction. 12 and / or the crystal structure of Li2Ti3O7. Lithium titanium oxide may be selected from Li4Ti5O 12 , Li2Ti3O7 and mixtures thereof.
[0114] The lithium titanium oxide may be doped with additional cations or anions. The lithium titanium oxide may be oxygen-deficient. The lithium titanium oxide may constitute a coating, optionally wherein the coating is selected from carbon, polymers, metals, metal oxides, metalloids, phosphates and fluorides.
[0115] Lithium titanium oxide can be synthesized by conventional ceramic techniques (eg, solid state synthesis or sol-gel synthesis). Alternatively, lithium titanium oxide can be obtained from commercial suppliers.
[0116] The lithium titanium oxide is preferably in the form of microparticles. The lithium titanium oxide may have a D in the range of 0.1-50 μm, or 0.25-20 μm, or 0.5-15 μm. 50 The lithium titanium oxide may have a particle size of at least 0.01 μm, or at least 0.1 μm, or at least 0.5 μm. 10The lithium titanium oxide may have a particle size of no more than 100 μm, no more than 50 μm, or no more than 25 μm. 90 Particle size. 90 Maintaining the particle size within this range improves the packing of the lithium titanium oxide particles in the mixture with the mixed niobium oxide particles.
[0117] Lithium titanium oxide is generally used in battery anodes in small particle sizes due to the low electronic conductivity of the material. In contrast, mixed niobium oxide as defined herein may be used in larger particle sizes because it generally has a higher lithium ion diffusion coefficient than lithium titanium oxide. Advantageously, in the composition, the lithium titanium oxide may have a smaller particle size than the mixed niobium oxide, for example such that the D of the lithium titanium oxide is 50 Particle size and D of mixed niobium oxide 50 The particle size ratio is in the range of 0.01: 1 to 0.9: 1, or 0.1: 1 to 0.7: 1. In this way, smaller lithium titanium oxide particles can be accommodated in the spaces between larger mixed niobium oxide particles, thereby improving the packing efficiency of the composition.
[0118] Lithium titanium oxide may have a range of 0.1-100 m 2 / g, or 1-50m 2 / g, or 3-30m 2 The BET surface area is in the range of 1000 Å / g.
[0119] The mass ratio of lithium titanium oxide to mixed niobium oxide may be in the range of 0.5:99.5 to 99.5:0.5, preferably in the range of 2:98 to 98:2. In one implementation, the active electrode material comprises a higher proportion of lithium titanium oxide than mixed niobium oxide, for example, a mass ratio of at least 2:1, at least 5:1, or at least 8:1. Advantageously, this allows the mixed niobium oxide to be incrementally introduced into existing electrodes based on lithium titanium oxide without requiring major changes to manufacturing technology, thereby providing an effective way to improve the properties of existing electrodes. In another implementation, the active electrode material has a higher proportion of mixed niobium oxide than lithium titanium oxide, for example, such that the mass ratio of lithium titanium oxide to mixed niobium oxide is less than 1:2, or less than 1:5, or less than 1:8. Advantageously, this allows the cost of the active electrode material to be reduced by replacing some of the mixed niobium oxide with lithium titanium oxide.
[0120] The active electrode material may comprise a mixed niobium oxide and niobium oxide. Niobium oxide may be selected from Nb 12 O 29 , NbO2, NbO and Nb2O5. Preferably, the niobium oxide is Nb2O5.
[0121] Niobium oxide may be doped with additional cations or anions, for example, assuming that the crystal structure of niobium oxide corresponds to an oxide consisting of Nb and O (e.g., Nb12 O 29 The niobium oxide may be oxygen-deficient. The niobium oxide may constitute a coating, optionally wherein the coating is selected from carbon, polymers, metals, metal oxides, metalloids, phosphates and fluorides.
[0122] Niobium oxide may have Nb 12 O 29 The niobium oxide may have a crystal structure of NbO, NbO2, NbO or Nb2O5 as determined by X-ray diffraction. For example, the niobium oxide may have a crystal structure of orthorhombic Nb2O5 or a crystal structure of monoclinic Nb2O5. Preferably, the niobium oxide has a crystal structure of monoclinic Nb2O5, most preferably a crystal structure of H-Nb2O5. Additional information on the crystal structure of Nb2O5 can be found in Griffith et al., J. Am. Chem. Soc. 2016, 138, 28, 8888–8899.
[0123] Niobium oxide can be synthesized by conventional ceramic techniques (eg, solid state synthesis or sol-gel synthesis). Alternatively, niobium oxide can be obtained from commercial suppliers.
[0124] The niobium oxide is preferably in particulate form. The niobium oxide may have a D in the range of 0.1-100 μm, or 0.5-50 μm, or 1-20 μm. 50 The niobium oxide may have a particle size of at least 0.05 μm, or at least 0.5 μm, or at least 1 μm. 10 The niobium oxide may have a particle size of no more than 100 μm, no more than 50 μm, or no more than 25 μm. 90 Particle size. 90 Maintaining the particle size within this range improves the packing of the niobium oxide particles in a mixture with the mixed niobium oxide particles.
[0125] Niobium oxide may have a range of 0.1-100 m 2 / g, or 1-50m 2 / g, or 1-20m 2 The BET surface area is in the range of 1000 Å / g.
[0126] The mass ratio of niobium oxide to mixed niobium oxide may be in the range of 0.5:99.5 to 99.5:0.5, or in the range of 2:98 to 98:2, or preferably in the range of 15:85 to 35:55.
[0127] The invention also provides an electrode comprising the active electrode material of the first aspect of the invention in electrical contact with a current collector. The electrode may form part of a battery cell. The electrode may form an anode as part of a metal ion battery, optionally a lithium ion battery.
[0128] The present invention also provides use of the active electrode material of the first aspect of the invention in an anode of a metal ion battery, optionally wherein the metal ion battery is a lithium ion battery.
[0129] Another implementation of the present invention is an electrochemical device comprising an anode, a cathode and an electrolyte disposed between the anode and the cathode, wherein the anode comprises an active electrode material according to the first aspect of the present invention; optionally wherein the electrochemical device is a metal ion battery, such as a lithium ion battery or a sodium ion battery. Preferably, the electrochemical device is a lithium ion battery having a reversible anode active material specific capacity of greater than 190 mAh / g at 20 mA / g, wherein the battery can be charged and discharged at a current density of 200 mA / g or greater, or 1000 mA / g or greater, or 2000 mA / g or greater, or 4000 mA / g or greater relative to the anode active material, while retaining more than 70% of the initial battery cell capacity at 20 mA / g. It has been found that the use of the active electrode material of the first aspect of the present invention can produce a lithium ion battery having such a combination of properties, which represents a lithium ion battery particularly suitable for applications where high charge and discharge current densities are desired. It is noteworthy that examples have shown that the active electrode material according to the first aspect of the present invention has improved electronic conductivity and improved delithiation voltage at high C-rates.
[0130] The mixed niobium oxide can be synthesized by conventional ceramic techniques. For example, the material is prepared by one or more of solid state synthesis or sol-gel synthesis. The material can also be synthesized by one or more of commonly used alternative techniques, such as hydrothermal or microwave hydrothermal synthesis, solvothermal or microwave solvothermal synthesis, coprecipitation synthesis, spark or microwave plasma synthesis, combustion synthesis, electrospinning and mechanical alloying.
[0131] The second aspect of the present invention provides a method for preparing a mixed niobium oxide as defined by the first aspect, the method comprising the following steps: providing one or more precursor materials; mixing the precursor materials to form a precursor material mixture; and heat treating the precursor material mixture at a temperature in the range of 400°C-1350°C or 800°C-1350°C to provide the mixed niobium oxide.
[0132] In order to provide a mixed niobium oxide containing element Q, the method may further include the steps of: mixing the mixed niobium oxide with a precursor containing element Q to provide an additional precursor material mixture; and heat treating the additional precursor material mixture in a temperature range of 300°C to 1200°C or 800°C to 1200°C, optionally under reducing conditions, to provide a mixed niobium oxide containing element Q.
[0133] For example, in order to provide a mixed niobium oxide containing N as the element Q, the method may further include the following steps: mixing the mixed niobium oxide with a precursor containing N (e.g., melamine) to provide an additional precursor material mixture; and heat treating the additional precursor material mixture under reducing conditions (e.g., in N2) in a temperature range of 300°C-1200°C to provide a mixed niobium oxide containing N as the element Q.
[0134] For example, in order to provide a mixed niobium oxide containing F as the element Q, the method may further include the following steps: mixing the mixed niobium oxide with a precursor containing F (e.g., polyvinylidene fluoride) to provide an additional precursor material mixture; and heat treating the additional precursor material mixture under oxidizing conditions (e.g., in air) in a temperature range of 300°C-1200°C to provide a mixed niobium oxide containing F as the element Q.
[0135] The method may include the following additional step: heat treating the mixed niobium oxide or the mixed niobium oxide containing element Q under reducing conditions in the temperature range of 400°C-1350°C or 800°C-1350°C, thereby inducing oxygen vacancies in the mixed niobium oxide. The induced oxygen vacancies may be in addition to oxygen vacancies already present in the mixed niobium oxide (for example, already present due to low-valent substitution of M2 and / or Nb with M1 and / or M3). Alternatively, the induced oxygen vacancies may be new oxygen vacancies, for example, if M1 and M3 have the same valence as M2 and Nb. The presence of induced oxygen vacancies provides the advantages discussed herein.
[0136] The precursor material may include one or more metal oxides, metal hydroxides, metal salts or ammonium salts. For example, the precursor material may include one or more metal oxides or metal salts of different oxidation states and / or different crystal structures. Examples of suitable precursor materials include, but are not limited to, Nb2O5, Nb(OH)5, niobic acid, NbO, ammonium niobate oxalate, NH4H2PO4, (NH4)2PO4, (NH4)3PO4, P2O5, H3PO3, Ta2O5, WO3, ZrO2, TiO2, MoO3, V2O5, ZrO2, CuO, ZnO, Al2O3, K2O, KOH, CaO, GeO2, Ga2O3, SnO2, CoO, Co2O3, Fe2O3, Fe3O4, MnO, MnO2, NiO, Ni2O3, H3BO3, ZnO and MgO. The precursor material may not include a metal oxide, or may include an ion source other than an oxide. For example, the precursor material may include a metal salt (e.g., NO3 - 、SO3 -) or other compounds (e.g., oxalates, carbonates). In order to replace oxygen anions with other negatively charged anions Q, the precursor comprising element Q may comprise one or more organic compounds, polymers, inorganic salts, organic salts, gases or ammonium salts. Examples of suitable precursor materials comprising element Q include, but are not limited to, melamine, NH4HCO3, NH3, NH4F, PVDF, PTFE, NH4Cl, NH4Br, NH4I, Br2, Cl2, I2, ammonium oxychloride amide, and hexamethylenetetramine.
[0137] Some or all of the precursor materials may be particulate materials. Where they are particulate materials, preferably they have a diameter D of less than 20 μm (e.g., 10 nm to 20 μm). 50 Particle size. Providing particulate material having such a particle size can help promote more intimate mixing of the precursor materials, thereby producing a more efficient solid state reaction during the thermal treatment step. However, it is not necessary for the precursor material to have an initial particle size of <20 μm in diameter, as the particle size of one or more precursor materials can be mechanically reduced during the step of mixing the precursor materials to form the precursor material mixture.
[0138] The step of mixing the precursor materials to form a precursor material mixture and / or an additional precursor material mixture may be performed by a method selected from (but not limited to) the following: dry or wet planetary ball milling, rolling ball milling, high energy ball milling, high shear milling, air jet milling, steam jet milling, planetary mixing and / or impact milling. The force used for mixing / milling may depend on the morphology of the precursor materials. For example, in the case where some or all of the precursor materials have a larger particle size (e.g., a particle size greater than 20 μm), the particle size of the precursor material may be increased. 50 In the case of a particle size of 20 μm or less, the grinding force can be selected to reduce the particle size of the precursor material so that the particle size of the precursor material mixture is reduced to a diameter of 20 μm or less. When the particle size of the particles in the precursor material mixture is 20 μm or less, this can promote a more efficient solid-state reaction of the precursor material in the precursor material mixture during the thermal treatment step. Solid-state synthesis can also be carried out in pellets formed from precursor powders under high pressure (>10 MPa).
[0139] The step of heat treating the precursor material mixture and / or the further precursor material mixture may be performed for a period of 1 hour to 24 hours, more preferably 3 hours to 18 hours. For example, the heat treating step may be performed for 1 hour or more, 2 hours or more, 3 hours or more, 6 hours or more, or 12 hours or more. The heat treating step may be performed for 24 hours or less, 18 hours or less, 16 hours or less, or 12 hours or less.
[0140] The step of heat treating the precursor material mixture may be performed in a gas atmosphere, preferably air. Suitable gas atmospheres include: air, N2, Ar, He, CO2, CO, O2, H2, NH3 and mixtures thereof. The gas atmosphere may be a reducing atmosphere. In the case where it is desired to prepare an oxygen-deficient material, the step of heat treating the precursor material mixture is preferably performed in an inert atmosphere or a reducing atmosphere.
[0141] The step of heat treating the further mixture of precursor materials is performed under reducing conditions. Reducing conditions include under an inert gas, such as nitrogen, helium, argon; or under a mixture of an inert gas and hydrogen; or under vacuum. Preferably, the step of heat treating the further mixture of precursor materials includes heating under an inert gas.
[0142] The further step of heat treating the mixed niobium oxide and / or the mixed niobium oxide comprising element Q under reducing conditions may be performed for a period of 0.5 hours to 24 hours, more preferably 2 hours to 18 hours. For example, the heat treatment step may be performed for 0.5 hours or more, 1 hour or more, 3 hours or more, 6 hours or more or 12 hours or more. The further step of heat treating may be performed for 24 hours or less, 18 hours or less, 16 hours or less or 12 hours or less. Reducing conditions include under an inert gas, such as nitrogen, helium, argon; or under a mixture of an inert gas and hydrogen; or under vacuum. Preferably, heating under reducing conditions includes heating under an inert gas.
[0143] In some methods, it may be advantageous to perform a two-step thermal treatment. For example, the precursor material mixture and / or the additional precursor material mixture may be heated at a first temperature for a first length of time, and then heated at a second temperature for a second length of time. Preferably, the second temperature is higher than the first temperature. Performing such a two-step thermal treatment may facilitate solid state reactions to form the desired crystal structure. This may be performed sequentially, or may be performed in the presence of an intermediate regrinding step.
[0144] The method may include one or more post-treatment steps after forming the mixed niobium oxide. In some cases, the method may include a post-treatment step of heat treating the mixed niobium oxide, which is sometimes referred to as 'annealing'. This post-treatment heat treatment step may be performed in a gas atmosphere different from the step of heat treating the precursor material mixture to form the mixed niobium oxide. The post-treatment heat treatment step may be performed in an inert or reducing gas atmosphere. This post-treatment heat treatment step may be performed at a temperature greater than 500°C, for example at about 900°C. Including a post-treatment heat treatment step may be beneficial, for example, to form vacancies or defects in the mixed niobium oxide, such as inducing oxygen deficiencies; or to perform anion exchange on the formed mixed niobium oxide, such as exchanging O anions with N.
[0145] The method may include the steps of grinding and / or classifying (e.g., impact milling, jet milling, steam jet milling, high energy milling, high shear milling, pin milling, air classifying, wheel classifying, sieving) the mixed niobium oxide to provide a material having any of the particle size parameters given above.
[0146] There may be a step of carbon coating the mixed niobium oxide to increase its surface conductivity or to prevent reaction with the electrolyte. This typically involves combining the mixed niobium oxide with a carbon precursor to form an intermediate material, which may include grinding, preferably high energy grinding. Alternatively or in addition, the step may include mixing the mixed niobium oxide with the carbon precursor in a solvent such as water, ethanol or THF. These represent effective methods of ensuring uniform mixing of the mixed niobium oxide with the carbon precursor.
[0147] It has been found that polyaromatic sp 2 The carbon precursor of carbon provides a particularly beneficial carbon coating on the mixed niobium oxide of the first aspect of the present invention. Therefore, the method of preparing the mixed niobium oxide may further include the steps of: mixing the mixed niobium oxide or the mixed niobium oxide containing element Q with a polyaromatic sp 2 a carbon precursor of carbon to form an intermediate material; and heating the intermediate material under reducing conditions to pyrolyze the carbon precursor, thereby forming a carbon coating on the mixed niobium oxide and inducing oxygen vacancies in the mixed niobium oxide.
[0148] The intermediate material may include a carbon precursor in an amount of up to 25 wt%, or 0.1-15 wt%, or 0.2-8 wt%, based on the total weight of the mixed niobium oxide and the carbon precursor. The carbon coating on the mixed niobium oxide may be present in an amount of up to 10 wt%, or 0.05-5 wt%, or 0.1-3 wt%, based on the total weight of the mixed niobium oxide. These amounts of carbon precursor and / or carbon coating provide a good balance between increasing the electronic conductivity through the carbon coating without excessively reducing the capacity of the mixed niobium oxide by excessively reducing the proportion of the mixed niobium oxide. The mass of carbon precursor lost during pyrolysis may be in the range of 30-70 wt%.
[0149] The step of heating the intermediate material under reducing conditions may be performed at a temperature in the range of 400° C. to 1,200° C., or 500° C. to 1,100° C., or 600° C. to 900° C. The step of heating the intermediate material under reducing conditions may be performed for a duration in the range of 30 minutes to 12 hours, 1-9 hours, or 2-6 hours.
[0150] The step of heating the intermediate material under reducing conditions may be performed under an inert gas, such as nitrogen, helium, argon; or may be performed under a mixture of an inert gas and hydrogen; or may be performed under vacuum.
[0151] Contains polyaromatic sp 2The carbon precursor of carbon can be selected from pitch carbon, graphene oxide, graphene and mixtures thereof. Preferably, the carbon precursor comprising polyaromatic sp 2 The carbon precursor of the carbon is selected from the group consisting of pitch carbon, graphene oxide and mixtures thereof. Most preferably, the carbon precursor comprises a polyaromatic sp 2 The carbon precursor of the carbon is selected from pitch carbon. The pitch carbon can be selected from coal tar pitch, petroleum pitch, mesophase pitch, wood tar pitch, isotropic pitch, ground pitch and mixtures thereof.
[0152] Pitch carbon is a mixture of aromatic hydrocarbons of varying molecular weights. Pitch carbon is a low-cost byproduct of petroleum refineries and is widely available. The use of pitch carbon is advantageous because pitch has a low oxygen content. Thus, in combination with heating the intermediate material under reducing conditions, the use of pitch facilitates the formation of oxygen vacancies in the mixed niobium oxide.
[0153] Other carbon precursors often contain large amounts of oxygen. For example, carbohydrates such as glucose and sucrose are often used as carbon precursors. These carbohydrates have the empirical formula C m (H2O) n and thus contain a large number of covalently bonded oxygen (e.g., sucrose has the formula C 12 H 22 O 11 and having about 42 wt % oxygen). Pyrolysis of carbon precursors containing a large amount of oxygen is believed to prevent or inhibit reduction of the mixed niobium oxide, or even lead to oxidation, which means that oxygen vacancies may not be induced in the mixed niobium oxide. Therefore, the carbon precursor may have an oxygen content of less than 10 wt %, preferably less than 5 wt %.
[0154] The carbon precursor may contain substantially no sp 3 For example, the carbon precursor may contain less than 10 wt % sp 3 Carbon source, preferably less than 5 wt% sp 3 Carbon source. Carbohydrates are sp 3 The carbon precursor may contain no carbohydrates. It should be understood that some of the carbon precursors used in the present invention may contain sp 3 Carbon impurities, for example up to 3 wt%.
[0155] The mixed niobium oxide of the first aspect of the present invention may include a carbon coating. Preferably, the carbon coating comprises a polyaromatic sp 2 This coating is preferably obtained by pyrolyzing polyaromatic sp 2 Carbon is formed from carbon precursors because sp 2 Hybridization is largely retained during pyrolysis. Typically, polyaromatic sp 2 Pyrolysis of carbon precursors under reducing conditions leads to sp 2 The domain size of the aromatic carbon increases. Therefore, the inclusion of polyaromatic sp 2The presence of a carbon coating can be determined through knowledge of the precursors used to prepare the coating. The carbon coating can be defined as a coating comprising polyaromatic sp 2 The carbon coating is formed by pyrolysis of a carbon precursor of the carbon. Preferably, the carbon coating is derived from pitch carbon.
[0156] The presence of polyaromatic sp 2 The presence of carbon coatings. For example, Raman spectroscopy provides characteristic peaks (mostly between 1,000-3,500 cm -1 The characteristic peaks can be used to identify the presence of different forms of carbon. 3 A carbon (e.g., diamond) sample has a peak at about 1332 cm -1 Provides narrow characteristic peaks at. 2 Carbon usually provides characteristic D, G and 2D peaks. The relative intensity of the D peak and the G peak (I D / I G ) can provide information about sp 2 With sp 3 The mixed niobium oxide may have an I in the range of 0.85-1.15, or 0.90-1.10, or 0.95-1.05 as observed by Raman spectroscopy. D / I G ratio.
[0157] X-ray diffraction can also be used to provide information about the type of carbon coating. For example, the XRD pattern of the mixed niobium oxide with the carbon coating can be compared with the XRD pattern of the uncoated mixed niobium oxide and / or the XRD pattern of the pyrolyzed sample of the carbon precursor used to prepare the carbon coating.
[0158] The carbon coating may be semi-crystalline.For example, the carbon coating may provide a peak in the XRD pattern of the mixed niobium oxide centered at about 26° 2θ with a width (full width at half maximum) of at least 0.20°, or at least 0.25°, or at least 0.30°.
[0159] Example
[0160] Mixed niobium oxides are synthesized by a solid-state route. In a first step, the precursor materials (Nb2O5, GeO2, ZnO, TiO2, Cr2O3, Al2O3, Fe2O3, ZrO2 and CuO) are ground to a D of less than 20 μm. 50(v / v) particle size. The materials are mixed in a stoichiometric ratio (50 g in total) and combined into a homogeneous powder mixture by impact grinding at 20,000 rpm. The resulting powder is heat treated in an alumina crucible in a muffle furnace in air at T1 = 600°C-1350°C for 0.5-24 hours to provide the desired Wadsley-Roth phase. After the heat treatment, the selected samples (9-11) are removed from the furnace, ground by impact grinding at 20,000 rpm, and then the heat treatment is repeated under similar conditions. Specifically, the precursor mixture is heated to a temperature at or below 800°C at a ramp rate of 5° / min, and then heated to the maximum temperature at a ramp rate of 1° / min for a certain holding period. In some cases, an additional heat treatment step is also applied at T2 = 600°C-1350°C under a N2 atmosphere for 0.5-12 hours. To include anions, there is an additional milling / mixing step for the precursor (PVDF at a 1:10 mass ratio for F; if N is required, C3H6N6 at a 1:3 mass ratio to the parent material can be used), followed by heating in N2 or air atmosphere at T 2a / T 2b = Heat treatment at 300°C-1200°C in one or two steps for 0.5–12 hours.
[0161] If necessary, the final deagglomeration step is utilized by impact grinding or jet grinding to adjust to the desired particle size distribution. Specifically, the material is deagglomerated by impact grinding at 20,000RPM for 10 seconds. The particle size distribution of the dry powder is obtained by a Horiba laser diffraction particle analyzer. The air pressure is maintained at 0.3 MPa. The results are listed in Table 1.
[0162]
[0163] *Comparative sample – unmodified ‘base’ Zn2Nb 34 O 87
[0164] **Induced hypoxia can be calculated from e.g. TGA
[0165] ***Assume that 4 +、Zn 2 +、Fe 3 +、Al 3 + and Nb 5 +, calculated oxygen stoichiometry
[0166] This heat treatment step was performed in an N2 atmosphere. All other steps were performed in an air atmosphere.
[0167] Table 1: Summary of the synthesized materials. Particle size distribution has been assessed by dry powder laser diffraction.
[0168] Material characterization
[0169] The phase purity of the samples was analyzed using a Rigaku Miniflex powder X-ray diffractometer in the 2θ range (10°-70°) at a scanning rate of 1° / min.
[0170] Figure 1 The measured XRD diffraction patterns of samples 1-4 are shown, and Figure 2 XRD diffraction patterns of samples 5-12 are shown. The diffraction patterns have peaks at the same positions (with some shifts up to about 0.2° due to crystal modification) and match the crystallographic database entry JCPDS 28-1478. Some samples were found to have the same Wadsley-Roth block structure (Zn2Nb 34 O 87 ) and has been refined to this mixture. There is no amorphous background noise, and the peaks are sharp and intense. This means that all samples are crystalline, where according to the Scherrer equation and matching Zn2Nb 34 O 87 The crystal structure of the quartz crystals was 45-55 nm in size, which confirmed the existence of the Wadsley-Roth crystal structure.
[0171]
[0172] Table 2 Summary of the unit cell parameters of each sample calculated by Rietveld refinement of the powder XRD spectrum of each sample using the software GSASII, and the average crystallite size calculated over the entire spectrum by the Scherrer equation. 2 Indicates the goodness of fit and accuracy of the Rietveld refinement.
[0173] Electrochemical characterization
[0174] The charge rate of a Li-ion battery cell is often expressed as the "C-rate". A 1C charge rate means the charge current at which the battery cell is fully charged in 1 hour, and a 10C charge means that the battery is fully charged in 1 / 10 of an hour (6 minutes). The C-rate here is defined by the observed reversible capacity of the anode within the voltage limit applied in its second cycle delithiation, i.e., within the voltage limit of 1.1–3.0 V, the anode exhibits 1.0 mAh cm -2Capacity, 1C rate corresponds to an applied 1.0 mA cm -2 In a typical MNO material as described herein, this corresponds to about 200 mA / g of active material.
[0175] Electrochemical tests were performed in half-button cell cells (CR2032 size) for analysis. In the half-button test, the active material was tested in an electrode relative to a Li metal electrode to evaluate its basic performance. In the following examples, the active material composition to be tested was combined with N-methylpyrrolidone (NMP), carbon black (Super P) acting as a conductive additive, and poly(vinylidene fluoride) (PVDF) binder, and mixed using a laboratory-scale centrifugal planetary mixer to form a slurry. The non-NMP composition of the slurry was 92 wt % active material, 3 wt % conductive additive, 5 wt % binder. The slurry was coated on an Al foil current collector by blade coating until 69-75 g m -2 The desired loading was obtained and dried by heating. The electrode was then calendered to a value of 2.6–2.9 g cm at 80 °C. -3 The density was adjusted to achieve a target porosity of 35%-40%. The electrodes were punched into the desired size and combined with a separator (Celgard porous PP / PE), Li metal and electrolyte (1.3M LiPF6 in EC / DEC) in a steel button cell housing and sealed under pressure. The cells were then cycled between 1.1-3.0V at a low current rate (C / 10) at 23°C to achieve 2 full cycles of lithiation and delithiation. After this, the performance of the cells was tested at increasing current densities. During these tests, the cells were cycled asymmetrically at 23°C, first slowly lithiated (C / 5), then increasing the delithiation rate (e.g., 1C, 5C, 10C) to provide capacity retention and provide a nominal voltage at 5C. The nominal voltage relative to Li / Li+ was calculated by dividing the integral of the V / Q curve by the total capacity at 5C during delithiation. No constant voltage step was used. The data of 5 cells prepared from the same electrode coating have been averaged, with the error shown by the standard deviation. Therefore, these data represent a reliable study showing that the material according to the invention achieves improvements compared to previous materials. These data are shown in Tables 4 and 5.
[0176] The cell resistance was calculated from the DC internal resistance (DCIR) of the half coin cell. In a typical measurement, the cell was lithiated to 100% state of charge (SOC), then delithiated to 50% SOC at a rate of C / 10, then after a 0.5 hour rest, a 5C delithiation pulse was applied for 10 seconds, followed by an additional 0.5 hour rest. The DCIR was then calculated from V=IR using the voltage just before the peak from the pulse, and the maximum voltage measured during the pulse.
[0177] The resistivity of the electrode coating was evaluated individually by a 4-point probe method with an Ossila instrument (T2001A3-UK) at 23°C. The slurry was prepared (the active material composition to be tested was combined with N-methylpyrrolidone (NMP), carbon black acting as a conductive additive, and poly(vinylidene fluoride) (PVDF) binder, and mixed using a laboratory-scale centrifugal planetary mixer to form a slurry; the non-NMP composition of the slurry was 80 wt% active material, 10 wt% conductive additive, 10 wt% binder). The slurry was then heated to 1 mg / cm 2 The loading amount was coated on a dielectric mylar film. Discs of electrode size were then punched out and the resistance of the coated film was measured using a 4-point probe. The results of sheet resistance (Ω / sq) are listed in Table 3, where the error is based on the standard deviation of 3 measurements.
[0178] For homogenous, smooth coatings on Cu and Al current collector foils, coatings without visible defects or agglomerates were also prepared as above for these samples using a centrifugal planetary mixer to compositions of up to 94 wt% active material, 4 wt% conductive additive, 2 wt% binder. These can be prepared with PVDF (i.e., NMP-based) and CMC:SBR (i.e., water-based) based binder systems. -2 The coatings can be calendered to 35% to 40% porosity at 80°C for PVDF and 50°C for CMC:SBR at a loading of 1000 Nm. This is important to demonstrate the feasibility of these materials in high energy and high power applications with high active material content.
[0179]
[0180] Table 3: Summary of 4-point probe resistivity measurement results
[0181]
[0182]
[0183] *Comparison samples
[0184] Table 4: Summary of electrochemical test results for Li-ion half-coin cells. In general, it is beneficial to have higher capacity, higher coulombic efficiency, and lower nominal voltage.
[0185]
[0186] *Comparison samples
[0187] Table 5 Summary of additional electrochemical test results for Li-ion half coin cells.
[0188]
[0189] * Compare samples
[0190] Table 6 Summary of additional electrochemical test results for Li-ion half-coin cell
[0191] discuss
[0192] Mixed niobium oxide sample 1* has been modified by the cation substitution method described in sample 3, with the focus on using Ge 4+ Replace Zn 2+ In samples 5-8, Cr 3+ The cation replaces the Zn 2+ cations, and with Ti 4+ The cation replaces the Nb 5+ cations, thus spanning a wide range of variables a and b. Sample 10 was treated with Fe 3+ Replaced Nb 5+ Sample 11 was made of Al 3+ Replace Zn 2+ Sample 12 is based on Cu2Nb 34 O 87 , where Cr 3+ The cation replaces the Cu 2+ Cations and Ti 4+ The cation replaces the Nb 5+ cations. The increased valence can be achieved by partial oxygen excess (i.e., c<0) and / or Nb 5+The reduced vacancies can be compensated by the formation of oxygen vacancies (i.e., c>0). These modifications are expected to provide advantages over the basic crystal structure of sample 1* by a combination of (a) changed ionic radius, (b) changed valence, and (c) changed voltage. The changed ionic radius can produce beneficial changes in electrochemical performance due to changes in unit cell size and local deformation of the crystal structure that change the available lithiation sites or lithiation pathways - potentially improving Coulombic efficiency, capacity, performance at high rates, and life. The changed valence provides significantly improved conductivity of the material due to the availability of available intermediate energy levels for charge carriers. These effects are shown by the lower resistivity of the modified samples relative to sample 1* observed in Table 3, and by the improvements in specific capacity, Coulombic efficiency, delithiation voltage at 5C, and capacity retention at 1C, 5C, and 10C observed in Tables 4-6. These are key results that demonstrate the utility of the modified mixed niobium oxide according to the present invention for use in high-power Li-ion battery cells designed for fast charge / discharge.
[0193] Table 2 shows the changes in unit cell parameters observed after cation exchange, which are observed due to changes in the ionic radius and electronic structure of these materials.
[0194] It is expected that similar benefits will be observed when this material is used in Li-ion battery cells via the cation exchange method described.
[0195] Mixed niobium oxide sample 1* is modified by introducing induced oxygen deficiency via heat treatment in an inert or reducing atmosphere to provide sample 2. By treating the 'base' oxide at high temperature in an inert or reducing atmosphere, the oxide can be partially reduced and maintain this state when returned to room temperature and exposed to an air atmosphere. This is accompanied by a significant color change, for example the color of sample 2 is gray / black, while sample 1* is white. This color change demonstrates a significant change in the electronic structure of the material, allowing the material to interact with visible light of different energies (i.e., wavelengths) due to the reduction in the band gap. This is reflected in sample 2, which exhibits an improved delithiation voltage at a rate of 5C, which corresponds to a reduction in the polarization level in the battery cell.
[0196] The induced oxygen deficiency causes defects in the crystal structure, such as where oxygen anions have been removed, and the overall redox state of the cations is in turn weakened. This provides additional energy states, significantly increasing the material conductivity, and changes the band gap energy, as evidenced by the color change. This is shown by the lower resistivity observed for sample 2 relative to sample 1* in Table 3. If the induced oxygen deficiency is present in excess of 5 atomic % (i.e., c>4.35), the crystal structure may be less stable.
[0197] Mixed niobium oxide sample 1* has been substituted by anions (with F - Replace O 2- ) was modified to provide Sample 4. An increase in specific capacity was observed (Tables 4 and 5).
[0198] It is expected that similar benefits will be observed when used in a Li-ion battery cell using any of the described mixed niobium oxides, within the described limitations, utilizing any combination of M1, M2, M3, Q, a, b, c, and d.
[0199] Mixture with LTO
[0200] The modified mixed niobium oxide was tested as an active electrode material in conjunction with commercial materials, demonstrating the utility of the modified mixed niobium oxide for incorporation into and improvement over existing battery technology.
[0201] Commercial grade LTO (Li4Ti5O 12 ) were purchased from Targray Technology International Inc, and the properties are listed in Table E1 (Sample E1). Wadsley-Roth materials were synthesized in-house via a solid-state route. In a first step, the precursor materials (Nb2O5, Cr2O3, ZnO, and TiO2) were mixed in stoichiometric proportions (200 g total) and ball milled at 550 rpm for 3 hours at a ball to powder ratio of 10:1. The resulting powder was heat treated in an alumina crucible in a muffle furnace in air at T1 = 1100°C for 12 hours to provide the desired Wadsley-Roth phase.
[0202] The active electrode material mixture of MNO and LTO was obtained by low-energy to high-energy powder mixing / blending techniques, such as mixing by rotation in multiple directions, V-blending on a single axis, planetary mixing, centrifugal planetary mixing, high shear mixing and other typical mixing / blending techniques. In this case, 5 g of batch material was mixed by a centrifugal planetary mixer at 2000 rpm for 3 minutes and 10 times.
[0203]
[0204] Table E1: Summary of materials utilized. Particle size distribution has been evaluated by dry powder laser diffraction and surface area has been evaluated by BET method using N2. *From manufacturer specification sheet.
[0205] Material characterization
[0206] The phase purity of the samples was analyzed using a Rigaku Miniflex powder X-ray diffractometer in the 2θ range (20°-70°) at a scanning rate of 1° / min. The diffraction pattern of sample E1 matched the JCPDS crystallographic database entry JCPDS 49-0207, which corresponds to Li4Ti5O 12 The spinel crystal structure of E2 is shown in Figure 2. There is no amorphous background noise, and the peaks are sharp and intense. This means that the sample is crystalline, and according to the Scherrer equation, the crystallite size is 43 ± 7 nm. The diffraction pattern of sample E2 confirms the expected Wadsley-Roth crystal structure of Zn2Nb 34 O 87 There is no amorphous background noise, and the peaks are sharp and intense. This means that the sample is phase pure and crystalline, and according to the Scherrer equation, the crystallite size is 49 ± 6 nm.
[0207] The particle size distribution of the dry powder was obtained by a Horiba laser diffraction particle analyzer. The air pressure was maintained at 0.3 MPa. The results are listed in Table E1. BET surface area analysis was performed on a BELSORP-miniX instrument with N2 at 77.35K and is listed in Table E1.
[0208] Electrochemical characterization
[0209] Electrochemical testing was performed in a half-button cell (CR2032 size) for analysis. There are some differences in the test methods used for the above samples 1-12, which means that the results may not be directly comparable. In the half-button test, the active material is tested in an electrode relative to a Li metal electrode to evaluate its basic performance. In the following examples, the active material composition to be tested is combined with N-methylpyrrolidone (NMP), carbon black acting as a conductive additive, and poly(vinylidene fluoride) (PVDF) binder, and mixed using a laboratory-scale centrifugal planetary mixer to form a slurry. The non-NMP composition of the slurry is 90 wt% active material, 6 wt% conductive additive, 4 wt% binder. The slurry is coated on an Al foil current collector by blade coating until 5.7–6.5 mg cm -2 The electrode was then calendered at 80 °C to a loading of 2.00–3.75 g cm -3density (depending on the material density) to achieve a target porosity of 35%-40%. Porosity is calculated as the measured electrode density divided by the weighted average density of each component of the composite electrode coating film. The electrodes are punched into the desired size and the electrodes are combined with separators (Celgard porous PP / PE), Li metal and electrolyte (1.3MLiPF6 in EC / DEC) in a steel button cell housing and sealed under pressure. Then cycled between 1.1-3.0V at a low current rate (C / 10) to achieve 2 full cycles of lithiation and delithiation. After this, the performance of the battery cell is tested at an increased current density. During the rate test, the battery cell is cycled asymmetrically, first slowly lithiation (C / 5, CV step to C / 20 current density at 1.1V), and then the delithiation rate is increased to perform delithiation rate testing. All electrochemical tests were performed at 23°C in a thermally controlled environment.
[0210] The first cycle efficiency was calculated as the fraction of delithiation capacity / lithiation capacity at C / 10 in the first cycle. The nominal voltage at each C-rate was determined by integrating the voltage-capacity curve and then dividing it by the total capacity.
[0211] To quantify the significance of the differences observed in the data, an error calculation was performed and applied to the values of specific capacity. The error of these data was approximated to be the same as that of the lowest loading electrode (5.7 mg cm) on a 14 mm electrode disk using a microbalance (±0.1 mg). -2 ). This provides an error of ±1.1%, which has been applied to each capacity measurement. Since the instrument accuracy far exceeds the significant figures stated and these values are independent of balancing errors, it is assumed that the errors in coulombic efficiency, capacity retention and voltage are negligible for the cells tested.
[0212]
[0213] Table E2: Summary of electrochemical tests performed on samples E1 and E2. For each test, reference is also made to the electrode conditions achieved, providing smooth electrodes free of agglomerates, which demonstrate good adhesion and cohesion to the current collector.
[0214]
[0215] Table E3: Summary of electrochemical testing results for Li-ion half coin cells.
[0216]
[0217] Table E4: Summary of electrochemical testing results of Li-ion half coin cells at increasing current densities.
[0218]
[0219] Table E5: Summary of nominal delithiation voltages at each C-rate.
[0220] ***
[0221] Although the present invention has been described in conjunction with the above exemplary embodiments, many equivalent modifications and variations will be apparent to those skilled in the art when this disclosure is given. Therefore, the above exemplary embodiments of the present invention are considered to be illustrative rather than restrictive. Various changes may be made to the described embodiments without departing from the spirit and scope of the present invention. In order to avoid any doubt, any theoretical explanation provided herein is provided to improve the reader's understanding. The inventor does not wish to be bound by any of these theoretical explanations. Any section headings used herein are only for organizational purposes and should not be construed as limiting the subject matter described.
Claims
1. An active electrode material comprising a mixed niobium oxide, wherein the mixed niobium oxide has a composition M1 a M2 2- a M3 b Nb 34-b O 87-c-d Q d ,in: M1 and M2 are different; M1 is selected from the group consisting of Mg, Ca, Sr, Y, La, Ce, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, In, Si, Ge, Sn, Pb, P, Sb, Bi, and mixtures thereof; M2 is Zn or Cu; M3 is selected from the group consisting of Mg, Ca, Sr, Y, La, Ce, Ti, Zr, Hf, V, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, In, Si, Ge, Sn, Pb, P, Sb, Bi, and mixtures thereof; Q is selected from F, Cl, Br, I, N, S, Se and mixtures thereof; 0≤a<1.0; 0≤b≤3.4; -0.5≤c≤4.35; 0≤d≤4.35; One or more of a, b, c, and d is not equal to 0; and When a, b, and d are equal to zero, c is greater than zero.
2. The active electrode material according to claim 1, wherein (i) a>0; and / or (ii) 0 ≤ a ≤ 0.6; and / or (iii)0≤a≤0.
2.
3. An active electrode material as claimed in any preceding claim, wherein (i) b>0; and / or (ii) 0 ≤ b ≤ 1.5; and / or (iii) 0 ≤ b ≤ 0.3; or (iv)b=0.
4. An active electrode material as claimed in any preceding claim, wherein (i) c ≠ 0; or (ii) 0 ≤ c ≤ 4.35; or (iii)0 <c≤4.35。 5. An active electrode material as claimed in any preceding claim, wherein (i) d > 0; and / or (ii) 0 ≤ d ≤ 3.0; and / or (iii) 0 ≤ d ≤ 2.17; or (iv)d=0.
6. An active electrode material as claimed in any preceding claim, wherein at least one of a and b > 0, or wherein both a and b > 0.
7. An active electrode material as claimed in any preceding claim, wherein M1 is selected from (i) Mg, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, Si, Ge, Sn, P and mixtures thereof; or (ii) Mg, Ti, Zr, V, Nb, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, B, Al, Si, Ge, P and mixtures thereof; or (iii) Mg, Zr, V, Cr, Mo, W, Fe, Cu, Zn, Al, Ge, P and mixtures thereof.
8. An active electrode material as claimed in any preceding claim, wherein M2 is Zn.
9. An active electrode material as claimed in any preceding claim, wherein M3 is selected from (i) Mg, Ti, Zr, Hf, V, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, Si, Sn, P and mixtures thereof; or (ii) Mg, Ti, Zr, V, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Si, P and mixtures thereof; or (iii) Ti, Zr, V, Cr, Mo, W, Fe, Cu, Zn, Al, P and mixtures thereof.
10. An active electrode material as claimed in any preceding claim, wherein (i) M1 has a 6-coordinate ionic radius and / or (ii) M1 has a 6-coordinated 2+ Different 6-coordinate ionic radii, optionally with a smaller radius than the 6-coordinate M2 2+ 6-coordinate ionic radius of (iii) M1 has a 6-coordinate ionic radius 11. An active electrode material as claimed in any preceding claim, wherein (i) M3 has a 6-coordinate ionic radius and / or (ii) M3 has a 6-coordinated Nb 5+ Different 6-coordinate ionic radii, optionally with a radius greater than that of the 6-coordinate Nb 5+ 6-coordinate ionic radius of (iii) M3 has a 6-coordinate ionic radius 12. An active electrode material as claimed in any preceding claim, wherein (i) M1 has a valence equal to or higher than 2+, optionally a higher valence; or (ii) M3 has a valence lower than 5+; or (iii) M1 has a valence equal to or higher than 2+ and M3 has a valence lower than 5+.
13. An active electrode material as claimed in any preceding claim, wherein M1 does not comprise Nb and wherein M3 does not comprise Zn and / or Cu.
14. An active electrode material as claimed in any preceding claim, wherein (i) Q is selected from F, Cl, N, S and mixtures thereof; or (ii) Q is selected from F, N and mixtures thereof; or (iii)where Q is F.
15. An active electrode material according to any preceding claim, wherein: M1 is selected from Cr, Al, Ge and mixtures thereof; M3 is selected from Ti, Zr, Fe and mixtures thereof and optionally includes Ti; 0<a<1.0; 0<b≤1.5; -0.5≤c≤4.35; d=0。 16. An active electrode material according to any preceding claim, wherein: M1 is Cr; M2 is Zn; M3 is selected from Ti, Zr and mixtures thereof and optionally includes Ti; 0.01<a<1.0; 0.01<b<1.0; -0.5≤c≤2; d=0。 17. An active electrode material according to any preceding claim, wherein the mixed niobium oxide is oxygen-deficient, optionally wherein the mixed niobium oxide has induced oxygen deficiency.
18. An active electrode material according to any preceding claim, wherein the mixed niobium oxide is coated with carbon.
19. The active electrode material of claim 18, wherein the carbon coating comprises polyaromatic sp 2 Carbon, optionally wherein the carbon coating is derived from pitch carbon.
20. An active electrode material according to any preceding claim, wherein the mixed niobium oxide is in particulate form, optionally wherein the mixed niobium oxide has a D in the range of 0.1-100 μm, or 0.5-50 μm, or 1-20 μm. 50 Particle size.
21. An active electrode material according to any preceding claim, wherein the mixed niobium oxide has a molecular weight in the range of 0.1 to 100 m 2 / g, or 0.5-50m 2 / g, or 1-20m 2 The BET surface area is in the range of 1000 Å / g.
22. An active electrode material according to any preceding claim, wherein the mixed niobium oxide further comprises Li and / or Na.
23. An active electrode material according to any preceding claim, wherein the crystal structure of the mixed niobium oxide as determined by X-ray diffraction corresponds to Zn2Nb 34 O 87 and Cu2Nb 34 O 87 The crystal structure of one or more of: or corresponding to Zn2Nb 34 O 87 of the crystal structure.
24. An active electrode material according to any preceding claim, comprising the mixed niobium oxide and at least one other component; optionally wherein the at least one other component is selected from the group consisting of a binder, a solvent, a conductive additive, a different active electrode material and mixtures thereof.
25. The active electrode material of claim 24, wherein the at least one other component is a different active electrode material selected from the group consisting of different mixed niobium oxides, lithium titanium oxides, niobium oxides and mixtures thereof having a composition as defined in any preceding claim.
26. An electrode comprising the active electrode material of any one of claims 1 to 25 in electrical contact with a current collector.
27. An electrochemical device comprising an anode, a cathode and an electrolyte disposed between the anode and the cathode, wherein the anode comprises an active electrode material according to any one of claims 1 to 25; optionally wherein the electrochemical device is a lithium ion battery or a sodium ion battery.
28. The electrochemical device of claim 27, wherein the electrochemical device is a lithium ion battery having a reversible anode active material specific capacity of greater than 190 mAh / g at 20 mA / g, wherein the battery can be charged and discharged at a current density of 200 mA / g or greater, or 1000 mA / g or greater, or 2000 mA / g or greater, or 4000 mA / g or greater relative to the anode active material while retaining greater than 70% of the initial cell capacity at 20 mA / g.
29. A method for preparing a mixed niobium oxide as defined by any one of claims 1 to 23, the method comprising the steps of: providing one or more precursor materials; mixing the precursor materials to form a precursor material mixture; and The precursor material mixture is heat treated at a temperature in the range of 400° C. to 1350° C. or 800° C. to 1250° C. to provide the mixed niobium oxide.
30. The method of claim 29, further comprising the steps of: mixing the mixed niobium oxide with a precursor comprising element Q to provide a further precursor material mixture; and The additional precursor material mixture is heat treated at a temperature in the range of 300°C to 1200°C or 800°C to 1200°C, optionally under reducing conditions, to provide a mixed niobium oxide comprising the element Q.
31. The method according to claim 29 or 30, comprising the further step of heat treating the mixed niobium oxide or the mixed niobium oxide comprising the element Q under reducing conditions in a temperature range of 400°C to 1350°C or 800°C to 1250°C, thereby inducing oxygen vacancies in the mixed niobium oxide.
32. The method of any one of claims 29-31, further comprising the steps of: The mixed niobium oxide or the mixed niobium oxide containing element Q is mixed with a polyaromatic sp 2 combining carbon precursors of carbon to form an intermediate material; as well as The intermediate material is heated under reducing conditions to pyrolyze the carbon precursor, thereby forming a carbon coating on the mixed niobium oxide and inducing oxygen vacancies in the mixed niobium oxide.