Core-shell type ternary precursor, preparation method thereof and positive electrode material
The core-shell ternary precursor is prepared by co-precipitation method, and the tungsten doped core and aluminum cladding shell are used to solve the problems of uneven doping and complex process in the existing technology, and achieve high stability and excellent performance of the material. The electrochemical performance improves the cycle and thermal stability of the battery.
Patent Information
- Application Number
- CN202410750786.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-11
AI Technical Summary
The existing ternary precursors have uneven coating of doping elements and complicated processes during the preparation process, resulting in insufficient material stability and cycle performance, and high-nickel materials are prone to cracks and electrolyte corrosion problems.
The core-shell ternary precursor is prepared in one step by co-precipitation method. By doping tungsten in the core and aluminum in the shell, a core-shell structure is formed to enhance the structural stability and electrochemical performance of the material.
It achieves high stability, long life, excellent electrochemical performance and high rate performance of the material, effectively inhibits electrolyte corrosion and improves the cycle stability and thermal stability of the battery.
Smart Images

Figure CN118754208A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ternary precursors, and in particular to a core-shell type ternary precursor and a preparation method thereof and a positive electrode material. Background Art
[0002] Lithium-ion batteries are environmentally friendly new energy sources, which are widely used due to their high energy density, cycle performance and stability. Among them, battery cathode materials are the key breakthrough in the development of lithium-ion battery technology. The early LiCoO2 cathode materials are high in cost and toxic and are no longer applicable. The ternary cathode materials that replace part of Co with other elements (Ni, Mn) have high specific capacity, low cost, large reversible capacity and cycle stability, and have become a research hotspot.
[0003] The 5 series and 6 series ternary precursors on the market have high cobalt content and low energy density. In order to improve the energy density, 8 series and 9 series ternary precursors are prepared. They have high nickel content and high energy density but poor stability, and the precursors are prone to cracks during the preparation process.
[0004] To improve the defects in the above materials, bulk doping and surface coating of the precursors are simple and feasible improvement strategies. Doping elements can enhance the structural stability of the material to a certain extent, while surface coating can inhibit crack propagation, prevent the battery structure from collapsing during charging and discharging, and effectively prevent the electrolyte from corroding the positive electrode material. However, in the specific preparation process, there are problems such as uneven element doping and coating, complex process, and low content of doped elements.
[0005] Doping Al in the ternary precursor can improve the stability of the material, improve the cation mixing phenomenon of high-nickel materials, thereby reducing the lattice distortion phenomenon and inhibiting the precipitation of nickel ions and manganese ions from the inside of the material, thereby improving the material's cycle performance. W doping can increase the operating voltage and energy density of lithium-ion batteries, increase the spacing between layered structures, improve rate performance, stabilize the precursor structure, and enhance the thermal stability of the positive electrode material.
[0006] CN117430173A prepared a ternary precursor with an Al concentration gradient and mixed it with an Al source and a Li source for calcination to prepare a positive electrode material. This method firstly uniformly coated the aluminum source on the surface of the nickel-cobalt-manganese precursor, and then mixed it with a lithium source, thereby avoiding the technical difficulty that part of the aluminum cannot be incorporated into the positive electrode material lattice during the high-temperature solid phase reaction. However, after the precursor was mixed with the Al source by ball milling, the degree of Al coating on the surface of the precursor was not high, and the Al coating effect was not effectively exerted.
[0007] CN104916837A prepares an aluminum-doped ternary cathode material precursor by a coprecipitation method, and then mixes it with a lithium source and a boron source and calcines it to obtain a cathode material, thereby improving the cycle performance of the material.3+ and Ni 2+ The ionic radius difference between them is large, and delamination is likely to occur at the coating interface.
[0008] CN109904432A dopes tungsten by mixing a ternary precursor with a tungsten source and a lithium source and then calcining them. However, the homogeneity of the ground mixture in this method is poor, which affects the uniformity of tungsten doping. In addition, when sintering with the lithium source, there will be competitive site occupation, thus affecting the sintering effect of the cathode material.
[0009] In summary, the doping element cannot be effectively coated on the surface of the precursor, delamination occurs between the coating layer and the precursor, the doping and coating are carried out in two steps and are ball-milled and mixed, the process is complex, and the requirements for equipment are high, which are urgent problems to be solved at present. Summary of the Invention
[0010] To solve the above technical problems, the present invention provides a core-shell type ternary precursor, its preparation method and a cathode material. The ternary precursor is prepared by a one-step coprecipitation method, which is simple, fast, has high production efficiency, strong adaptability to various different metal solutions, and the cathode material prepared by doping and modifying the precursor often has high stability, high battery working voltage and energy density, and high rate performance.
[0011] To achieve this purpose, the present invention adopts the following technical solutions:
[0012] In the first aspect, the present invention provides a core-shell type ternary precursor, and the core-shell type ternary precursor includes a core and a shell coated outside the core; the expression of the core is Ni x Co y Mn z (OH) 2-a (WO4) a , where 0 < x < 1, 0 < y < 1, 0 < z < 1, and x + y + z = 1, and the value range of a is 0.01 to 1; the shell contains aluminum.
[0013] The core of the core-shell type ternary precursor provided by the present invention is doped with tungsten. The doping of tungsten may enhance the structural stability of the cathode material, thereby reducing the structural collapse and degradation during charge and discharge, and prolonging the service life of the battery; moreover, the doped tungsten can help reduce the phase change of the cathode material at high voltages, thereby reducing capacity attenuation and improving the cycle stability of the battery. Furthermore, the high melting point characteristic of tungsten may help improve the thermal stability of the battery and reduce the risk of thermal runaway. Due to the conductivity of tungsten, the doped material may perform better during high-current charge and discharge, that is, the rate performance is improved. And the shell contains aluminum, and the aluminum coating may help reduce the cation mixing phenomenon in the core-shell type ternary precursor, maintain the orderliness of the crystal structure, and cooperate with the tungsten doping in the core to jointly improve the application prospect of the core-shell type ternary precursor.
[0014] Among them, 0 < x < 1. For example, it can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, or 0.9, etc., but not limited to the listed values. Other unlisted values within this range are equally applicable; 0 < y < 1. For example, it can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, or 0.9, etc., but not limited to the listed values. Other unlisted values within this range are equally applicable; 0 < z < 1. For example, it can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, or 0.9, etc., but not limited to the listed values. Other unlisted values within this range are equally applicable. The value range of a is 0.01 to 1. For example, it can be 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or 1, etc., but not limited to the listed values. Other unlisted values within this range are equally applicable.
[0015] Preferably, the expression of the outer shell is Ni b Co c Mn d Al e (OH) 2(b+c+d)+3e , where 0 < b < 1, 0 < c < 1, 0 < d < 1 and 0 < e < 1.
[0016] Specifically, 0 < b < 1. For example, it can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, or 0.9, etc., but not limited to the listed values. Other unlisted values within this range are equally applicable; 0 < c < 1. For example, it can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, or 0.9, etc., but not limited to the listed values. Other unlisted values within this range are equally applicable; 0 < d < 1. For example, it can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, or 0.9, etc., but not limited to the listed values. Other unlisted values within this range are equally applicable; 0 < e < 1. For example, it can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, or 0.9, etc., but not limited to the listed values. Other unlisted values within this range are equally applicable.
[0017] Preferably, the aluminum content in the shell is 0.01-2wt%, for example, it can be 0.01wt%, 0.1wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt% or 12wt%, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0018] Preferably, the size of the core is 3 to 14 μm, for example, it can be 3 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm or 14 μm, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0019] Preferably, the shell thickness of the outer shell is 0.1 to 4 μm, for example, it can be 0.1 μm, 0.2 μm, 0.3 μm, 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm or 4 μm, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0020] Preferably, the particle size range of the core-shell type ternary precursor is 3.1 to 18 μm, for example, it can be 3.1 μm, 3.2 μm, 3.5 μm, 4 μm, 5 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 15 μm or 18 μm, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0021] The main advantage of the core-shell ternary precursor described in the present invention is that the particle size is highly controllable and the particle size can be controlled within the above range, thereby having better electrochemical performance.
[0022] In a second aspect, the present invention provides a method for preparing the core-shell ternary precursor according to the first aspect, the preparation method comprising the following steps:
[0023] Under a reaction atmosphere, a base liquid containing ammonia is prepared, and then a ternary salt solution, a tungstate solution, a precipitant and a complexing agent are introduced into the base liquid to carry out a first reaction to form a core.
[0024] The introduction of the ternary salt solution is stopped, and a mixed salt solution containing aluminum salt is introduced at the same time to carry out a second reaction to form a shell covering the outside of the core.
[0025] The core-shell ternary precursor described in the first aspect of the present invention is preferably prepared by the preparation method of the second aspect. Through the co-precipitation method, the precursor in the kettle is guaranteed to grow and form once. The preparation method is simple, the particle size is highly controllable, the application prospect is broad, and the aluminum coating is not likely to separate from the core.
[0026] It is worth noting that in the present invention, it is necessary to strictly control the introduction of the ternary salt solution first and then the mixed salt solution containing the aluminum salt, so as to form a core first and then a shell coated on the outside of the core, which can ensure that the particle size of the core-shell type ternary precursor finally obtained is within the ideal range. The core-shell precursor obtained by this method can effectively improve the surface structure of the precursor, inhibit the expansion of surface cracks of the high-nickel large-particle precursor, and can also effectively inhibit the corrosion of the electrolyte to the positive electrode material, thereby improving the battery life.
[0027] Preferably, the reaction atmosphere comprises nitrogen and / or air.
[0028] Preferably, the precipitant comprises an alkaline solution, and preferably the precipitant is a sodium hydroxide solution.
[0029] Preferably, the concentration of the alkaline solution is 20-40wt%, for example, it can be 20wt%, 23wt%, 25wt%, 27wt%, 29wt%, 32wt%, 34wt%, 36wt%, 38wt% or 40wt%, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0030] Preferably, the complexing agent comprises aqueous ammonia and / or ammonium salt solution.
[0031] Preferably, the concentration of the aqueous ammonia and / or ammonium salt solution is 10-20wt%, for example, it can be 10wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt% or 20wt%, etc., but is not limited to the listed values, and other unlisted values within this range are also applicable.
[0032] Preferably, the ammonia concentration of the base liquid is 6 to 10 g / L, for example, it can be 6 g / L, 6.5 g / L, 7 g / L, 7.5 g / L, 8 g / L, 9 g / L, 9.5 g / L or 10 g / L, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0033] Preferably, the pH of the base solution is 9-12, for example, 9, 9.5, 10, 10.3, 10.5, 10.7, 10.9, 11.2, 11.4, 11.6, 11.8 or 12, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0034] Preferably, the ternary salt solution comprises a nickel salt, a cobalt salt and a manganese salt.
[0035] Preferably, the nickel salt comprises nickel nitrate and / or nickel sulfate.
[0036] Preferably, the cobalt salt comprises cobalt nitrate and / or cobalt sulfate.
[0037] Preferably, the manganese salt comprises manganese nitrate and / or manganese sulfate.
[0038] Preferably, the molar ratio of Ni:Co:Mn in the ternary salt solution is x:y:z, where 0 < x < 1, 0 < y < 1, 0 < z < 1, and x + y + z = 1.
[0039] Preferably, the temperature of the first reaction is 50 - 60°C. For example, it can be 50°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C or 60°C, etc., but is not limited to the listed values, and other unlisted values within this range are equally applicable.
[0040] Preferably, the feeding rate of the ternary salt solution is 1 - 10 L / h. For example, it can be 1 L / h, 2 L / h, 3 L / h, 4 L / h, 5 L / h, 6 L / h, 7 L / h, 8 L / h, 9 L / h or 10 L / h, etc., but is not limited to the listed values, and other unlisted values within this range are equally applicable.
[0041] In the present invention, preferably controlling the feeding rate of the ternary salt solution within the above range can better ensure the complete progress of the precipitation reaction and further control the growth particle size of the core - shell precursor within a reasonable range.
[0042] Preferably, the tungsten concentration in the tungstate solution is 100 - 5000 mg / L. For example, it can be 100 mg / L, 200 mg / L, 500 mg / L, 700 mg / L, 800 mg / L, 1000 mg / L, 1200 mg / L, 2000 mg / L, 3000 mg / L, 4000 mg / L or 5000 mg / L, etc., but is not limited to the listed values, and other unlisted values within this range are equally applicable.
[0043] Preferably, the feeding rate of the tungstate solution is 0.1 - 5 L / h. For example, it can be 0.1 L / h, 0.2 L / h, 0.3 L / h, 0.4 L / h, 0.5 L / h, 0.6 L / h, 0.7 L / h, 0.8 L / h, 0.9 L / h, 1 L / h, 1.2 L / h, 2 L / h, 3 L / h, 4 L / h, 4.5 L / h or 5 L / h, etc., but is not limited to the listed values, and other unlisted values within this range are equally applicable.
[0044] The present invention preferably controls the introduction speed of the tungstate solution within the above range, which can further avoid the problem of low tungsten doping amount and unclear electrical performance improvement caused by low introduction speed, and can ensure the particle size of the ternary precursor particles, effectively reduce the difficulty of preparation, and reduce raw material waste.
[0045] Preferably, the tungstate solution includes ammonium tungstate.
[0046] Preferably, the introduction rate of the precipitant is 0.1 to 10 L / h, for example, 0.1 L / h, 0.2 L / h, 0.3 L / h, 0.4 L / h, 0.5 L / h, 0.6 L / h, 0.7 L / h, 0.8 L / h, 0.9 L / h, 1 L / h, 2 L / h, 3 L / h, 4 L / h, 5 L / h, 8 L / h, 9 L / h or 10 L / h, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0047] Preferably, the introduction rate of the complexing agent is 0.1 to 10 L / h, for example, it can be 0.1 L / h, 0.2 L / h, 0.3 L / h, 0.4 L / h, 0.5 L / h, 0.6 L / h, 0.7 L / h, 0.8 L / h, 0.9 L / h, 1 L / h, 2 L / h, 3 L / h, 4 L / h, 5 L / h, 8 L / h, 9 L / h or 10 L / h, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0048] Preferably, the introduction rate of the precipitant is adjusted to control the pH to 9-12, for example, 9, 9.4, 9.7, 10, 10.4, 10.7, 11, 11.4, 11.7 or 12, etc., but not limited to the listed values, and other values not listed within the range are also applicable.
[0049] The present invention preferably controls the pH in the above range during the precipitation process, which is more conducive to forming a core-shell precursor with a target particle size.
[0050] Preferably, the introduction rate of the complexing agent is adjusted to control the ammonia concentration to 4-10 g / L, for example, it can be 4 g / L, 5 g / L, 5.6 g / L, 6.2 g / L, 6.7 g / L, 7.3 g / L, 7.8 g / L, 8.4 g / L, 8.9 g / L, 9.5 g / L or 10 g / L, but is not limited to the listed values, and other values not listed within this range are also applicable.
[0051] The present invention preferably controls the ammonia concentration within the above range, which can be more conducive to obtaining a core-shell precursor with moderate density, thereby avoiding the problem that lithium ions are difficult to diffuse during the sintering process and ultimately lead to a decrease in the charge and discharge performance of the positive electrode material; and can obtain primary crystal grains with larger particle size, further improving the stability of the positive electrode material.
[0052] Preferably, the particle size of the core is 5μm to 14μm, for example, it can be 5μm, 5.5μm, 6μm, 6.5μm, 7μm, 8μm, 9μm, 9.5μm, 10μm, 11μm, 12μm, 13μm or 14μm, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0053] Preferably, the mixed salt solution containing aluminum salt comprises a ternary salt solution and aluminum salt.
[0054] Preferably, the aluminum salt comprises aluminum sulfate and / or aluminum nitrate.
[0055] Preferably, the aluminum concentration in the mixed salt solution containing aluminum salt is 100-5000 mg / L, for example, it can be 100 mg / L, 200 mg / L, 300 mg / L, 400 mg / L, 500 mg / L, 600 mg / L, 1000 mg / L, 1200 mg / L, 1500 mg / L, 2000 mg / L, 3000 mg / L, 4000 mg / L or 5000 mg / L, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0056] Preferably, the introduction rate of the mixed salt solution containing aluminum salt is 1 to 10 L / h, for example, it can be 1 L / h, 2 L / h, 3 L / h, 4 L / h, 5 L / h, 6 L / h, 7 L / h, 8 L / h, 9 L / h or 10 L / h, but is not limited to the listed values, and other values not listed within this range are also applicable.
[0057] The present invention firstly controls the addition of the mixed salt solution containing aluminum salt after the core is formed, and the growth of the aluminum-doped shell is at the end of the growth, the particle size is relatively large, and it is not suitable to feed alone during the reaction. Therefore, Al is doped in the ternary salt solution and fed together, which is more conducive to the combination of the aluminum shell and the core, and avoids the peeling of the aluminum shell.
[0058] Moreover, the present invention further preferably controls the introduction rate of the mixed salt solution containing aluminum salt to 1-10 L / h, so as to ensure that the particle size is uniform and large during the growth process, and small particle products are not likely to appear.
[0059] Preferably, the temperature of the second reaction is 50-60°C, for example, it can be 50°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C or 60°C, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0060] Preferably, the preparation method further comprises: sequentially performing solid-liquid separation, washing the solid phase and drying on the reacted material after the shell is formed, so as to obtain the core-shell type ternary precursor.
[0061] The present invention has no special limitation on the solid-liquid separation in the above process. Any device and method for solid-liquid separation known to those skilled in the art can be used, and can also be adjusted according to the actual process, such as filtration, centrifugation or sedimentation separation, or a combination of different methods.
[0062] The present invention has no particular limitation on the drying in the above process. Any drying device and method known to those skilled in the art can be used, and can also be adjusted according to the actual process, for example, it can be air drying, vacuum drying, oven drying or freeze drying, or a combination of different methods.
[0063] As a preferred technical solution of the present invention, the preparation method comprises the following steps:
[0064] Under a protective atmosphere, a base liquid with a pH of 9 to 12 and an ammonia concentration of 6 to 10 g / L is prepared, and then a ternary salt solution is introduced into the base liquid at a rate of 1 to 10 L / h, a tungstate solution with a tungsten concentration of 100 to 5000 mg / L is introduced at a rate of 0.1 to 5 L / h, a precipitant is introduced at a rate of 0.1 to 10 L / h, and a complexing agent is introduced at a rate of 0.1 to 10 L / h, and the introduction rate of the precipitant is adjusted to control the pH to 9 to 12; the introduction rate of the complexing agent is adjusted to control the ammonia concentration to 5 to 10 g / L, and a first reaction is carried out at 50 to 60° C. to form a core;
[0065] Stop feeding the ternary salt solution, and simultaneously feed a mixed salt solution containing aluminum salt with an aluminum concentration of 100 to 5000 mg / L at 1 to 10 L / h, and perform a second reaction at 50 to 60° C. to form a shell covering the outside of the core;
[0066] The reacted material after the shell is formed is sequentially subjected to solid-liquid separation, solid phase washing and drying to obtain the core-shell type ternary precursor.
[0067] In a third aspect, the present invention provides a positive electrode material, which includes a positive electrode active material made from the core-shell type ternary precursor described in the first aspect.
[0068] The positive electrode material prepared in the third aspect of the present invention has excellent electrochemical properties and can improve the battery life.
[0069] The present invention has no limitation on the structure of the positive electrode material and other materials, and any structure and other materials that can be used for the positive electrode material and are known to those skilled in the art can be used.
[0070] Compared with the prior art, the present invention has at least the following beneficial effects:
[0071] (1) The core-shell type ternary precursor provided by the present invention has tungsten doped in the core and aluminum doped in the outer part, and has the advantages of both. The core and the shell cooperate with each other, which can effectively improve the surface structure of the precursor, inhibit the expansion of cracks on the surface of the high-nickel large-particle precursor, and effectively inhibit the corrosion of the electrolyte to the positive electrode material, thereby improving the battery life. Under preferred conditions, after being prepared into a positive electrode material and assembled into a battery, the rate performance is above 91.59%, the 0.1C charge and discharge efficiency is above 88.26%, and the discharge capacity retention rate after 100 cycles is above 93.25%;
[0072] (2) The preparation method of the core-shell type ternary precursor provided by the present invention is prepared by a co-precipitation method, which is simple and easy to operate, low in cost, and controls the preparation of the core first and then the shell, which can strictly control the particle size of the core-shell type ternary precursor and improve the electrochemical performance;
[0073] (3) The positive electrode material provided by the present invention has excellent performance and can better inhibit the corrosion of the electrolyte to the positive electrode material when used in the battery, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0074] Figure 1 This is an electron probe X-ray microscopic analysis diagram of the core-shell type ternary precursor provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0075] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0076] It should be understood that, in the description of the present invention, the terms "first", "second", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "plurality" means two or more.
[0077] Example 1
[0078] This embodiment provides a core-shell type ternary precursor, which includes a core and a shell covering the core; the core is represented by Ni x Co y Mn z (OH) 2-a (WO4) a, where x is 0.9, y is 0.06, z is 0.04, and a is 0.1; the shell contains aluminum. The shell is expressed as Ni b Co c Mn d Al e (OH) (2(b+c+d)+3e) , wherein b is 0.9, c is 0.06, d is 0.04 and e is 0.017. The aluminum content in the shell is 0.5wt%. The size of the core is 7μm. The shell thickness of the shell is 1μm. The D50 of the core-shell ternary precursor is 8.0μm.
[0079] This embodiment also provides a method for preparing the core-shell ternary precursor, the preparation method comprising the following steps:
[0080] Ternary salt solution: obtained by dissolving nickel sulfate, cobalt sulfate and manganese sulfate in water, wherein the concentration of the solute is 100 g / L.
[0081] Mixed salt solution containing aluminum salt: obtained by mixing aluminum sulfate with a ternary salt solution.
[0082] Precipitating agent: 31 wt% sodium hydroxide solution; complexing agent: 15 wt% ammonia water.
[0083] In a nitrogen atmosphere, 100 L of a base liquid (prepared with sodium hydroxide and ammonia water) with an initial pH of 11.4 and an ammonia concentration of 8 g / L was prepared, and then a ternary salt solution (Ni:Co:Mn molar ratio of 90:6:4, nitrate, solute concentration of 2500 mg / L) was introduced into the base liquid at 8 L / h, a tungstate ammonia solution with a tungsten concentration of 200 mg / L was introduced at 6 L / h, a precipitant was introduced at 2.4 L / h, and a complexing agent was introduced at 1 L / h, the introduction rate of the precipitant was adjusted to control the pH to between 11 and 11.2; the introduction rate of the complexing agent was adjusted to control the ammonia concentration to between 7 and 8 g / L, and the first reaction was carried out at 58°C, the reaction time was controlled to be 82 h, and a core with an average particle size of 7 μm was formed.
[0084] Stop introducing the ternary salt solution, and simultaneously introduce an aluminum-containing mixed salt solution (aluminum nitrate, nickel nitrate, manganese nitrate and manganese nitrate, Ni:Co:Mn molar ratio of 90:6:4) with an aluminum concentration of 450 mg / L at 8 L / h, and continue the second reaction at 58° C. until the particle size reaches 8 μm, forming a shell covering the outside of the core, and the shell thickness is 1 μm;
[0085] The reacted material after the shell is formed is filtered, the solid phase is washed and dried in sequence to obtain the core-shell type ternary precursor.
[0086] Test method: Malvern 3000 was used to test the particle size of the core-shell ternary precursor, and ICP was used to test the aluminum content of the outer shell in the core-shell ternary precursor.
[0087] The electron probe X-ray microscopic analysis of the core-shell ternary precursor prepared in Example 1 is shown in FIG. Figure 1 As shown, from Figure 1 It can be seen that the core-shell ternary precursor has a uniform particle size distribution, large particle size, and an obvious core and coating shell structure.
[0088] Example 2
[0089] This embodiment provides a core-shell type ternary precursor, which includes a core and a shell covering the core; the core is represented by Ni x Co y Mn z (OH) 2-a (WO4) a , where x is 0.8, y is 0.1, z is 0.1, and a is 0.5; the shell contains aluminum. The shell is expressed as Ni b Co c Mn d Al e (OH) (2(b+c+d)+3e) , wherein b is 0.8, c is 0.1, d is 0.1 and e is 0.034. The aluminum content in the shell is 1wt%. The size of the core is 5.5μm. The shell thickness of the shell is 1.5μm. The D50 of the core-shell ternary precursor is 8.0μm.
[0090] This embodiment also provides a method for preparing the core-shell ternary precursor, the preparation method comprising the following steps:
[0091] Ternary salt solution: obtained by dissolving nickel nitrate, cobalt nitrate and manganese nitrate in water, wherein the concentration of the solute is 100 g / L.
[0092] Mixed salt solution containing aluminum salt: obtained by mixing aluminum nitrate with a ternary salt solution.
[0093] Precipitating agent: 32 wt% sodium hydroxide solution; complexing agent: 10 wt% ammonia water.
[0094] In a nitrogen atmosphere, 120 L of a base liquid (prepared with sodium hydroxide and ammonia water) with an initial pH of 11.5 and an ammonia concentration of 9 g / L was prepared, and then a ternary salt solution (Ni:Co:Mn molar ratio of 80:10:10, nitrate, solute concentration of 3500 mg / L) was introduced into the base liquid at 6 L / h, an ammonia tungstate solution with a tungsten concentration of 250 mg / L was introduced at 8 L / h, a precipitant was introduced at 2 L / h, and a complexing agent was introduced at 0.8 L / h, the introduction rate of the precipitant was adjusted to control the pH between 11.5 and 12; the introduction rate of the complexing agent was adjusted to control the ammonia concentration between 8 and 9 g / L, and the first reaction was carried out at 60°C, the reaction time was controlled to be 63 h, and a core with an average particle size of 5.5 μm was formed.
[0095] Stop feeding the ternary salt solution, and simultaneously feed a mixed salt solution containing aluminum salts (aluminum nitrate, nickel nitrate, manganese nitrate and manganese nitrate, Ni:Co:Mn molar ratio of 80:10:10) with an aluminum concentration of 300 mg / L at 4 L / h, and continue the second reaction at 60° C. until the particle size reaches 7 μm, forming a shell covering the outside of the core, and the shell thickness is 1.5 μm;
[0096] The reacted material after the shell is formed is filtered, the solid phase is washed and dried in sequence to obtain the core-shell type ternary precursor.
[0097] Example 3
[0098] This embodiment provides a core-shell type ternary precursor, which includes a core and a shell covering the core; the core is represented by Ni x Co y Mn z (OH) 2-a (WO4) a , where x is 0.6, y is 0.1, z is 0.3, and a is 1; the shell contains aluminum. The shell is expressed as Ni b Co c Mn d Al e (OH) (2(b+c+d)+3e) , wherein b is 0.6, c is 0.1, d is 0.3 and e is 0.07. The content of aluminum in the shell is 2wt%. The size of the core is 6.0μm. The shell thickness of the shell is 2.0μm. The particle size range of the core-shell ternary precursor is 8.0μm.
[0099] This embodiment also provides a method for preparing the core-shell ternary precursor, the preparation method comprising the following steps:
[0100] Ternary salt solution: obtained by dissolving nickel sulfate, cobalt sulfate and manganese sulfate in water, wherein the concentration of the solute is 100 g / L.
[0101] Mixed salt solution containing aluminum salt: obtained by mixing aluminum sulfate with a ternary salt solution.
[0102] Precipitating agent: 25wt% sodium hydroxide solution; complexing agent: 12wt% ammonia water.
[0103] In a nitrogen atmosphere, 90 L of a base liquid (prepared with sodium hydroxide and ammonia water) with an initial pH of 10.0 and an ammonia concentration of 7 g / L was prepared, and then a ternary salt solution (Ni:Co:Mn molar ratio of 60:10:30, sulfate, solute concentration of 3800 mg / L) was introduced into the base liquid at 10 L / h, a tungstate ammonia solution with a tungsten concentration of 250 mg / L was introduced at 2 L / h, a precipitant was introduced at 3 L / h, and a complexing agent was introduced at 1.2 L / h, the introduction speed of the precipitant was adjusted to control the pH between 9 and 10; the introduction speed of the complexing agent was adjusted to control the ammonia concentration between 5 and 7 g / L, and the first reaction was carried out at 50°C, the reaction time was controlled to be 72 h, and a core with an average particle size of 6.0 μm was formed.
[0104] Stop feeding the ternary salt solution, and simultaneously feed a mixed salt solution containing aluminum salt (aluminum sulfate, nickel sulfate, manganese sulfate and manganese sulfate, Ni:Co:Mn molar ratio is 90:6:4) with an aluminum concentration of 280 mg / L at 10 L / h, and continue the second reaction at 50° C. until D50 reaches 8 μm, forming a shell covering the outside of the core, and the shell thickness is 2 μm;
[0105] The reacted material after the shell is formed is filtered, the solid phase is washed and dried in sequence to obtain the core-shell type ternary precursor.
[0106] Example 4
[0107] This embodiment provides a core-shell type ternary precursor. The core-shell type ternary precursor is the same as that in Embodiment 1 except that the ternary salt solution is introduced at 12 L / h during the preparation method, and will not be described in detail here.
[0108] Example 5
[0109] This embodiment provides a core-shell type ternary precursor. The core-shell type ternary precursor is the same as that in Embodiment 1 except that the ternary salt solution is introduced at 4 L / h in the preparation method, and will not be described again.
[0110] Example 6
[0111] This embodiment provides a core-shell type ternary precursor. The core-shell type ternary precursor is the same as Example 1 except that a tungstate solution with a tungsten content of 200 mg / L is introduced at 12 L / h in the preparation method, and the rest is not repeated here.
[0112] Example 7
[0113] This embodiment provides a core-shell type ternary precursor. The core-shell type ternary precursor is the same as Example 1 except that a tungstate solution with a tungsten content of 200 mg / L is introduced at 1 L / h in the preparation method, and the rest is not repeated here.
[0114] Example 8
[0115] This embodiment provides a core-shell type ternary precursor. The core-shell type ternary precursor is the same as Example 1 except that a mixed salt solution containing aluminum salt with an aluminum concentration of 450 mg / L is introduced at 12 L / h in the preparation method, and is not described again.
[0116] Example 9
[0117] This embodiment provides a core-shell type ternary precursor. The core-shell type ternary precursor is the same as Example 1 except that a mixed salt solution containing aluminum salt with an aluminum concentration of 450 mg / L is introduced at 1 L / h in the preparation method, and is not described again.
[0118] Example 10
[0119] This embodiment provides a core-shell type ternary precursor. Except for adjusting the introduction speed of the complexing agent and controlling the ammonia concentration to be between 11 and 12 g / L in the preparation method, the rest of the core-shell type ternary precursor is the same as Example 1 and will not be repeated here.
[0120] Embodiment 11
[0121] This embodiment provides a core-shell type ternary precursor. Except for adjusting the introduction speed of the complexing agent and controlling the ammonia concentration to be between 3 and 4 g / L in the preparation method, the rest of the core-shell type ternary precursor is the same as Example 1 and will not be repeated here.
[0122] Example 12
[0123] This embodiment provides a core-shell type ternary precursor. Except for adjusting the introduction speed of the precipitant and controlling the pH to be between 13 and 14 in the preparation method, the rest of the core-shell type ternary precursor is the same as that in Example 1, which will not be repeated here.
[0124] Comparative Example 1
[0125] This comparative example provides a core-shell type ternary precursor. The core-shell type ternary precursor is the same as Example 1 except that ammonium tungstate is replaced by ammonium molybdate in the preparation method, and the rest is not repeated here.
[0126] Comparative Example 2
[0127] This comparative example provides a core-shell type ternary precursor. The core-shell type ternary precursor is the same as Example 1 except that the aluminum salt is replaced by an iron salt in the preparation method, and the details are not repeated here.
[0128] Comparative Example 3
[0129] This comparative example provides a core-shell type ternary precursor. The core-shell type ternary precursor is the same as Example 1 except that the mixed salt solution containing aluminum salt is first introduced and then the tungstate solution is introduced in the preparation method, and the details will not be repeated here.
[0130] The core-shell ternary precursors of the above embodiments and comparative examples were mixed with lithium and calcined, graphite was used as the negative electrode, and an organic solution containing lithium salt was used as the electrolyte to assemble a battery, and the charge and discharge efficiency of the battery at 0.1C was tested, and the 100-week cycle retention rate of the battery was tested. The rate performance of the battery was also tested.
[0131] The test results of the above embodiments and comparative examples are shown in Table 1.
[0132] Table 1
[0133]
[0134]
[0135] From Table 1, we can see the following points:
[0136] (1) It can be seen from Examples 1 to 3 that the core-shell ternary precursor provided by the present invention has excellent rate performance. After being prepared into a positive electrode material and assembled into a battery, the rate performance is above 91.59%, the 0.1C charge and discharge efficiency is above 88.26%, and the discharge capacity retention rate after 100 cycles is above 93.25%, and the cycle stability is high;
[0137] (2) Combining Example 1 and Examples 4 to 5, it can be seen that in Example 1, 8 L / h of ternary salt solution is introduced. Compared with 12 L / h and 4 L / h respectively in Examples 4 to 5, the rate performance in Example 1 is 92.96%, the 0.1C charge and discharge efficiency is 90.12%, and the discharge capacity retention rate after 100 cycles is 93.25%, while the rate performance in Examples 4 to 5 is only 90.89% and 89.25%, respectively, and the discharge capacity retention rate after 100 cycles is only 91.63% and 90.32%, respectively. This shows that the present invention can better achieve the growth of the precursor by preferably adopting an appropriate speed to introduce the ternary salt solution, and the particle size is moderate, which can further improve the rate performance and cycle stability of the battery;
[0138] (3) Combining Example 1 and Examples 6 to 7, it can be seen that in Example 1, 6 L / h of ammonium tungstate solution is introduced. Compared with 12 L / h and 1 L / h respectively in Examples 6 to 7, the rate performance in Example 1 is 92.96%, the 0.1C charge and discharge efficiency is 90.12%, and the discharge capacity retention rate after 100 cycles is 93.25%. In Example 6, the tungsten element is not completely precipitated, and re-nucleation occurs, and small particles grow, resulting in increased process difficulty. In Example 7, the electrical performance of the positive electrode material is less improved. Specifically, The rate performance in Examples 6 to 7 is only 90.16% and 91.69%, respectively, and the discharge capacity retention after 100 cycles is only 90.32% and 91.22%, respectively. This shows that the present invention can better achieve the growth of the precursor by preferably adopting an appropriate speed to pass the tungstate solution, and the particle size is moderate, which can further improve the rate performance and cycle stability of the battery; it can also be seen from Examples 1 and Examples 8 to 9 that the present invention controls the introduction speed of the mixed salt solution containing aluminum salt within a specific range, which can better improve the performance of the precursor;
[0139] (4) It can be seen from Example 1 and Examples 10 to 12 that the present invention preferably controls the ammonia concentration and pH within a reasonable range during the precipitation process, which can better achieve the growth of the precursor, and the particle size of the final product is more moderate, further improving the rate performance, cycle stability and charge and discharge efficiency of the battery;
[0140] (5) It can be seen from Example 1 and Comparative Examples 1 to 3 that the ammonium molybdate used in Comparative Example 1 is not as effective in improving the electrical properties of the positive electrode material as the ammonium tungstate used in Example 1. Iron salt is used for precipitation in Comparative Example 2, but iron is very easy to oxidize, making it difficult to prepare a feasible core-shell ternary precursor. In Comparative Example 3, tungsten is doped in the outer layer and aluminum is doped in the inner layer. The rate performance, cycle stability and charge and discharge efficiency of the final battery are not as good as those in Example 1. This shows that the present invention combines the advantages of tungsten doping in the inner layer with aluminum doping in the outer layer, thereby significantly improving the performance of the precursor and having broad application prospects.
[0141] The present invention illustrates the detailed features of the present invention through the above embodiments, but the present invention is not limited to the above detailed features, that is, it does not mean that the present invention must rely on the above detailed features to be implemented. Those skilled in the art should understand that any improvement to the present invention, equivalent replacement of the technical features selected by the present invention, addition of auxiliary technical features, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A core-shell ternary precursor, characterized in that: The core-shell type ternary precursor includes a core and a shell coated outside the core; The expression of the core is Ni x Co y Mn z (OH) 2-a (WO4) a , where 0 < x < 1, 0 < y < 1, 0 < z < 1, and x + y + z = 1, and the value range of a is 0.01 to 1; The shell contains aluminum.
2. The core-shell ternary precursor according to claim 1, characterized in that: The preferred value range of a is 0.1 to 1; Preferably, the expression of the outer shell is Ni b Co c Mn d Al e (OH) (2(b+c+d)+3e) , where 0 < b < 1, 0 < c < 1, 0 < d < 1 and 0 < e < 1; Preferably, the aluminum content in the shell is 0.01 to 2 wt%.
3. The core-shell ternary precursor according to claim 1 or 2, characterized in that: The size of the core is 3 to 14 μm; Preferably, the shell thickness of the shell is 0.1 to 4 μm; Preferably, the particle size range of the core-shell type ternary precursor is 3.1 to 18 μm.
4. A method for preparing a core-shell ternary precursor according to any one of claims 1 to 3, characterized in that: The preparation method includes the following steps: Under a reaction atmosphere, a bottom liquid containing ammonia is prepared, and then a ternary salt solution, a tungstate solution, a precipitant, and a complexing agent are introduced into the bottom liquid to carry out a first reaction to form a core; The introduction of the ternary salt solution is stopped, and at the same time, a mixed salt solution containing an aluminum salt is introduced to carry out a second reaction to form a shell coated outside the core.
5. The preparation method according to claim 4, characterized in that: The reaction atmosphere includes nitrogen and / or air; Preferably, the precipitant includes an alkali solution, and the preferred precipitant is sodium hydroxide solution; Preferably, the concentration of the alkali solution is 20 to 40 wt%; Preferably, the complexing agent includes ammonia water and / or an ammonium salt solution; Preferably, the concentration of the ammonia water and / or the ammonium salt solution is 10 to 20 wt%; Preferably, the ammonia concentration of the bottom liquid is 6 to 10 g / L; Preferably, the pH of the bottom liquid is 9 to 12.
6. The preparation method according to claim 4 or 5, characterized in that: The ternary salt solution includes a nickel salt, a cobalt salt, and a manganese salt; Preferably, the nickel salt includes nickel nitrate and / or nickel sulfate; Preferably, the cobalt salt includes cobalt nitrate and / or cobalt sulfate; Preferably, the manganese salt includes manganese nitrate and / or manganese sulfate; Preferably, the molar ratio of Ni:Co:Mn in the ternary salt solution is x:y:z, where 0 < x < 1, 0 < y < 1, 0 < z < 1, and x + y + z = 1.
7. The preparation method according to any one of claims 4 to 6, characterized in that: The temperature of the first reaction is 50 to 60 °C; Preferably, the introduction rate of the ternary salt solution is 1 to 10 L / h.
8. The preparation method according to any one of claims 4 to 7, characterized in that: The tungsten concentration in the tungstate solution is 100 to 5000 mg / L; Preferably, the introduction rate of the tungstate solution is 0.1 to 5 L / h; Preferably, the introduction rate of the precipitant is 0.1 to 10 L / h; Preferably, the introduction rate of the complexing agent is 0.1 to 10 L / h; Preferably, the introduction rate of the precipitant is adjusted to control the pH to 9 to 12; Preferably, the introduction rate of the complexing agent is adjusted to control the ammonia concentration to 4 to 10 g / L; Preferably, the particle size of the core is 5 μm to 14 μm.
9. The preparation method according to any one of claims 4 to 8, characterized in that: The mixed salt solution containing an aluminum salt includes a ternary salt solution and an aluminum salt; Preferably, the aluminum salt includes aluminum sulfate and / or aluminum nitrate; Preferably, the aluminum concentration in the mixed salt solution containing an aluminum salt is 100 to 5000 mg / L; Preferably, the introduction rate of the mixed salt solution containing an aluminum salt is 1 to 10 L / h; Preferably, the temperature of the second reaction is 50 to 60 °C; Preferably, the preparation method further includes: sequentially performing solid-liquid separation, washing the solid phase, and drying the reaction product after forming the shell to obtain the core-shell type ternary precursor.
10. A positive electrode material, characterized in that: The positive electrode material includes a positive electrode active material prepared from the core-shell type ternary precursor according to any one of claims 1 to 3.