Preparation method of high-transparency nano photovoltaic glass
By using SiO2, Al2O3 and other materials in photovoltaic glass to prepare glass substrates and combining vapor deposition and ultrasonic atomization coating technology, a nanoscale alkali metal oxide combination film is formed, which solves the problem of low light transmittance of photovoltaic glass and improves light conversion. efficiency and film adhesion, achieving the preparation of highly transparent nanophotovoltaic glass.
Patent Information
- Application Number
- CN202411237338.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-09-05
AI Technical Summary
The light transmittance of existing photovoltaic glass is low, which affects the light conversion efficiency of solar cells, and the coating process has efficiency and cost issues.
The glass substrate is prepared using SiO2, Al2O3, CsOH, Na2O, K2O, MgO, CdO and other materials, and is melted, clarified and homogenized through a platinum-rhodium crucible, combined with vapor deposition and ultrasonic atomization coating technology, to form a nanoscale alkali metal oxide combination membrane, improving the tightness of the glass structure and ion exchange efficiency.
The light transmittance and light conversion efficiency of photovoltaic glass are significantly improved, the adhesion and stability of the film layer are enhanced, and the preparation of highly transparent nanophotovoltaic glass is achieved.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photovoltaic glass, and in particular to a method for preparing highly transparent nano photovoltaic glass. Background Art
[0002] Solar photovoltaic glass is a special glass that can generate electricity by using solar radiation through lamination of solar cells and has relevant current extraction devices and cables. It is composed of low-iron glass, solar cells, film, back glass, and special metal wires. The solar cells are sealed between a piece of low-iron glass and a piece of back glass through film. It is a new high-tech glass product for construction.
[0003] Since crystalline silicon solar panels cannot be exposed to the external environment for a long time, photovoltaic glass is currently one of the best packaging materials that protects crystalline silicon cells and has a high transmittance. Among the factors that determine the conversion efficiency of crystalline silicon solar cells, the most important factor is the crystalline silicon technology in the photovoltaic components, followed by the photovoltaic glass that protects the photovoltaic components. Relatively speaking, improving the optical properties of photovoltaic glass is easier than improving the conversion efficiency of crystalline silicon cells, and the cost is slightly lower. Therefore, the development and production of photovoltaic glass with higher transmittance is very urgent, both for component manufacturers and in the final terminal market, so as to achieve the effect of improving light conversion. The present invention provides a method for preparing highly transparent nano photovoltaic glass, starting from the process modification of coating to solve the above problems. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing highly transparent nano photovoltaic glass to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing highly transparent nano photovoltaic glass, comprising the following preparation steps: (1) SiO2, Al2O3, CsOH, Na2O, K2O, MgO, and CdO are prepared in a mass ratio of 30-32:6-8:0.2-0.4:6-8:0.5-1:1-4:1-2, mixed, melted, clarified, and homogenized in a silicon-molybdenum rod high-temperature electric furnace at 1640°C using a platinum-rhodium crucible as a melting container, with a melting cycle of more than 6 hours. After the glass liquid is clarified and homogenized, the glass liquid is poured into a 200×100×50 mm metal mold to form the glass. The demolded glass test piece is annealed in a muffle furnace to form a transparent glass substrate. (2) First, clean the surface of the substrate with clean water, then immerse the substrate in a concentrated sulfuric acid solution containing potassium dichromate for 2-4 hours, then put it in an ultrasonic cleaner and clean it with distilled water for 30 minutes, take it out and place it in a clean oven at 50°C for drying for 2 hours for use; the dried glass substrate is coated, and the vapor deposition coating and ultrasonic atomization coating are carried out simultaneously during the coating process. After the deposition is completed, annealing is performed at 400-480°C for 30 minutes, and cooling to room temperature can obtain transparent nano photovoltaic glass.
[0006] Furthermore, in step (1), the average particle size of MgO is 50 nm, and the average particle size of CdO is 10 nm.
[0007] Furthermore, the annealing process in step (1) is as follows: a heating rate of 20°C / min-30°C / min, a temperature of 690°C, and a time of 30 minutes, and after the annealing is completed, the annealing is cooled to room temperature in the furnace.
[0008] Furthermore, the method for vapor deposition coating in step (2) is: SiH4 diluted with nitrogen is mixed with ethylene in a volume ratio of 1:1 as a raw material gas, the substrate is fixed on a quartz tube during the coating process, and the raw material gas is sprayed from a nozzle moving at a uniform speed. The speed of the nozzle is the speed of the substrate on the actual production line. The deposition temperature is 580-660°C and the nozzle speed is 1-2.4 cm / s.
[0009] Furthermore, the volume concentration of SiH4 in the SiH4 diluted by nitrogen is 10%.
[0010] Furthermore, in step (2), the ultrasonic spray coating method is as follows: 20-28 parts of ethanol, 0.1-0.5 parts of inorganic acid catalyst, 2-4 parts of tetraethyl silicate, and 1-5 parts of octyltrimethoxysilane are mixed, stirred at 60 rpm for 30 minutes, and poured into an ultrasonic atomizer. The distance between the nozzle of the ultrasonic atomizer and the substrate is 6-12 mm. The nozzle is driven by a stepper motor at a speed of 0.5-2.5 m / s, and the atomization volume is 1800-2500 dm 3 h -1 and nitrogen pressure is 1.2×10 -5 -2.0×10 -5 After Pa, turn on the stepper motor and ultrasonic atomizer. The ultrasonic vibration of the piezoelectric ceramic transducer in the ultrasonic atomizer atomizes the prepared solution, which is carried to the nozzle of the ultrasonic atomizer by the carrier gas. Under the control of the stepper motor, the drug droplets are evenly sent to the heated glass substrate, and a chemical reaction occurs on the substrate at high temperature, so that a uniform silane film can be deposited on the substrate.
[0011] Furthermore, the frequency used by the ultrasonic cleaner in step (2) is 30-40 kHz.
[0012] Furthermore, the mass fraction of potassium dichromate in the concentrated sulfuric acid solution containing potassium dichromate in step (2) is 11.7%.
[0013] Furthermore, the inorganic acid catalyst is a 10% by mass hydrochloric acid aqueous solution.
[0014] Furthermore, the piezoelectric ceramic transducer chip is of a transmitting type, and its ultrasonic vibration frequency is 1.6 MHz.
[0015] Compared with the prior art, the beneficial effects achieved by the present invention are: The present invention is prepared by coating a silane film on the surface of a self-made transparent glass substrate to achieve the effects of high light conversion and high transparency.
[0016] Firstly, nano-scale alkali metal oxides CdO, MgO and Al2O3 are combined and added in appropriate amounts to a transparent glass substrate prepared with SiO2 as raw material, so that the glass structure tends to be more compact and is conducive to the realization of chemical ion exchange; Al2O3 is an intermediate oxide, which can form two structural units, AlO4 and AlO6, with AlO4 becoming a network former and AlO6 becoming a network exogenous body; when preparing the substrate, light magnesium oxide is sintered at high temperature to form a crystalline embedded network structure, making the glass structure space looser, the gap of the network structure larger, forming a larger ion exchange channel, improving the ion exchange efficiency and the depth of the ion exchange layer, and forming multiple rings to meet the integrity of the glass structure; the cadmium ions and oxygen ions in cadmium oxide are combined with each other through ionic bonds to form a cubic octahedral structure, which gives the glass structure a stable support force, thereby improving its performance; the glass substrate void structure and ion exchange efficiency further improve the substrate's light transmittance, thereby improving the light conversion efficiency of solar cells.
[0017] Secondly, ultrasonic atomization technology is used to make up for the shortcomings of the spray gun in the spray technology. The piezoelectric ceramic transducer chip is vibrated at a certain frequency. The vibration of the ultrasonic frequency produces cavitation on the surface of the water column, so that the solution is atomized into a large number of suspended particles. During the flight of the suspended droplet particles in the reactor, they are simultaneously affected by the drag force of the gas and gravity. The solute hits the substrate, and the temperature of the solute on the substrate rises and decomposes into a film. In coordination with the silane monomer deposited by the meteorological atmosphere, the silane forms a nano-particle mosaic structure with a crystalline structure at a specific temperature. The surface is covered with a thin film formed by the impact of ultrasonic particles. The mist particles have enough momentum to hit the surface of the substrate and flatten it, which is conducive to the formation of a dense and uniform film, and form a composite three-dimensional structure with the nanoparticles, which increases the light absorption rate of the light board and increases the transparency of the film; the nano-silane particles are rich in hydroxyl functional groups to ensure that the bottom film layer has good adhesion with the glass substrate and the bottom film layer and the surface film layer, and the film layer is not easy to fall off, thereby enhancing the dispersibility and stability. DETAILED DESCRIPTION
[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0019] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of a highly transparent nano photovoltaic glass prepared in the following examples are as follows: Light transmittance: The average light transmittance at 400-800 nm and the transmittance at 550 nm were measured using a Hitachi U-41000 spectrophotometer.
[0020] Photoconversion: The photovoltaic glass prepared in the examples and comparative examples was assembled with a crystalline silicon cell, and the electrical performance was tested according to the test standard of Photovoltaic Devices Part 10: Linear Characteristics Measurement Method GB / T 6495.10-2012 / IEC60904-10:1998.
[0021] Adhesion: The photovoltaic glass prepared in the embodiment and the comparative example was tested for adhesion of the coating according to GB / T9286-1998.
[0022] Example 1; (1) SiO2, Al2O3, CsOH, Na2O, K2O, MgO, and CdO are prepared in a mass ratio of 30:6:0.2:6:0.5:1:1 to prepare a batch material, wherein the average particle size of MgO is 50 nm, and the average particle size of CdO is 10 nm, and then mixed, and melted, clarified, and homogenized in a silicon-molybdenum rod high-temperature electric furnace at 1640°C using a platinum-rhodium crucible as a melting container, with a melting cycle of more than 6 hours. After the glass liquid is clarified and homogenized, the glass liquid is poured into a 200×100×50 mm metal mold to form a glass sample. After demolding, the glass sample is annealed in a muffle furnace at a heating rate of 20°C / min, a temperature of 690°C, and a time of 30 minutes. After the annealing is completed, the glass sample is cooled to room temperature in the furnace to form a transparent glass substrate; (2) First, clean the surface of the substrate with clean water, and then immerse the substrate in a concentrated sulfuric acid solution containing potassium dichromate for 2 hours, wherein the mass fraction of potassium dichromate in the concentrated sulfuric acid solution containing potassium dichromate is 11.7%; then, place the substrate in an ultrasonic cleaner and clean it with distilled water for 30 minutes at a frequency of 30 kHz, take it out and place it in a clean oven at 50°C for drying for 2 hours for use; coat the dried glass substrate, and during the coating process, vapor deposition coating and ultrasonic atomization coating are carried out simultaneously; the method for vapor deposition coating is: SiH4 diluted with nitrogen and ethylene are mixed in a volume ratio of 1:1 as the raw material gas, wherein the volume of SiH4 in the nitrogen-diluted SiH4 is 1:1. The deposition concentration is 10%. During the coating process, the substrate is fixed on the quartz tube, and the raw gas is sprayed from a nozzle moving at a uniform speed. The nozzle speed is the substrate speed of the actual production line. The deposition temperature is 580 ° C, and the nozzle speed is 1 cm / s. The ultrasonic spray coating method is as follows: 20 parts of ethanol, 0.1 parts of 10% hydrochloric acid aqueous solution, 2 parts of tetraethyl silicate, and 1 part of octyltrimethoxysilane are mixed, stirred at 60 rpm for 30 minutes, and poured into the ultrasonic atomizer. The distance between the nozzle of the ultrasonic atomizer and the substrate is 6 mm. The nozzle is driven by a stepper motor at a speed of 0.5 m / s, and the atomization volume is 1800 dm 3 h -1 and nitrogen pressure is 1.2×10 -5 After Pa, turn on the stepper motor and ultrasonic atomizer, the ultrasonic vibration of the piezoelectric ceramic transducer in the ultrasonic atomizer atomizes the prepared solution, the piezoelectric ceramic transducer chip is an emission type, and its ultrasonic vibration frequency is 1.6MHz, which is carried to the nozzle of the ultrasonic atomizer by the carrier gas. Under the control of the stepper motor, the drug droplets are evenly sent to the heated glass substrate, and a chemical reaction occurs on the substrate at high temperature, so that a uniform silane film can be deposited on the substrate; after the deposition is completed, annealing is carried out at 400°C for 30 minutes, and transparent nano photovoltaic glass can be obtained by cooling to room temperature.
[0023] Example 2; (1) SiO2, Al2O3, CsOH, Na2O, K2O, MgO, and CdO are prepared in a mass ratio of 31:7:0.3:7:0.75:2.5:1.5 to prepare a batch material, wherein the average particle size of MgO is 50 nm, and the average particle size of CdO is 10 nm, and then mixed, and a platinum-rhodium crucible is used as a melting container, and the mixture is melted, clarified, and homogenized in a silicon-molybdenum rod high-temperature electric furnace at 1640°C. The melting cycle is greater than 6 hours. After the glass liquid is clarified and homogenized, the glass liquid is poured into a 200×100×50 mm metal mold to form. The demolded glass test piece is annealed in a muffle furnace at a heating rate of 25°C / min, a temperature of 690°C, and a time of 30 minutes. After the annealing is completed, the glass is cooled to room temperature in the furnace to form a transparent glass substrate; (2) First, clean the surface of the substrate with clean water, and then immerse the substrate in a concentrated sulfuric acid solution containing potassium dichromate for 3 hours, wherein the mass fraction of potassium dichromate in the concentrated sulfuric acid solution containing potassium dichromate is 11.7%; then, place the substrate in an ultrasonic cleaner and clean it with distilled water for 30 minutes at a frequency of 35 kHz, take it out and place it in a clean oven at 50°C for drying for 2 hours for use; coat the dried glass substrate, and during the coating process, vapor deposition coating and ultrasonic atomization coating are carried out simultaneously; the method for vapor deposition coating is: SiH4 diluted with nitrogen and ethylene are mixed in a volume ratio of 1:1 as the raw material gas, wherein the volume of SiH4 in the SiH4 diluted with nitrogen is The concentration is 10%. During the coating process, the substrate is fixed on the quartz tube, and the raw gas is sprayed from a nozzle moving at a uniform speed. The speed of the nozzle is the speed of the substrate on the actual production line. The deposition temperature is 620°C, and the nozzle speed is 1.7 cm / s. The ultrasonic spray coating method is as follows: 24 parts of ethanol, 0.3 parts of 10% hydrochloric acid aqueous solution, 3 parts of tetraethyl silicate, and 3 parts of octyltrimethoxysilane are mixed, stirred at 60 rpm for 30 minutes, and poured into the ultrasonic atomizer. The distance between the nozzle of the ultrasonic atomizer and the substrate is 9 mm. The nozzle is driven by a stepper motor at a speed of 1.5 m / s, and the atomization volume is 2150 dm 3 h -1 and nitrogen pressure is 1.6×10 -5 After Pa, turn on the stepper motor and ultrasonic atomizer, the ultrasonic vibration of the piezoelectric ceramic transducer in the ultrasonic atomizer atomizes the prepared solution, the piezoelectric ceramic transducer chip is an emission type, and its ultrasonic vibration frequency is 1.6MHz, which is carried to the nozzle of the ultrasonic atomizer by the carrier gas. Under the control of the stepper motor, the drug droplets are evenly sent to the heated glass substrate, and a chemical reaction occurs on the substrate at high temperature, so that a uniform silane film can be deposited on the substrate; after the deposition is completed, annealing is carried out at 440℃ for 30min, and transparent nano photovoltaic glass can be obtained by cooling to room temperature.
[0024] Example 3; (1) SiO2, Al2O3, CsOH, Na2O, K2O, MgO, and CdO are prepared in a mass ratio of 32:8:0.4:8:1:4:2, wherein the average particle size of MgO is 50 nm, and the average particle size of CdO is 10 nm. The mixture is then mixed and melted, clarified, and homogenized in a silicon-molybdenum rod high-temperature electric furnace at 1640°C using a platinum-rhodium crucible as a melting container. The melting cycle is greater than 6 hours. After the glass liquid is clarified and homogenized, the glass liquid is poured into a 200×100×50 mm metal mold to form a glass sample. The demoulding glass sample is annealed in a muffle furnace at a heating rate of 30°C / min, a temperature of 690°C, and a time of 30 minutes. After the annealing is completed, the glass sample is cooled to room temperature in the furnace to form a transparent glass substrate. (2) First, clean the surface of the substrate with clean water, and then immerse the substrate in a concentrated sulfuric acid solution containing potassium dichromate for 4 hours, wherein the mass fraction of potassium dichromate in the concentrated sulfuric acid solution containing potassium dichromate is 11.7%; then, place the substrate in an ultrasonic cleaner and clean it with distilled water for 30 minutes at a frequency of 40 kHz, take it out and place it in a clean oven at 50°C for drying for 2 hours for use; coat the dried glass substrate, and during the coating process, vapor deposition coating and ultrasonic atomization coating are carried out simultaneously; the method for vapor deposition coating is: SiH4 diluted with nitrogen and ethylene are mixed in a volume ratio of 1:1 as the raw material gas, wherein the volume of SiH4 in the SiH4 diluted with nitrogen is The concentration is 10%. During the coating process, the substrate is fixed on the quartz tube, and the raw gas is sprayed from a nozzle moving at a uniform speed. The speed of the nozzle is the speed of the substrate on the actual production line. The deposition temperature is 660°C, and the nozzle speed is 2.4 cm / s. The ultrasonic spray coating method is as follows: 28 parts of ethanol, 0.5 parts of 10% hydrochloric acid aqueous solution, 4 parts of tetraethyl silicate, and 5 parts of octyltrimethoxysilane are mixed, stirred at 60 rpm for 30 minutes, and poured into the ultrasonic atomizer. The distance between the nozzle of the ultrasonic atomizer and the substrate is 12 mm. The nozzle is driven by a stepper motor at a speed of 2.5 m / s, and the atomization volume is 2500 dm 3 h -1 and nitrogen pressure is 2.0×10 -5 After Pa, turn on the stepper motor and ultrasonic atomizer. The ultrasonic vibration of the piezoelectric ceramic transducer in the ultrasonic atomizer atomizes the prepared solution. The piezoelectric ceramic transducer chip is an emission type, and its ultrasonic vibration frequency is 1.6MHz. It is carried to the nozzle of the ultrasonic atomizer by the carrier gas. Under the control of the stepper motor, the drug droplets are evenly sent to the heated glass substrate, and a chemical reaction occurs on the substrate at high temperature, so that a uniform silane film can be deposited on the substrate. After the deposition is completed, annealing is carried out at 480°C for 30 minutes, and transparent nano photovoltaic glass can be obtained by cooling to room temperature.
[0025] Comparative Example 1: The difference between Comparative Example 1 and Example 2 is that step (1) is different. Step (1) is changed to: SiO2, Al2O3, CsOH, Na2O, K2O, and CdO are prepared in a mass ratio of 31:7:0.3:7:0.75:1.5 to obtain a batch material, wherein the average particle size of MgO is 50 nm and the average particle size of CdO is 10 nm, and then mixed. A platinum-rhodium crucible is used as a melting container, and the mixture is melted, clarified and homogenized in a silicon-molybdenum rod high-temperature electric furnace at 1640°C. The melting cycle is greater than 6 hours. After the glass liquid is clarified and homogenized, the glass liquid is poured into a 200×100×50 mm metal mold to form the glass. The demolded glass test block is annealed in a muffle furnace at a heating rate of 25°C / min, a temperature of 690°C, and a time of 30 minutes. After the annealing is completed, the glass substrate is cooled to room temperature in the furnace to form a transparent glass substrate. The remaining steps are the same as those in Example 2.
[0026] Comparative Example 2: The difference between Comparative Example 2 and Example 2 is that step (1) is different. Step (1) is changed to: SiO2, Al2O3, CsOH, Na2O, K2O, and MgO are prepared in a mass ratio of 31:7:0.3:7:0.75:2.5 to obtain a batch material, wherein the average particle size of MgO is 50 nm and the average particle size of CdO is 10 nm, and then mixed. A platinum-rhodium crucible is used as a melting container, and the mixture is melted, clarified and homogenized in a silicon-molybdenum rod high-temperature electric furnace at 1640°C. The melting cycle is greater than 6 hours. After the glass liquid is clarified and homogenized, the glass liquid is poured into a 200×100×50 mm metal mold to form the glass. The demolded glass test block is annealed in a muffle furnace at a heating rate of 25°C / min, a temperature of 690°C, and a time of 30 minutes. After the annealing is completed, the glass substrate is cooled to room temperature in the furnace to form a transparent glass substrate. The remaining steps are the same as those in Example 2.
[0027] Comparative Example 3: The difference between Comparative Example 3 and Example 2 is that step (2) is different. Step (2) is changed to: first clean the surface of the substrate with clean water, then immerse the substrate in a concentrated sulfuric acid solution containing potassium dichromate for 3 hours, wherein the mass fraction of potassium dichromate in the concentrated sulfuric acid solution containing potassium dichromate is 11.7%; then put the substrate into an ultrasonic cleaner and clean it with distilled water for 30 minutes at a frequency of 35kHz, take it out and place it in a clean oven at 50°C for drying for 2 hours for use; the dried glass substrate is subjected to vapor deposition coating: SiH4 diluted with nitrogen and ethylene are mixed in a volume ratio of 1:1 as raw material gas, wherein the volume concentration of SiH4 in the SiH4 diluted with nitrogen is 10%; during the coating process, the substrate is fixed on a quartz tube, and the raw material gas is sprayed from a nozzle moving at a uniform speed, the nozzle speed is the substrate speed of the actual production line, the deposition temperature is 620°C, and the nozzle speed is 1.7 cm / s; the remaining steps are the same as in Example 2.
[0028] Comparative Example 4: The difference between Comparative Example 4 and Example 2 is that step (2) is different. Step (2) is changed to: first clean the surface of the substrate with clean water, and then immerse the substrate in a concentrated sulfuric acid solution containing potassium dichromate for 3 hours, wherein the mass fraction of potassium dichromate in the concentrated sulfuric acid solution containing potassium dichromate is 11.7%; then put it into an ultrasonic cleaner and clean it with distilled water for 30 minutes at a frequency of 35kHz, take it out and place it in a clean oven at 50°C for drying for 2 hours; ultrasonic spray coating is performed on the dried glass substrate; 24 parts of ethanol, 0.3 parts of 10% hydrochloric acid aqueous solution, 3 parts of tetraethyl silicate, and 3 parts of octyltrimethoxysilane are mixed, stirred at 60rpm for 30 minutes, and poured into an ultrasonic atomizer. The distance between the nozzle of the ultrasonic atomizer and the substrate is 9mm. The nozzle is driven by a stepper motor at a speed of 1.5m / s, and the atomization amount is 2150dm 3 h-1 and nitrogen pressure is 1.6×10 -5 After Pa, the stepper motor and the ultrasonic atomizer are turned on. The ultrasonic vibration of the piezoelectric ceramic transducer in the ultrasonic atomizer atomizes the prepared solution. The piezoelectric ceramic transducer chip is an emission type, and its ultrasonic vibration frequency is 1.6MHz. It is carried to the nozzle of the ultrasonic atomizer by the carrier gas. Under the control of the stepper motor, the drug droplets are uniformly sent to the heated glass substrate, and a chemical reaction occurs on the substrate at high temperature, so that a uniform silane film can be deposited on the substrate. After the deposition is completed, annealing is performed at 440°C for 30 minutes, and transparent nano photovoltaic glass can be obtained by cooling to room temperature. The remaining steps are the same as those in Example 2.
[0029] Effect example Table 1 below shows the performance analysis results of a highly transparent nano photovoltaic glass using Examples 1 to 3 of the present invention and Comparative Examples 1 to 4.
[0030] From the comparison of the experimental data of light transmittance and light conversion of the embodiment and the comparative example, it can be found that the present invention combines nano-scale alkali metal oxides CdO, MgO and Al2O3, and adds them in appropriate amounts to a transparent glass substrate prepared with SiO2 as a raw material, the glass structure tends to be more compact and is conducive to the realization of chemical ion exchange; Al2O3 is an intermediate oxide, which can form two structural units, AlO4 and AlO6, AlO4 becomes a network former, and AlO6 becomes a network exosome; light magnesium oxide is sintered at high temperature to form a crystalline embedded network structure when preparing the substrate, so that the glass structure space is looser, the gap of the network structure is larger, a larger ion exchange channel is formed, the ion exchange efficiency and the depth of the ion exchange layer are improved, and multiple rings are formed to meet the integrity of the glass structure; cadmium ions and oxygen ions in cadmium oxide are combined with each other through ionic bonds to form a cubic octahedral structure, which gives the glass structure a stable supporting force, thereby improving its performance; the glass substrate gap structure and ion exchange efficiency further improve the light transmittance of the substrate, thereby improving the light conversion efficiency of the solar cell. In addition, the present invention utilizes ultrasonic atomization technology to make up for the deficiency of spray gun in spray technology, vibrates the piezoelectric ceramic transducer chip at a certain frequency, and the vibration of ultrasonic frequency produces cavitation on the surface of water column, so that the solution is atomized into a large number of suspended particles. The suspended droplet particles are simultaneously subjected to the drag force and gravity of gas during the flight process in the reactor, and the solute hits the substrate. The temperature of the solute on the substrate rises and decomposes into a film, and cooperates with the silane monomer of meteorological deposition. At a specific temperature, the silane forms a nanoparticle mosaic structure with a crystalline structure, and the surface is covered with a film formed by the impact of ultrasonic particles. The mist particles have enough momentum to hit the surface of the substrate and flatten, which is conducive to forming a dense and uniform film, and form a composite three-dimensional structure with the nanoparticles, while improving the light absorption rate of the light board to the light, so that the transparency of the film is increased. From the experimental data comparison of the film adhesion of the embodiment and the comparative example, it can be found that the nanosilane particles of the present invention are rich in hydroxyl functional groups to ensure that the bottom film layer and the glass substrate, the bottom film layer and the surface film layer have good adhesion, the film layer is not easy to fall off, and the dispersibility and stability are enhanced.
[0031] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing highly transparent nano photovoltaic glass, characterized in that: The method comprises the following preparation steps: (1) SiO2, Al2O3, CsOH, Na2O, K2O, MgO, and CdO are prepared in a mass ratio of 30-32:6-8:0.2-0.4:6-8:0.5-1:1-4:1-2, mixed, melted, clarified, and homogenized in a silicon-molybdenum rod high-temperature electric furnace at 1640°C using a platinum-rhodium crucible as a melting container, with a melting cycle of more than 6 hours. After the glass liquid is clarified and homogenized, the glass liquid is poured into a 200×100×50 mm metal mold to form the glass. The demolded glass test piece is annealed in a muffle furnace to form a transparent glass substrate. (2) First, clean the surface of the substrate with clean water, then immerse the substrate in a concentrated sulfuric acid solution containing potassium dichromate for 2-4 hours, then put it in an ultrasonic cleaner and clean it with distilled water for 30 minutes, take it out and place it in a clean oven at 50°C for drying for 2 hours for use; the dried glass substrate is coated, and the vapor deposition coating and ultrasonic atomization coating are carried out simultaneously during the coating process. After the deposition is completed, annealing is performed at 400-480°C for 30 minutes, and cooling to room temperature can obtain transparent nano photovoltaic glass.
2. The method for preparing a highly transparent nano photovoltaic glass according to claim 1, characterized in that: In the step (1), the average particle size of MgO is 50 nm, and the average particle size of CdO is 10 nm.
3. The method for preparing a highly transparent nano photovoltaic glass according to claim 1, characterized in that: The annealing process in step (1) is as follows: heating rate is 20°C / min-30°C / min, temperature is 690°C, time is 30min, and after annealing, the furnace is cooled to room temperature.
4. The method for preparing a highly transparent nano photovoltaic glass according to claim 1, characterized in that: The method for vapor deposition coating in step (2) is: using SiH4 diluted with nitrogen and mixed with ethylene in a volume ratio of 1:1 as raw material gas, fixing the substrate on a quartz tube during the coating process, and spraying the raw material gas from a nozzle moving at a uniform speed, the nozzle speed being the substrate speed of the actual production line, the deposition temperature being 580-660°C, and the nozzle speed being 1-2.4 cm / s.
5. The method for preparing a highly transparent nano photovoltaic glass according to claim 4, characterized in that: The volume concentration of SiH4 in the SiH4 diluted with nitrogen is 10%.
6. The method for preparing a highly transparent nano photovoltaic glass according to claim 1, characterized in that: The ultrasonic spray coating method in step (2) is as follows: 20-28 parts of ethanol, 0.1-0.5 parts of inorganic acid catalyst, 2-4 parts of tetraethyl silicate, and 1-5 parts of octyltrimethoxysilane are mixed, stirred at 60 rpm for 30 minutes, and poured into an ultrasonic atomizer. The distance between the nozzle of the ultrasonic atomizer and the substrate is 6-12 mm. The nozzle is driven by a stepper motor at a speed of 0.5-2.5 m / s, and the atomization volume is 1800-2500 dm 3 h -1 and nitrogen pressure is 1.2×10 -5 -2.0×10 -5 After Pa, turn on the stepper motor and ultrasonic atomizer. The ultrasonic vibration of the piezoelectric ceramic transducer in the ultrasonic atomizer atomizes the prepared solution, which is carried to the nozzle of the ultrasonic atomizer by the carrier gas. Under the control of the stepper motor, the drug droplets are evenly sent to the heated glass substrate, and a chemical reaction occurs on the substrate at high temperature, so that a uniform silane film can be deposited on the substrate.
7. The method for preparing a highly transparent nano photovoltaic glass according to claim 1, characterized in that: The frequency used by the ultrasonic cleaner in step (2) is 30-40 kHz.
8. The method for preparing highly transparent nano photovoltaic glass according to claim 1, characterized in that: The mass fraction of potassium dichromate in the concentrated sulfuric acid solution containing potassium dichromate in step (2) is 11.7%.
9. The method for preparing highly transparent nano photovoltaic glass according to claim 5, characterized in that: The inorganic acid catalyst is a hydrochloric acid aqueous solution with a mass fraction of 10%.
10. The method for preparing highly transparent nano photovoltaic glass according to claim 5, characterized in that: The piezoelectric ceramic transducer chip is of emission type, and its ultrasonic vibration frequency is 1.6 MHz.
Citation Information
Patent Citations
High-performance nanometer conducting glass manufactured by adopting chemical vapor deposition method combined with thermal spraying method
CN102515568A
Method for preparing separation membrane by utilizing ultrasonic atomization and deposition method
CN108854571A
Conductive glass for thin-film solar cell and preparation method and application thereof
CN118420226A
Process of mfg. electrothermal SnO2:F film heating pipe by ultrasonic spray
CN1402594A