Surface layer protection glaze for 3D (three-dimensional) printed rock plate and preparation method of surface layer protection glaze
By using a glaze dispersant containing methacryloyloxyethyl phosphate and γ-methacryloyloxypropyltrimethoxysilane on the surface of 3D printed rock slabs to form chemical bonds at high temperatures, problems in the existing technology are solved. The problem of insufficient adhesion and color-fixing properties has significantly improved the thermal stability and aesthetics of the rock slabs.
Patent Information
- Application Number
- CN202411092290.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-08-09
AI Technical Summary
Existing 3D printed rock plate surface protection glazes have insufficient adhesion and poor color fixing performance at high temperatures, resulting in reduced service life and aesthetics. Moreover, the direct addition of high-temperature binders and interface modifiers has limited effects and is susceptible to process control. Influence.
Using a formula containing basic glaze, nano-alumina, organic solvent, defoaming agent, leveling agent, polyurethane and glaze dispersant, it is made by copolymerizing methacryloyloxyethyl phosphate and acrylic compounds at high temperatures. γ-Methacryloyloxypropyltrimethoxysilane forms chemical bonds to enhance the glaze's adhesion and color-fixing properties.
Significantly improves the thermal stability, mechanical stability and antioxidant properties of the glaze, ensuring color stability and adhesion, extending service life and improving overall performance.
Abstract
Description
Technical Field
[0001] The present invention relates to the field of ceramic glazes, and in particular to a surface protective glaze for 3D printed rock slabs and a preparation method thereof. Background Art
[0002] With the development and increasing demand for building decoration materials, 3D printed rock slabs, as a high-performance, environmentally friendly and beautiful building decoration material, have received widespread attention and application. 3D printed rock slabs have excellent properties such as high hardness, high wear resistance, high temperature resistance and corrosion resistance, and are widely used in indoor and outdoor decoration, furniture countertops, floor paving and other fields. However, in actual applications, the surface of 3D printed rock slabs is easily affected by wear, pollution and the environment, resulting in a decrease in service life and aesthetics. Therefore, it is particularly important to effectively protect the surface of the rock slab.
[0003] The traditional way to protect 3D printed rock panels mainly relies on coating with protective glaze. Protective glaze can not only give the surface of 3D printed rock panels gloss and beauty, but also effectively improve the wear resistance, stain resistance and weather resistance of rock panels. However, existing protective glazes have some technical defects, such as insufficient adhesion, poor color fixation performance, and low high temperature stability. These problems limit the performance and application effect of rock panel protective glazes.
[0004] The main components of traditional glazes include base glazes, organic solvents, defoamers, leveling agents, etc. These components can improve the performance of glazes to a certain extent, but during high-temperature firing, the adhesion between the glaze and the substrate is often insufficient, and it is easy to fall off and crack, resulting in poor protection. In addition, the color fixing performance of traditional glazes at high temperatures is also poor, and color particles are easy to lose and diffuse, affecting the aesthetics of the rock slab.
[0005] In order to improve the adhesion and color fixation of glazes, researchers have introduced some new materials and processes. For example, by adding nanomaterials (such as nano-alumina, nano-titanium dioxide), the hardness and wear resistance of glazes can be significantly improved, and their dispersibility and stability can be enhanced. However, although these improvement measures have improved the performance of glazes to a certain extent, they are still not enough to solve the problem of insufficient adhesion between glazes and substrates at high temperatures.
[0006] In recent years, with the continuous progress of chemistry and materials science, some chemical substances with special functions have been introduced into the formula of glazes in order to further improve their performance. For example, the introduction of high-temperature binders and interface modifiers can react chemically with the surface of the substrate during high-temperature firing to form strong chemical bonds, significantly enhancing the adhesion and color fixation performance of the glaze.
[0007] High-temperature binders such as methacryloxyethyl phosphate (MPEP) and interfacial modifiers such as γ-methacryloxypropyltrimethoxysilane (MPTA) are two chemical substances with bifunctional groups. MPEP and MPTA can not only copolymerize with acrylic monomers to form high molecular polymers to improve the mechanical strength and durability of the glaze, but also react chemically with the surface of the substrate at high temperatures to form a strong chemical bond and enhance the bonding force between the glaze and the substrate. In addition, the introduction of these substances can also improve the antioxidant properties and thermal stability of the glaze, further improving the overall performance of the glaze.
[0008] However, although directly adding high-temperature binders and interface modifiers can improve adhesion to a certain extent, the effect is limited and is easily affected by process control. In addition, directly adding high-temperature binders and interface modifiers can easily lead to uneven dispersion, affecting the mechanical properties of the rock slab. MPEP and MPTA may also decompose or migrate at high temperatures, thereby affecting the stability of the glaze. Summary of the invention
[0009] In view of the deficiencies in the prior art, the present invention provides a surface protective glaze for 3D printed rock slabs and a preparation method thereof.
[0010] The present invention provides a surface protective glaze for 3D printing rock plate, which comprises the following raw materials in parts by mass:
[0011] Basic glaze: 35-55 parts;
[0012] Nano-alumina: 2-5 parts;
[0013] Organic solvent: 45-55 parts;
[0014] Defoaming agent: 0.04-0.8 parts;
[0015] Leveling agent: 0.04-0.08 parts;
[0016] Polyurethane: 2-5 parts;
[0017] Glaze dispersant: 4-8 parts.
[0018] The basic glaze is a common basic glaze formula in the art, including transparent glaze and opaque glaze.
[0019] Preferably, the organic solvent is at least one of dimethyl sulfoxide, dimethylformamide, dimethylacetamide, ethyl acetate, acetone, and methyl ethyl ketone; more preferably, the organic solvent is dimethyl sulfoxide.
[0020] Preferably, the defoamer is BYK-052 defoamer, Airex902W defoamer, At least one of 111 defoamer, BYK-065 defoamer, and DeeFo2150 defoamer.
[0021] Preferably, the leveling agent is BYK-306 leveling agent, Glide450 leveling agent, EFKA-3770 leveling agent, BYK-358N leveling agent, At least one of Flow375 leveling agents.
[0022] Preferably, the polyurethane is 5703 polyurethane, 9370A polyurethane, HT-2000 polyurethane, 985A polyurethane, 2363-80AE polyurethane, 1180A polyurethane; preferably, the polyurethane is 9370A Polyurethane.
[0023] The preparation method of the glaze dispersant comprises the following steps:
[0024] (1) adding an acrylic acid compound and an acrylic acid ester compound to dimethyl sulfoxide;
[0025] (2) adding vinyl triethoxysilane and N-vinyl pyrrolidone;
[0026] (3) adding azobisisobutyronitrile and an adhesion enhancer, stirring, and obtaining the glaze dispersant.
[0027] Preferably, the preparation method of the glaze dispersant comprises the following steps:
[0028] (1) adding 50-60 g of an acrylic acid compound and 20-30 g of an acrylic acid ester compound to 30-50 g of dimethyl sulfoxide at 70-80° C. and nitrogen atmosphere, and stirring at 150-200 r / min to obtain an acrylic acid prepolymer solution;
[0029] (2) maintaining stirring at 150-200 r / min, adding 5-15 g of vinyl triethoxysilane as a crosslinking agent to the acrylic polymer solution obtained in step (1) at a rate of 3-5 g / min to enhance the network structure and durability of the material, and then adding 1-3 g of N-vinyl pyrrolidone, stirring at 100-300 r / min for 5-15 min, and controlling the molecular weight and molecular weight distribution of the polymer by capturing the polymerization active center to obtain a cross-linked acrylic polymer solution;
[0030] (3) adding 1-3 g of azobisisobutyronitrile as an initiator for free radical polymerization to the cross-linked acrylic polymer solution obtained in step (2), adding 6-12 g of an adhesion enhancer under stirring at 150-200 r / min, and restarting the polymerization reaction. These substances have bifunctional groups and can copolymerize with acrylic compounds to form a polymer, and react with the surface of the substrate at high temperature to enhance the bonding force; stirring at 70-80° C. and 100-300 r / min for 60-180 min to ensure that the polymerization reaction is fully carried out to form the desired high molecular polymer, and cooling to room temperature to obtain the glaze dispersant.
[0031] Preferably, the acrylic compound is at least one of acrylic acid and methacrylic acid.
[0032] Preferably, the acrylic acid ester compound is at least one of methyl methacrylate and butyl acrylate.
[0033] Preferably, the adhesion enhancer is at least one of methacryloxyethyl phosphate and γ-methacryloxypropyltrimethoxysilane; preferably, the adhesion enhancer is a mixture of methacryloxyethyl phosphate and γ-methacryloxypropyltrimethoxysilane in a mass ratio of (5-10): (1-2).
[0034] The present invention also provides a method for preparing a surface protective glaze for a 3D printed rock plate, comprising the following steps: adding 35-55 parts of a basic glaze, 2-5 parts of nano-alumina, 45-55 parts of an organic solvent, 0.04-0.8 parts of a defoaming agent, 0.04-0.08 parts of a leveling agent, 2-5 parts of a polyurethane, and 4-8 parts of a glaze dispersant, by mass, into a sand mill and grinding them evenly to obtain the surface protective glaze for a 3D printed rock plate.
[0035] Preferably, zirconia balls with a diameter of 0.5-1.5 mm are used as grinding media, the sanding time is 3-6 hours, and the grinding speed is 500-1500 r / min.
[0036] The organic glaze prepared by the present invention can effectively prevent water penetration and protect the substrate, and can better penetrate into the surface of the substrate and improve adhesion compared with the traditional water-soluble glaze.
[0037] In addition, traditional glazes have weak bonding with the substrate at high temperatures, which makes the glaze prone to falling off and color loss during high-temperature firing. Although directly adding methacryloyloxyethyl phosphate and γ-methacryloyloxypropyltrimethoxysilane can improve adhesion to a certain extent, the effect is limited and is easily affected by process control. It may decompose or migrate at high temperatures, affecting the stability of the glaze. Uneven dispersion of additives may also lead to inconsistent mechanical properties.
[0038] In order to improve this defect, the present invention introduces methacryloxyethyl phosphate and γ-methacryloxypropyltrimethoxysilane, and copolymerizes with acrylic compounds. Methacryloxyethyl phosphate and γ-methacryloxypropyltrimethoxysilane form chemical bonds with the substrate at high temperature. Such chemical bonds improve the thermal stability of the glaze, making it more stable during high-temperature sintering and not easy to decompose or deteriorate. The polymer chains formed by copolymerization form stronger chemical bonds with the surface of the substrate, significantly improving the adhesion and bonding force, giving the glaze higher mechanical strength and wear resistance, thereby improving the overall stability of the glaze.
[0039] Since methacryloyloxyethyl phosphate and γ-methacryloyloxypropyltrimethoxysilane can form strong chemical bonds with the surface of the substrate at high temperatures, this chemical bond not only enhances the adhesion of the glaze, but also effectively locks the color particles to prevent color loss and diffusion during high-temperature firing.
[0040] However, the unimproved glaze lacks the chemical bonding effect at high temperature and the protection of nanomaterials. During the high-temperature firing process, the color particles are easily lost and diffused, resulting in poor color fixing performance.
[0041] Beneficial effects of the present invention:
[0042] By introducing methacryloxyethyl phosphate and γ-methacryloxypropyltrimethoxysilane and copolymerizing with acrylic compounds, the improved glaze has significantly improved thermal stability, mechanical stability, antioxidant and color fixation properties. These improvements enable the glaze to better maintain color stability and adhesion during high-temperature firing, thereby improving overall performance and service life. Through experimental verification, the effects of these improvements can be further confirmed to ensure their reliability and superiority in practical applications. Although this method is complex in process, the performance improvement and long-term stability it brings give it greater advantages and prospects in the application of high-performance 3D printed rock slab protective glazes. DETAILED DESCRIPTION
[0043] Nano-alumina, model: TAP-A26, Nanjing Tianxing New Materials Co., Ltd.
[0044] Methacryloyloxyethyl phosphate, CAS number: 32435-46-4.
[0045] γ-Methacryloyloxypropyltrimethoxysilane, CAS number: 2530-85-0.
[0046] N-vinylpyrrolidone, CAS number: 88-12-0.
[0047] The basic glaze used in the following examples and comparative examples is composed of the following raw materials in weight percentage: potassium feldspar: 30%, quartz: 20%, zinc borate: 10%, titanium oxide: 10%, barium carbonate: 15%, and kaolin: 15%.
[0048] A method for preparing a surface protective glaze for a 3D printed rock plate comprises the following steps: by weight, 50 parts of a basic glaze, 3 parts of nano-alumina, 50 parts of an organic solvent, 0.2 parts of a defoamer, 0.06 parts of a leveling agent, 3 parts of a polyurethane, and 6 parts of a glaze dispersant are added into a sand mill and ground evenly to obtain the surface protective glaze for the 3D printed rock plate.
[0049] Zirconia balls with a diameter of 1 mm were used as grinding media, the sanding time was 4 h, and the grinding speed was 1200 r / min.
[0050] Example 1
[0051] A surface protective glaze for 3D printing rock plate, comprising the following raw materials in parts by mass:
[0052] Basic glaze: 50 parts;
[0053] Nano-alumina: 3 parts;
[0054] Organic solvent: 50 parts;
[0055] Defoaming agent: 0.2 parts;
[0056] Leveling agent: 0.06 parts;
[0057] Polyurethane: 3 parts;
[0058] Glaze dispersant: 6 parts.
[0059] The organic solvent is dimethyl sulfoxide.
[0060] The defoamer is BYK-052 defoamer.
[0061] The leveling agent is BYK-306 leveling agent.
[0062] The polyurethane is 9370A Polyurethane.
[0063] The preparation method of the glaze dispersant comprises the following steps:
[0064] (1) adding 55 g of an acrylic acid compound and 25 g of an acrylic acid ester compound to 40 g of dimethyl sulfoxide at 75° C. and nitrogen atmosphere, and stirring at 200 r / min to obtain an acrylic acid prepolymer solution;
[0065] (2) maintaining stirring at 200 r / min, adding 10 g of vinyl triethoxysilane to the acrylic polymer solution obtained in step (1) at a rate of 5 g / min, then adding 2 g of N-vinyl pyrrolidone, and stirring at 300 r / min for 10 min to obtain a cross-linked acrylic polymer solution;
[0066] (3) Add 2 g of azobisisobutyronitrile to the cross-linked acrylic polymer solution obtained in step (2), add 10 g of an adhesion enhancer while stirring at 200 r / min, stir at 75° C. and 300 r / min for 120 min, and cool to room temperature to obtain the glaze dispersant.
[0067] The acrylic compound is prepared by mixing acrylic acid and methacrylic acid in a mass ratio of 1:2.
[0068] The acrylic acid ester compound is prepared by mixing methyl methacrylate and butyl acrylate in a mass ratio of 2:3.
[0069] The adhesion enhancer is prepared by mixing methacryloyloxyethyl phosphate and gamma-methacryloyloxypropyl trimethoxysilane in a mass ratio of 5:1.
[0070] Example 2
[0071] A surface protective glaze for 3D printing rock plate, comprising the following raw materials in parts by mass:
[0072] Basic glaze: 50 parts;
[0073] Nano-alumina: 3 parts;
[0074] Organic solvent: 50 parts;
[0075] Defoaming agent: 0.2 parts;
[0076] Leveling agent: 0.06 parts;
[0077] Polyurethane: 3 parts;
[0078] Glaze dispersant: 6 parts.
[0079] The organic solvent is dimethyl sulfoxide.
[0080] The defoamer is BYK-052 defoamer.
[0081] The leveling agent is BYK-306 leveling agent.
[0082] The polyurethane is 9370A Polyurethane.
[0083] The preparation method of the glaze dispersant comprises the following steps:
[0084] (1) adding 55 g of an acrylic acid compound and 25 g of an acrylic acid ester compound to 40 g of dimethyl sulfoxide at 75° C. and nitrogen atmosphere, and stirring at 200 r / min to obtain an acrylic acid prepolymer solution;
[0085] (2) maintaining stirring at 200 r / min, adding 10 g of vinyl triethoxysilane to the acrylic polymer solution obtained in step (1) at a rate of 5 g / min, and stirring for 10 min to obtain a cross-linked acrylic polymer solution;
[0086] (3) Add 2 g of azobisisobutyronitrile to the cross-linked acrylic polymer solution obtained in step (2), add 10 g of an adhesion enhancer while stirring at 200 r / min, stir at 75° C. and 300 r / min for 120 min, and cool to room temperature to obtain the glaze dispersant.
[0087] The acrylic compound is prepared by mixing acrylic acid and methacrylic acid in a mass ratio of 1:2.
[0088] The acrylic acid ester compound is prepared by mixing methyl methacrylate and butyl acrylate in a mass ratio of 2:3.
[0089] The adhesion enhancer is prepared by mixing methacryloyloxyethyl phosphate and gamma-methacryloyloxypropyl trimethoxysilane in a mass ratio of 5:1.
[0090] Example 3
[0091] A surface protective glaze for 3D printing rock plate, comprising the following raw materials in parts by mass:
[0092] Basic glaze: 50 parts;
[0093] Nano-alumina: 3 parts;
[0094] Organic solvent: 50 parts;
[0095] Defoaming agent: 0.2 parts;
[0096] Leveling agent: 0.06 parts;
[0097] Polyurethane: 3 parts;
[0098] Glaze dispersant: 6 parts.
[0099] The organic solvent is dimethyl sulfoxide.
[0100] The defoamer is BYK-052 defoamer.
[0101] The leveling agent is BYK-306 leveling agent.
[0102] The polyurethane is 9370A Polyurethane.
[0103] The preparation method of the glaze dispersant comprises the following steps:
[0104] (1) adding 55 g of an acrylic acid compound and 25 g of an acrylic acid ester compound to 40 g of dimethyl sulfoxide at 75° C. and nitrogen atmosphere, and stirring at 200 r / min to obtain an acrylic acid prepolymer solution;
[0105] (2) maintaining stirring at 200 r / min, adding 10 g of vinyltriethoxysilane to the acrylic polymer solution obtained in step (1) at a rate of 5 g / min, then adding 2 g of N-vinylpyrrolidone, stirring at 300 r / min for 10 min, and cooling to room temperature to obtain the glaze dispersant.
[0106] The acrylic compound is prepared by mixing acrylic acid and methacrylic acid in a mass ratio of 1:2.
[0107] The acrylic acid ester compound is prepared by mixing methyl methacrylate and butyl acrylate in a mass ratio of 2:3.
[0108] Example 4
[0109] A surface protective glaze for 3D printing rock plate, comprising the following raw materials in parts by mass:
[0110] Basic glaze: 50 parts;
[0111] Nano-alumina: 3 parts;
[0112] Organic solvent: 50 parts;
[0113] Defoaming agent: 0.2 parts;
[0114] Leveling agent: 0.06 parts;
[0115] Polyurethane: 3 parts;
[0116] Glaze dispersant: 6 parts.
[0117] The organic solvent is dimethyl sulfoxide.
[0118] The defoamer is BYK-052 defoamer.
[0119] The leveling agent is BYK-306 leveling agent.
[0120] The polyurethane is 9370A Polyurethane.
[0121] The preparation method of the glaze dispersant comprises the following steps:
[0122] (1) adding 55 g of an acrylic acid compound and 25 g of an acrylic acid ester compound to 40 g of dimethyl sulfoxide at 75° C. and nitrogen atmosphere, and stirring at 200 r / min to obtain an acrylic acid prepolymer solution;
[0123] (2) maintaining stirring at 200 r / min, adding 10 g of vinyltriethoxysilane to the acrylic polymer solution obtained in step (1) at a rate of 5 g / min, stirring at 300 r / min for 10 min, and cooling to room temperature to obtain the glaze dispersant.
[0124] The acrylic compound is prepared by mixing acrylic acid and methacrylic acid in a mass ratio of 1:2.
[0125] The acrylic acid ester compound is prepared by mixing methyl methacrylate and butyl acrylate in a mass ratio of 2:3.
[0126] Example 5
[0127] A surface protective glaze for 3D printing rock plate, comprising the following raw materials in parts by mass:
[0128] Basic glaze: 50 parts;
[0129] Nano-alumina: 3 parts;
[0130] Organic solvent: 50 parts;
[0131] Defoaming agent: 0.2 parts;
[0132] Leveling agent: 0.06 parts;
[0133] Polyurethane: 3 parts;
[0134] Glaze dispersant: 6 parts.
[0135] The organic solvent is dimethyl sulfoxide.
[0136] The defoamer is BYK-052 defoamer.
[0137] The leveling agent is BYK-306 leveling agent.
[0138] The polyurethane is 9370A Polyurethane.
[0139] The preparation method of the glaze dispersant comprises the following steps:
[0140] (1) adding 55 g of an acrylic acid compound and 25 g of an acrylic acid ester compound to 40 g of dimethyl sulfoxide at 75° C. and nitrogen atmosphere, and stirring at 200 r / min to obtain an acrylic acid prepolymer solution;
[0141] (2) maintaining stirring at 200 r / min, adding 10 g of vinyl triethoxysilane to the acrylic polymer solution obtained in step (1) at a rate of 5 g / min, then adding 2 g of N-vinyl pyrrolidone, and stirring at 300 r / min for 10 min to obtain a cross-linked acrylic polymer solution;
[0142] (3) Add 2 g of azobisisobutyronitrile to the cross-linked acrylic polymer solution obtained in step (2), add 10 g of an adhesion enhancer while stirring at 200 r / min, stir at 75° C. and 300 r / min for 120 min, and cool to room temperature to obtain the glaze dispersant.
[0143] The acrylic compound is prepared by mixing acrylic acid and methacrylic acid in a mass ratio of 1:2.
[0144] The acrylic acid ester compound is prepared by mixing methyl methacrylate and butyl acrylate in a mass ratio of 2:3.
[0145] The adhesion enhancer is methacryloyloxyethyl phosphate.
[0146] Example 6
[0147] A surface protective glaze for 3D printing rock plate, comprising the following raw materials in parts by mass:
[0148] Basic glaze: 50 parts;
[0149] Nano-alumina: 3 parts;
[0150] Organic solvent: 50 parts;
[0151] Defoaming agent: 0.2 parts;
[0152] Leveling agent: 0.06 parts;
[0153] Polyurethane: 3 parts;
[0154] Glaze dispersant: 6 parts.
[0155] The organic solvent is dimethyl sulfoxide.
[0156] The defoamer is BYK-052 defoamer.
[0157] The leveling agent is BYK-306 leveling agent.
[0158] The polyurethane is 9370A Polyurethane.
[0159] The preparation method of the glaze dispersant comprises the following steps:
[0160] (1) adding 55 g of an acrylic acid compound and 25 g of an acrylic acid ester compound to 40 g of dimethyl sulfoxide at 75° C. and nitrogen atmosphere, and stirring at 200 r / min to obtain an acrylic acid prepolymer solution;
[0161] (2) maintaining stirring at 200 r / min, adding 10 g of vinyl triethoxysilane to the acrylic polymer solution obtained in step (1) at a rate of 5 g / min, then adding 2 g of N-vinyl pyrrolidone, and stirring at 300 r / min for 10 min to obtain a cross-linked acrylic polymer solution;
[0162] (3) Add 2 g of azobisisobutyronitrile to the cross-linked acrylic polymer solution obtained in step (2), add 10 g of an adhesion enhancer while stirring at 200 r / min, stir at 75° C. and 300 r / min for 120 min, and cool to room temperature to obtain the glaze dispersant.
[0163] The acrylic compound is prepared by mixing acrylic acid and methacrylic acid in a mass ratio of 1:2.
[0164] The acrylic acid ester compound is prepared by mixing methyl methacrylate and butyl acrylate in a mass ratio of 2:3.
[0165] The adhesion enhancer is γ-methacryloxypropyltrimethoxysilane.
[0166] Comparative Example 1
[0167] A surface protective glaze for 3D printing rock plate, comprising the following raw materials in parts by mass:
[0168] Basic glaze: 50 parts;
[0169] Nano-alumina: 3 parts;
[0170] Organic solvent: 50 parts;
[0171] Defoaming agent: 0.2 parts;
[0172] Leveling agent: 0.06 parts;
[0173] Glaze dispersant: 6 parts.
[0174] The organic solvent is dimethyl sulfoxide.
[0175] The defoamer is BYK-052 defoamer.
[0176] The leveling agent is BYK-306 leveling agent.
[0177] The preparation method of the glaze dispersant comprises the following steps:
[0178] (1) adding 55 g of an acrylic acid compound and 25 g of an acrylic acid ester compound to 40 g of dimethyl sulfoxide at 75° C. and nitrogen atmosphere, and stirring at 200 r / min to obtain an acrylic acid prepolymer solution;
[0179] (2) maintaining stirring at 200 r / min, adding 10 g of vinyl triethoxysilane to the acrylic polymer solution obtained in step (1) at a rate of 5 g / min, then adding 2 g of N-vinyl pyrrolidone, and stirring at 300 r / min for 10 min to obtain a cross-linked acrylic polymer solution;
[0180] (3) Add 2 g of azobisisobutyronitrile to the cross-linked acrylic polymer solution obtained in step (2), add 10 g of an adhesion enhancer while stirring at 200 r / min, stir at 75° C. and 300 r / min for 120 min, and cool to room temperature to obtain the glaze dispersant.
[0181] The acrylic compound is prepared by mixing acrylic acid and methacrylic acid in a mass ratio of 1:2.
[0182] The acrylic acid ester compound is prepared by mixing methyl methacrylate and butyl acrylate in a mass ratio of 2:3.
[0183] The adhesion enhancer is prepared by mixing methacryloyloxyethyl phosphate and gamma-methacryloyloxypropyl trimethoxysilane in a mass ratio of 5:1.
[0184] Comparative Example 2
[0185] A surface protective glaze for 3D printing rock plate, comprising the following raw materials in parts by mass:
[0186] Basic glaze: 50 parts;
[0187] Nano-alumina: 3 parts;
[0188] Organic solvent: 50 parts;
[0189] Defoaming agent: 0.2 parts;
[0190] Leveling agent: 0.06 parts;
[0191] Polyurethane: 3 parts;
[0192] The organic solvent is dimethyl sulfoxide.
[0193] The defoamer is BYK-052 defoamer.
[0194] The leveling agent is BYK-306 leveling agent.
[0195] The polyurethane is 9370A Polyurethane.
[0196] Test Example 1:
[0197] A method for preparing a printed rock plate comprises the following steps: performing inkjet printing decoration on the surface of the 3D printed rock plate to obtain a printed 3D printed rock plate;
[0198] Use an inkjet machine to spray the surface protective glaze of the 3D printed rock plate on the surface of the printed 3D printed rock plate, and control the spraying amount to 50g / m 2 , sintered at 1120°C for 60 minutes, cooled to room temperature, and obtained a printed rock plate.
[0199] The ink is cobalt blue ink with a grayscale value of 100%.
[0200] The above-mentioned preparation method was used to prepare the printed rock plates with the surface protective glaze attached to the 3D printed rock plates obtained in Examples 1-6 and Comparative Examples 1-2, and the Lab values thereof were measured with a standard colorimeter to obtain the color development range of the ink. Among them, the L value in Lab represents brightness; the a value represents red-green value; and the b value represents yellow-blue value.
[0201] During the test, the printed 3D printed rock slabs obtained in Examples 1-6 and Comparative Examples 1-2 without applying surface protective glaze and without sintering were used as standard color cards for each and their corresponding comparative examples.
[0202] The Lab data of each embodiment and comparative example are compared with the Lab data of the respective standard color cards, and the color difference value is calculated using a formula to determine the effect of the glaze on the inkjet color.
[0203] Color difference formula: ΔEab*=[(ΔL*) 2 +(Δa*) 2 +(Δb*) 2 ] 1 / 2
[0204] Table 1: Color difference
[0205] ΔEab Example 1 1.2 Example 2 1.6 Example 3 2.7 Example 4 3.3 Example 5 1.5 Example 6 1.6 Comparative Example 1 4.2 Comparative Example 2 5.3
[0206] Test Example 2
[0207] The pull-out test was carried out with reference to GB / T5210-2006 standard, and a printed rock plate was prepared with reference to the preparation method of the printed rock plate in Test Example 1. A disc with a diameter of 30 mm was cut from the printed rock plate and placed on a pull-out testing machine for a pull-out test. The adhesion is the pulling force required for the glaze to fall off.
[0208] Table 2: Adhesion
[0209] Adhesion / MPa Example 1 8.4 Example 2 7.2 Example 3 6.1 Example 4 5.3 Example 5 7.2 Example 6 7.1 Comparative Example 1 4.1 Comparative Example 2 3.7
[0210] It can be seen from Table 1 and Table 2 that the surface protective glaze of the 3D printed rock plate prepared in Example 1 of the present invention has the best color fixing effect and the strongest adhesion. Example 2 is slightly worse than Example 1. This is because N-vinyl pyrrolidone is not added in the process of preparing the glaze dispersant, which can control the molecular weight of the acrylic polymer within a certain range, prevent the polymer molecular weight from being too large, difficult to dissolve and disperse, and is more conducive to the subsequent polymerization of the adhesion enhancer. Example 3 does not add an adhesion enhancer, and its color fixation effect and adhesion are significantly lower than those of Example 1. This proves that the introduction of methacryloxyethyl phosphate and γ-methacryloxypropyl trimethoxysilane and copolymerization with acrylic compounds, methacryloxyethyl phosphate and γ-methacryloxypropyl trimethoxysilane form chemical bonds with the substrate at high temperatures, and this chemical bond improves the thermal stability of the glaze, making it more stable during high-temperature sintering, not easy to decompose or deteriorate, and the polymer chain formed by copolymerization forms a stronger chemical bond with the surface of the substrate, significantly improving the adhesion and bonding force, giving the glaze higher mechanical strength and wear resistance, thereby improving the overall stability of the glaze. Since methacryloxyethyl phosphate and γ-methacryloxypropyl trimethoxysilane can form strong chemical bonds with the surface of the substrate at high temperatures, this chemical bond not only enhances the adhesion of the glaze, but also effectively locks the color particles to prevent the loss and diffusion of color during high-temperature firing. Example 4 uses a simple acrylic copolymer as a glaze dispersant, and its effect is significantly lower than that of Example 1. The effects of using methacryloxyethyl phosphate or γ-methacryloxypropyltrimethoxysilane alone in Examples 5 and 6 are slightly lower than those in Example 1, which proves that the combination of methacryloxyethyl phosphate and γ-methacryloxypropyltrimethoxysilane has the best effect.
[0211] In summary: by introducing methacryloxyethyl phosphate and γ-methacryloxypropyltrimethoxysilane and copolymerizing with acrylic compounds, the improved glaze has significantly improved thermal stability, mechanical stability, antioxidant and color fixation properties. These improvements enable the glaze to better maintain color stability and adhesion during high-temperature firing, thereby improving overall performance and service life. Through experimental verification, the effects of these improvements can be further confirmed to ensure their reliability and superiority in practical applications. Although this method is complex in process, the performance improvement and long-term stability it brings give it greater advantages and prospects in the application of high-performance 3D printed rock slab protective glazes.
Claims
1. A surface protective glaze for 3D printed rock slabs, characterized in that: The following raw materials are included by mass: Basic glaze: 35-55 parts; Nano-alumina: 2-5 parts; Organic solvent: 45-55 parts; Defoaming agent: 0.04-0.8 parts; Leveling agent: 0.04-0.08 parts; Polyurethane: 2-5 parts; Glaze dispersant: 4-8 parts; The preparation method of the glaze dispersant comprises the following steps: (1) adding an acrylic acid compound and an acrylic acid ester compound to dimethyl sulfoxide; (2) adding vinyl triethoxysilane and N-vinyl pyrrolidone; (3) adding azobisisobutyronitrile and an adhesion enhancer, stirring, and obtaining the glaze dispersant.
2. The surface protective glaze for 3D printing rock plate according to claim 1, characterized in that: The preparation method of the glaze dispersant comprises the following steps: (1) adding 50-60 g of an acrylic acid compound and 20-30 g of an acrylic acid ester compound to 30-50 g of dimethyl sulfoxide at 70-80° C. and nitrogen atmosphere, and stirring at 150-200 r / min to obtain an acrylic acid prepolymer solution; (2) maintaining stirring at 150-200 r / min, adding 5-15 g of vinyl triethoxysilane to the acrylic polymer solution obtained in step (1) at a rate of 3-5 g / min, then adding 1-3 g of N-vinyl pyrrolidone, and stirring at 100-300 r / min for 5-15 min to obtain a cross-linked acrylic polymer solution; (3) adding 1-3 g of azobisisobutyronitrile to the cross-linked acrylic polymer solution obtained in step (2), adding 6-12 g of an adhesion enhancer while stirring at 150-200 r / min, stirring at 70-80° C. and 100-300 r / min for 60-180 min, and cooling to room temperature to obtain the glaze dispersant.
3. The surface protective glaze for 3D printing rock slabs as claimed in claim 2, characterized in that: The acrylic compound is at least one of acrylic acid and methacrylic acid.
4. The surface protective glaze for 3D printing rock plate according to claim 2, characterized in that: The acrylic acid ester compound is at least one of methyl methacrylate and butyl acrylate.
5. The surface protective glaze for 3D printing rock plate according to claim 2, characterized in that: The adhesion enhancer is at least one of methacryloxyethyl phosphate and γ-methacryloxypropyltrimethoxysilane.
6. The surface protective glaze for 3D printing rock slabs according to any one of claims 1 to 5, characterized in that: The organic solvent is at least one of dimethyl sulfoxide, dimethylformamide, dimethylacetamide, ethyl acetate, acetone, and methyl ethyl ketone.
7. The surface protective glaze for 3D printing rock slabs according to any one of claims 1 to 5, characterized in that: The defoamer is BYK-052 defoamer, Airex902W defoamer, At least one of 111 defoamer, BYK-065 defoamer, and DeeFo2150 defoamer.
8. The surface protective glaze for 3D printing rock slabs according to any one of claims 1 to 5, characterized in that: The leveling agent is BYK-306 leveling agent, Glide450 leveling agent, EFKA-3770 leveling agent, BYK-358N leveling agent, At least one of Flow375 leveling agents.
9. The surface protective glaze for 3D printing rock slabs according to any one of claims 1 to 5, characterized in that: The polyurethane is 5703 polyurethane, 9370A polyurethane, HT-2000 polyurethane, 985A polyurethane, 2363-80AE polyurethane, 1180A At least one of polyurethane.
10. A method for preparing a surface protective glaze for 3D printed rock slabs as claimed in any one of claims 1 to 9, characterized in that: The following steps are involved: Add basic glaze, nano-alumina, organic solvent, defoamer, leveling agent, polyurethane, and glaze dispersant into a sand mill and grind them evenly to obtain the surface protective glaze for 3D printing rock slabs.
Citation Information
Patent Citations
Glaze for ultrathin ceramic rock plate and preparation method and application of glaze
CN113387582A
Rock plate protection glaze and preparation method of printed rock plate
CN117534326A
Coating composition for metal can as well as preparation method and application of coating composition
CN117925072A