Waterborne polyurethane printing ink and preparation process thereof
By combining the modified aqueous polyurethane linker and vinyl epoxy silicone crosslinking agent, an interpenetrating three-dimensional network structure is formed, which solves the hydrophobic and adhesion properties of the aqueous polyurethane ink, and significantly improves the moisture-heat resistance of the printing ink and Adhesion improves printing effect.
Patent Information
- Application Number
- CN202411219417.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-09-02
AI Technical Summary
Water-based polyurethane inks have problems such as poor hydrophobic properties, easy expansion in water, and low printing fastness, resulting in poor printing effect.
By modifying the aqueous polyurethane linker, isocyanate-based end-ended polyurethane is formed by reaction of isophorone diisocyanate and polyethylene glycol 2000, and epoxy-terminated polyurethane is formed by combining hydroxyethyl methacrylate and glycidol, and ethylene is added The base epoxy silicone assisted crosslinking agent forms an interpenetrating three-dimensional network structure, enhances the crosslinking density and cohesive strength of the chain segment, and improves adhesion and moisture-heat resistance.
It significantly improves the adhesion and humidity resistance of water-based polyurethane inks, enhances the adhesion between the coating and the substrate, avoids deformation and bubbles, and improves the printing effect.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inks, in particular to a water-based polyurethane printing ink and a preparation process thereof. Background Art
[0002] Compared with solvent-based inks, water-based inks have the advantage of being green and environmentally friendly, which can greatly reduce safety issues in food packaging and reduce the harm caused by harmful substances to the human body. Therefore, they are more widely used in the plastic food packaging industry. The most commonly used water-based ink is water-based polyurethane ink. The printing performance of water-based polyurethane ink is mainly determined by the water-based polyurethane binder. Therefore, it is particularly important to improve the heat resistance, water resistance and adhesion performance of the water-based polyurethane binder.
[0003] At present, water-based polyurethane has problems such as poor hydrophobicity and easy swelling in water. In addition, since the substrates are mostly polymer materials, the low polarity surface leads to low printing adhesion of the ink, which makes it easy for the pattern to become blurred after printing and fade when exposed to water or heat, resulting in poor printing effect. The key to improving the printing adaptability of water-based polyurethane ink is to improve the water resistance, heat resistance and adhesion performance of the polyurethane adhesive material. Therefore, it is very necessary to develop a water-based polyurethane printing ink based on the above properties. Summary of the invention
[0004] The object of the present invention is to provide a water-based polyurethane printing ink and a preparation process thereof to solve the problems raised in the above background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a water-based polyurethane printing ink and a preparation process thereof, comprising the following steps: Step 1: Ethanol and deionized water are mixed in a weight ratio of 10:1 to obtain an ethanol aqueous solution; 3-[(2,3)-epoxypropyloxy]propylmethyldimethoxysilane and dimethylethoxyvinylsilane are added to the ethanol aqueous solution, stirred for 10-15 minutes, and then heated to 70-80°C, and a catalyst dibutyltin dilaurate is added to the mixture while maintaining the temperature, and the mixture is reacted for 3-4 hours. After vacuum rotary evaporation, the product is mixed with 1,1,3,3-tetramethyldisiloxane, and a Custer catalyst is added. The mixture is reacted for 48-52 hours while maintaining the temperature at 60-70°C under a nitrogen environment to obtain a vinyl epoxy silicone co-crosslinking agent; Step 2: S1: performing vacuum dehydration treatment on polyethylene glycol 2000 at 110-120°C for 2-3h, mixing isophorone diisocyanate and polyethylene glycol 2000, raising the temperature to 70-80°C, using dibutyltin dilaurate as a catalyst, keeping the temperature for reaction for 2-3h, lowering the temperature to 50-60°C, adding dimethylolpropionic acid, raising the temperature to 70-80°C, and continuing the reaction for 1-2h. During the reaction, adding acetone to adjust the viscosity, and obtaining a polyurethane prepolymer; S2: Take a polyurethane prepolymer, mix it with hydroxyethyl methacrylate in a molar ratio of isocyanate group to hydroxyl group of 1:1, add a polymerization inhibitor p-hydroxyanisole and a catalyst dibutyltin dilaurate, heat it to 70-80°C for reaction for 2-3h to obtain a double-bond terminated polyurethane; take a polyurethane prepolymer, mix it with glycidol in a molar ratio of isocyanate group to hydroxyl group of 1:1, add a catalyst dibutyltin dilaurate, heat it to 60-70°C for reaction for 2-3h to obtain an epoxy-terminated polyurethane; mix the double-bond terminated polyurethane and the epoxy-terminated polyurethane in a mass ratio of 1:1, use triethylamine as a neutralizing agent, neutralize at 45-55°C, add distilled water, stir and emulsify, and then remove acetone by reduced pressure distillation to obtain a mixed polyurethane material; mix 92-95% of the mixed polyurethane material and 5-8% of the vinyl epoxy silicone co-crosslinking agent to obtain a waterborne polyurethane connecting material; Step 3: The carbon black is ground and sieved to obtain 300-500 mesh carbon black powder; the water-based polyurethane binder, ethanol, isopropanol, dispersant, wetting agent, leveling agent, defoaming agent, carbon black powder, photoinitiator and epoxy curing agent are mixed by weight and stirred to obtain water-based polyurethane printing ink.
[0006] Furthermore, in step 1, the molar ratio of 3-[(2,3)-epoxypropyloxy]propylmethyldimethoxysilane, dimethylethoxyvinylsilane and 1,1,3,3-tetramethyldisiloxane is 2:4:1.
[0007] Furthermore, in S1, the amounts of the components are, by weight, 110-120 parts of isophorone diisocyanate, 180-200 parts of polyethylene glycol 2000, 15-18 parts of dimethylol propionic acid, and 18-22 parts of acetone.
[0008] Furthermore, in S2, the double bond terminated polyurethane and the epoxy terminated polyurethane are mixed in a mass ratio of 1:1.
[0009] Furthermore, in S2, the solid content of the mixed polyurethane material is 30-40%.
[0010] Furthermore, in S2, the content of each component in the waterborne polyurethane connecting material, by weight percentage, is 90-95% of the mixed polyurethane material and 5-10% of the vinyl epoxy silicone co-crosslinking agent.
[0011] Further, in step 3, the contents of each component in the water-based polyurethane printing ink, by weight, are 100 parts of water-based polyurethane binder, 20 to 30 parts of ethanol, 5 to 10 parts of isopropanol, 1.2 to 1.6 parts of dispersant, 1 to 1.5 parts of wetting agent, 1.4 to 1.8 parts of leveling agent, 0.8 to 1.2 parts of defoaming agent, 8 to 13 parts of carbon black powder, 1 to 1.5 parts of photoinitiator, and 7 to 10 parts of epoxy curing agent.
[0012] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: the present invention provides a method for preparing a water-based polyurethane printing ink, wherein a water-based polyurethane binder, ethanol, isopropanol, a dispersant, a wetting agent, a leveling agent, a defoaming agent, carbon black powder, a photoinitiator, and an epoxy curing agent are mixed and stirred to obtain the water-based polyurethane printing ink.
[0013] In order to improve the printing performance of water-based polyurethane ink, the present invention modifies the water-based polyurethane binder. First, isophorone diisocyanate and polyethylene glycol 2000 are used as raw materials to react to obtain an isocyanate-terminated polyurethane prepolymer, and the polyurethane prepolymer is respectively terminated with hydroxyethyl methacrylate and glycidol, and then the two different polyurethanes are mixed to obtain a mixed polyurethane material; due to the different curing conditions of the two polyurethanes, after the mixed polyurethane material is cured, the two form an interpenetrating three-dimensional network in a physical manner, which greatly improves the crosslinking density between the chain segments, thereby improving the adhesion performance of the coating on the surface of the substrate.
[0014] The present invention also adds a vinyl epoxy silicone co-crosslinking agent. 3-[(2,3)-epoxypropyloxy]propylmethyldimethoxysilane and dimethylethoxyvinylsilane are reacted to obtain an intermediate, and then the intermediate is reacted with 1,1,3,3-tetramethyldisiloxane to obtain a vinyl epoxy silicone co-crosslinking agent. The vinyl epoxy silicone co-crosslinking agent contains multiple reactive functional groups, which can participate in the photocuring and thermal curing reactions of the mixed polyurethane material, and further crosslink the two polyurethanes by chemical bonding, so that the interaction between the chain segments is enhanced, the cohesive strength is also enhanced, and the peel strength between the cured coating and the substrate is increased. Conventional polyurethane coatings will absorb moisture from the surrounding environment in a hot and humid environment, causing wrinkles, expansion and bubbles, and the thicker the coating, the larger the bubbles. When the coating is thin, moisture will penetrate into the coating to generate osmotic pressure and form bubbles. After the vinyl epoxy silicone co-crosslinker cross-links with the polyurethane, it introduces silicon-oxygen bonds into the molecular chain segments, reducing the surface energy of the cured coating, thereby exhibiting good hydrophobicity and anti-fouling properties, ensuring that the coating does not deform in a hot and humid environment.
[0015] In addition, it should be noted that, on the one hand, there are many reactive functional groups in the vinyl epoxy silicone co-crosslinking agent. When its dosage is too high, it will lead to excessive crosslinking density, which will limit the mobility of the polyurethane chain segment, making the cohesive strength of the chain segment exceed the bonding strength between it and the adhesive substrate, thereby causing the interface adhesion to decrease; on the other hand, the vinyl epoxy silicone co-crosslinking agent has a high content of silicone, and its compatibility with the mixed polyurethane material is poor. If its dosage is too high, the two are prone to stratification after physical blending, resulting in poor stability in the ink, affecting the printing effect. Through repeated experiments, it was found that the water-based polyurethane connecting material obtained by mixing 90~95% mixed polyurethane material and 5~10% vinyl epoxy silicone co-crosslinking agent by weight percentage has the best performance. DETAILED DESCRIPTION
[0016] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.
[0017] Materials and sources used in the present invention: dispersant comes from Guangdong Zhonglian Federation Fine Chemical Co., Ltd., item number BD-40; defoamer comes from Guangzhou Dachuan Fine Chemical Co., Ltd., item number H448; leveling agent comes from Shanghai Banggao Chemical Co., Ltd., item number JS-3018; wetting agent comes from Guangzhou Yangsong Trading Co., Ltd., item number WT-500; carbon black comes from Anhui Heiyu Pigment New Materials Co., Ltd., model PowCarbon ® 4311F.
[0018] Embodiment 1: A water-based polyurethane printing ink and a preparation process thereof, comprising the following steps: Step 1: Ethanol and deionized water are mixed in a weight ratio of 10:1 to obtain an ethanol aqueous solution; 3-[(2,3)-epoxypropoxy]propylmethyldimethoxysilane and dimethylethoxyvinylsilane are added to the ethanol aqueous solution, stirred for 10 minutes, then heated to 70°C, and a catalyst dibutyltin dilaurate is added to the mixture while maintaining the temperature, and the mixture is reacted for 3 hours. After vacuum rotary evaporation, the product is mixed with 1,1,3,3-tetramethyldisiloxane, and a Custer catalyst is added. The mixture is reacted for 48 hours while maintaining the temperature at 60°C under a nitrogen environment to obtain a vinyl epoxy silicone co-crosslinking agent; wherein the molar ratio of 3-[(2,3)-epoxypropoxy]propylmethyldimethoxysilane, dimethylethoxyvinylsilane, and 1,1,3,3-tetramethyldisiloxane is 2:4:1; Step 2: S1: vacuum dehydrating polyethylene glycol 2000 at 110°C for 2h, mixing 120g of isophorone diisocyanate with 180g of polyethylene glycol 2000, heating to 70°C, using dibutyltin dilaurate as a catalyst, keeping the temperature for reaction for 2h, cooling to 50°C, adding 17g of dimethylolpropionic acid, heating to 70°C and continuing the reaction for 1h, adding 20g of acetone during the reaction to adjust the viscosity, and obtaining a polyurethane prepolymer; S2: Take a polyurethane prepolymer, mix it with hydroxyethyl methacrylate in a molar ratio of isocyanate group to hydroxyl group of 1:1, add a polymerization inhibitor p-hydroxyanisole and a catalyst dibutyltin dilaurate, heat it to 70°C and react for 2h to obtain a double-bond terminated polyurethane; take a polyurethane prepolymer, mix it with glycidol in a molar ratio of isocyanate group to hydroxyl group of 1:1, add a catalyst dibutyltin dilaurate, heat it to 60°C and react for 2h to obtain an epoxy-terminated polyurethane; mix the double-bond terminated polyurethane and the epoxy-terminated polyurethane in a mass ratio of 1:1, use triethylamine as a neutralizer, neutralize at 45°C, add distilled water, stir and emulsify, and then remove acetone by reduced pressure distillation to obtain a mixed polyurethane material with a solid content of 30%; by weight, mix 95% of the mixed polyurethane material and 5% of the vinyl epoxy silicone co-crosslinking agent to obtain a water-based polyurethane connecting material; Step 3: The carbon black was ground and sieved to obtain a 500-mesh carbon black powder; 100 g of an aqueous polyurethane binder, 26 g of ethanol, 8 g of isopropanol, 1.4 g of a dispersant, 1.3 g of a wetting agent, 1.6 g of a leveling agent, 1.1 g of a defoaming agent, 12 g of carbon black powder, 1 g of a photoinitiator 1173, and 8 g of isophorone diamine were mixed and stirred to obtain an aqueous polyurethane printing ink.
[0019] Embodiment 2: A water-based polyurethane printing ink and a preparation process thereof, comprising the following steps: Step 1: Ethanol and deionized water are mixed in a weight ratio of 10:1 to obtain an ethanol aqueous solution; 3-[(2,3)-epoxypropoxy]propylmethyldimethoxysilane and dimethylethoxyvinylsilane are added to the ethanol aqueous solution, stirred for 13 minutes, then heated to 75°C, and a catalyst dibutyltin dilaurate is added to the mixture while maintaining the temperature, and the mixture is reacted for 3.5 hours. After vacuum rotary evaporation, the product is mixed with 1,1,3,3-tetramethyldisiloxane, and a Custer catalyst is added. The mixture is reacted for 50 hours while maintaining the temperature at 65°C under a nitrogen environment to obtain a vinyl epoxy silicone co-crosslinking agent; wherein the molar ratio of 3-[(2,3)-epoxypropoxy]propylmethyldimethoxysilane, dimethylethoxyvinylsilane, and 1,1,3,3-tetramethyldisiloxane is 2:4:1; Step 2: S1: vacuum dehydrating polyethylene glycol 2000 at 115°C for 2.5 hours, mixing 120g of isophorone diisocyanate with 180g of polyethylene glycol 2000, heating to 75°C, using dibutyltin dilaurate as a catalyst, keeping the temperature for reaction for 2.5 hours, cooling to 55°C, adding 17g of dimethylolpropionic acid, heating to 75°C and continuing the reaction for 1.5 hours, adding 20g of acetone during the reaction to adjust the viscosity, and obtaining a polyurethane prepolymer; S2: Take a polyurethane prepolymer, mix it with hydroxyethyl methacrylate in a molar ratio of isocyanate group to hydroxyl group of 1:1, add a polymerization inhibitor p-hydroxyanisole and a catalyst dibutyltin dilaurate, heat it to 75°C and react for 2.5 hours to obtain a double-bond terminated polyurethane; take a polyurethane prepolymer, mix it with glycidol in a molar ratio of isocyanate group to hydroxyl group of 1:1, add a catalyst dibutyltin dilaurate, heat it to 65°C and react for 2.5 hours to obtain an epoxy-terminated polyurethane; mix the double-bond terminated polyurethane and the epoxy-terminated polyurethane in a mass ratio of 1:1, use triethylamine as a neutralizer, neutralize at 50°C, add distilled water, stir and emulsify, and then remove acetone by reduced pressure distillation to obtain a mixed polyurethane material with a solid content of 30%; by weight, mix 93% of the mixed polyurethane material and 7% of the vinyl epoxy silicone co-crosslinking agent to obtain a water-based polyurethane connecting material; Step 3: The carbon black was ground and sieved to obtain a 500-mesh carbon black powder; 100 g of an aqueous polyurethane binder, 26 g of ethanol, 8 g of isopropanol, 1.4 g of a dispersant, 1.3 g of a wetting agent, 1.6 g of a leveling agent, 1.1 g of a defoaming agent, 12 g of carbon black powder, 1 g of a photoinitiator 1173, and 8 g of isophorone diamine were mixed and stirred to obtain an aqueous polyurethane printing ink.
[0020] Embodiment 3: A water-based polyurethane printing ink and a preparation process thereof, comprising the following steps: Step 1: Ethanol and deionized water are mixed in a weight ratio of 10:1 to obtain an ethanol aqueous solution; 3-[(2,3)-epoxypropoxy]propylmethyldimethoxysilane and dimethylethoxyvinylsilane are added to the ethanol aqueous solution, stirred for 15 minutes, then heated to 80°C, and a catalyst dibutyltin dilaurate is added to the mixture while maintaining the temperature, and the mixture is reacted for 4 hours. After vacuum rotary evaporation, the product is mixed with 1,1,3,3-tetramethyldisiloxane, and a Custer catalyst is added. The mixture is reacted for 52 hours while maintaining the temperature at 70°C under a nitrogen environment to obtain a vinyl epoxy silicone co-crosslinking agent; wherein the molar ratio of 3-[(2,3)-epoxypropoxy]propylmethyldimethoxysilane, dimethylethoxyvinylsilane, and 1,1,3,3-tetramethyldisiloxane is 2:4:1; Step 2: S1: vacuum dehydrating polyethylene glycol 2000 at 120°C for 3h, mixing 120g of isophorone diisocyanate with 180g of polyethylene glycol 2000, heating to 80°C, using dibutyltin dilaurate as a catalyst, keeping the temperature for reaction for 3h, cooling to 60°C, adding 17g of dimethylolpropionic acid, heating to 80°C and continuing the reaction for 2h, adding 20g of acetone during the reaction to adjust the viscosity, and obtaining a polyurethane prepolymer; S2: Take a polyurethane prepolymer, mix it with hydroxyethyl methacrylate in a molar ratio of isocyanate group to hydroxyl group of 1:1, add a polymerization inhibitor p-hydroxyanisole and a catalyst dibutyltin dilaurate, heat it to 80°C for reaction for 3h, and obtain a double-bond terminated polyurethane; take a polyurethane prepolymer, mix it with glycidol in a molar ratio of isocyanate group to hydroxyl group of 1:1, add a catalyst dibutyltin dilaurate, heat it to 70°C for reaction for 3h, and obtain an epoxy-terminated polyurethane; mix the double-bond terminated polyurethane and the epoxy-terminated polyurethane in a mass ratio of 1:1, use triethylamine as a neutralizer, neutralize at 55°C, add distilled water, stir and emulsify, and then remove acetone by reduced pressure distillation to obtain a mixed polyurethane material with a solid content of 30%; by weight, mix 90% of the mixed polyurethane material and 10% of the vinyl epoxy silicone co-crosslinking agent to obtain a water-based polyurethane connecting material; Step 3: The carbon black was ground and sieved to obtain a 500-mesh carbon black powder; 100 g of an aqueous polyurethane binder, 26 g of ethanol, 8 g of isopropanol, 1.4 g of a dispersant, 1.3 g of a wetting agent, 1.6 g of a leveling agent, 1.1 g of a defoaming agent, 12 g of carbon black powder, 1 g of a photoinitiator 1173, and 8 g of isophorone diamine were mixed and stirred to obtain an aqueous polyurethane printing ink.
[0021] Comparative Example 1: The polyurethane connecting material was prepared by conventional technology.
[0022] Step 1: The polyethylene glycol 2000 was subjected to vacuum dehydration treatment at 110°C for 2 hours, 120g of isophorone diisocyanate was mixed with 180g of polyethylene glycol 2000, the temperature was raised to 70°C, dibutyltin dilaurate was used as a catalyst, the temperature was kept for reaction for 2 hours, the temperature was lowered to 50°C, 17g of dimethylolpropionic acid was added, the temperature was raised to 70°C and the reaction was continued for 1 hour, 20g of acetone was added during the reaction to adjust the viscosity, and a polyurethane prepolymer was obtained; triethylamine was used as a neutralizing agent, the mixture was neutralized at 45°C, distilled water was added for stirring and emulsification, 4.6g of ethylenediamine was added for reaction for 30 minutes, and the acetone was removed by reduced pressure distillation to obtain a water-based polyurethane binder with a solid content of 30%; Step 2: The carbon black was ground and sieved to obtain a 500-mesh carbon black powder; 100 g of an aqueous polyurethane binder, 26 g of ethanol, 8 g of isopropanol, 1.4 g of a dispersant, 1.3 g of a wetting agent, 1.6 g of a leveling agent, 1.1 g of a defoaming agent, 12 g of carbon black powder, 1 g of a photoinitiator 1173, and 8 g of isophorone diamine were mixed and stirred to obtain an aqueous polyurethane printing ink.
[0023] Comparative Example 2: No vinyl epoxy silicone co-crosslinking agent was added, and the other parameters were the same as those in Example 2.
[0024] Step 1: S1: vacuum dehydrating polyethylene glycol 2000 at 115°C for 2.5 hours, mixing 120g of isophorone diisocyanate with 180g of polyethylene glycol 2000, heating to 75°C, using dibutyltin dilaurate as a catalyst, keeping the temperature for reaction for 2.5 hours, cooling to 55°C, adding 17g of dimethylolpropionic acid, heating to 75°C and continuing the reaction for 1.5 hours, adding 20g of acetone during the reaction to adjust the viscosity, and obtaining a polyurethane prepolymer; S2: Take a polyurethane prepolymer, mix it with hydroxyethyl methacrylate in a molar ratio of isocyanate group to hydroxyl group of 1:1, add a polymerization inhibitor p-hydroxyanisole and a catalyst dibutyltin dilaurate, heat it to 75°C and react for 2.5 hours to obtain a double-bond terminated polyurethane; take a polyurethane prepolymer, mix it with glycidol in a molar ratio of isocyanate group to hydroxyl group of 1:1, add a catalyst dibutyltin dilaurate, heat it to 65°C and react for 2.5 hours to obtain an epoxy-terminated polyurethane; mix the double-bond terminated polyurethane and the epoxy-terminated polyurethane in a mass ratio of 1:1, use triethylamine as a neutralizer, neutralize at 50°C, add distilled water, stir and emulsify, and then remove acetone by reduced pressure distillation to obtain a water-based polyurethane connecting material with a solid content of 30%; Step 3: The carbon black was ground and sieved to obtain a 500-mesh carbon black powder; 100 g of an aqueous polyurethane binder, 26 g of ethanol, 8 g of isopropanol, 1.4 g of a dispersant, 1.3 g of a wetting agent, 1.6 g of a leveling agent, 1.1 g of a defoaming agent, 12 g of carbon black powder, 1 g of a photoinitiator 1173, and 8 g of isophorone diamine were mixed and stirred to obtain an aqueous polyurethane printing ink.
[0025] Comparative Example 3: The dosage of the vinyl epoxy silicone co-crosslinking agent was increased, and the other parameters were the same as those in Example 3.
[0026] Step 1: Ethanol and deionized water are mixed in a weight ratio of 10:1 to obtain an ethanol aqueous solution; 3-[(2,3)-epoxypropoxy]propylmethyldimethoxysilane and dimethylethoxyvinylsilane are added to the ethanol aqueous solution, stirred for 15 minutes, then heated to 80°C, and a catalyst dibutyltin dilaurate is added to the mixture while maintaining the temperature, and the mixture is reacted for 4 hours. After vacuum rotary evaporation, the product is mixed with 1,1,3,3-tetramethyldisiloxane, and a Custer catalyst is added. The mixture is reacted for 52 hours while maintaining the temperature at 70°C under a nitrogen environment to obtain a vinyl epoxy silicone co-crosslinking agent; wherein the molar ratio of 3-[(2,3)-epoxypropoxy]propylmethyldimethoxysilane, dimethylethoxyvinylsilane, and 1,1,3,3-tetramethyldisiloxane is 2:4:1; Step 2: S1: vacuum dehydrating polyethylene glycol 2000 at 120°C for 3h, mixing 120g of isophorone diisocyanate with 180g of polyethylene glycol 2000, heating to 80°C, using dibutyltin dilaurate as a catalyst, keeping the temperature for reaction for 3h, cooling to 60°C, adding 17g of dimethylolpropionic acid, heating to 80°C and continuing the reaction for 2h, adding 20g of acetone during the reaction to adjust the viscosity, and obtaining a polyurethane prepolymer; S2: Take a polyurethane prepolymer, mix it with hydroxyethyl methacrylate in a molar ratio of isocyanate group to hydroxyl group of 1:1, add a polymerization inhibitor p-hydroxyanisole and a catalyst dibutyltin dilaurate, heat it to 80°C for reaction for 3h, and obtain a double-bond terminated polyurethane; take a polyurethane prepolymer, mix it with glycidol in a molar ratio of isocyanate group to hydroxyl group of 1:1, add a catalyst dibutyltin dilaurate, heat it to 70°C for reaction for 3h, and obtain an epoxy-terminated polyurethane; mix the double-bond terminated polyurethane and the epoxy-terminated polyurethane in a mass ratio of 1:1, use triethylamine as a neutralizer, neutralize at 55°C, add distilled water, stir and emulsify, and then remove acetone by reduced pressure distillation to obtain a mixed polyurethane material with a solid content of 30%; by weight, mix 85% of the mixed polyurethane material and 15% of the vinyl epoxy silicone co-crosslinking agent to obtain a water-based polyurethane connecting material; Step 3: The carbon black was ground and sieved to obtain a 500-mesh carbon black powder; 100 g of an aqueous polyurethane binder, 26 g of ethanol, 8 g of isopropanol, 1.4 g of a dispersant, 1.3 g of a wetting agent, 1.6 g of a leveling agent, 1.1 g of a defoaming agent, 12 g of carbon black powder, 1 g of a photoinitiator 1173, and 8 g of isophorone diamine were mixed and stirred to obtain an aqueous polyurethane printing ink.
[0027] Experiment: A water-based polyurethane printing ink was prepared by referring to the methods in Examples 1 to 3 and Comparative Examples 1 to 3 and coated on the surface of a PET plate (Foshan Shouke Plastic Technology Co., Ltd., item number 033), dried naturally at room temperature for 24 hours, placed in an oven at 50°C for 24 hours, and heated with 30 mW / cm2 The film was irradiated with ultraviolet light for 30-40 minutes and thermally cured at 120°C for 2 hours to form a film with a thickness of 50 μm. The hydrophilicity and hydrophobicity of the dried film were measured by the dynamic contact angle measuring instrument and the peel strength tester was used to test the T-peel strength according to GB / T 2791-1995. The film was placed in a test box with a set temperature of 70±1°C and a humidity of 95±3% for 3 days to test the moisture and heat resistance, and the surface morphology of the film was observed. The experimental results are shown in the following table.
[0028]
[0029] Conclusion: The data of Examples 1 to 3 show that the water-based polyurethane ink prepared by the present invention has good performance. The data of Example 1 and Comparative Example 1 show that, compared with conventional water-based polyurethane ink, the product in Example 1 has stronger surface hydrophobicity, greater adhesion strength with the substrate, and has resistance to moisture and heat. The data of Example 2 and Comparative Example 2 show that the addition of a vinyl epoxy silicone co-crosslinking agent is beneficial to improving the adhesion between the ink and the substrate, and can also improve the hydrophobicity and moisture and heat resistance. The data of Example 3 and Comparative Example 3 show that excessive use of a vinyl epoxy silicone co-crosslinking agent will result in a decrease in the adhesion between the ink and the substrate.
[0030] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A process for preparing a water-based polyurethane printing ink, characterized in that: The following steps are involved: The carbon black is ground and sieved to obtain carbon black powder; a water-based polyurethane connecting material, ethanol, isopropanol, a dispersant, a wetting agent, a leveling agent, a defoaming agent, the carbon black powder, a photoinitiator and an epoxy curing agent are mixed and stirred to obtain a water-based polyurethane printing ink.
2. The process for preparing a water-based polyurethane printing ink according to claim 1, characterized in that: The particle size of carbon black powder is 300~500 mesh.
3. The process for preparing a water-based polyurethane printing ink according to claim 1, characterized in that: The content of each component in the water-based polyurethane printing ink, by weight, is 100 parts of water-based polyurethane binder, 20-30 parts of ethanol, 5-10 parts of isopropanol, 1.2-1.6 parts of dispersant, 1-1.5 parts of wetting agent, 1.4-1.8 parts of leveling agent, 0.8-1.2 parts of defoaming agent, 8-13 parts of carbon black powder, 1-1.5 parts of photoinitiator, and 7-10 parts of epoxy curing agent.
4. The process for preparing a water-based polyurethane printing ink according to claim 1, characterized in that: The preparation method of the waterborne polyurethane connecting material is as follows: S1: performing vacuum dehydration treatment on polyethylene glycol 2000 at 110-120°C for 2-3h, mixing isophorone diisocyanate and polyethylene glycol 2000, raising the temperature to 70-80°C, using dibutyltin dilaurate as a catalyst, keeping the temperature for reaction for 2-3h, lowering the temperature to 50-60°C, adding dimethylolpropionic acid, raising the temperature to 70-80°C, and continuing the reaction for 1-2h. During the reaction, adding acetone to adjust the viscosity, and obtaining a polyurethane prepolymer; S2: Take a polyurethane prepolymer, mix it with hydroxyethyl methacrylate in a molar ratio of isocyanate group to hydroxyl group of 1:1, add inhibitor p-hydroxyanisole and catalyst dibutyltin dilaurate, heat it to 70-80℃ and react for 2-3h to obtain a double-bond terminated polyurethane; take a polyurethane prepolymer, mix it with glycidol in a molar ratio of isocyanate group to hydroxyl group of 1:1, add catalyst dibutyltin dilaurate, heat it to 60-70℃ and react for 2-3h to obtain an epoxy-terminated polyurethane; mix the double-bond terminated polyurethane and the epoxy-terminated polyurethane in a mass ratio of 1:1, use triethylamine as a neutralizing agent, neutralize at 45-55℃, add distilled water, stir and emulsify, and then remove acetone by reduced pressure distillation to obtain a mixed polyurethane material; mix the mixed polyurethane material and vinyl epoxy silicone co-crosslinking agent to obtain a waterborne polyurethane connecting material.
5. The process for preparing a water-based polyurethane printing ink according to claim 4, characterized in that: In S1, the amounts of the components, by weight, are 110-120 parts of isophorone diisocyanate, 180-200 parts of polyethylene glycol 2000, 15-18 parts of dimethylol propionic acid, and 18-22 parts of acetone.
6. The process for preparing a water-based polyurethane printing ink according to claim 4, characterized in that: In S2, double bond terminated polyurethane and epoxy terminated polyurethane are mixed in a mass ratio of 1:
1.
7. The process for preparing a water-based polyurethane printing ink according to claim 4, characterized in that: In S2, the solid content of the mixed polyurethane material is 30-40%.
8. The process for preparing a water-based polyurethane printing ink according to claim 4, characterized in that: In S2, the content of each component in the waterborne polyurethane binder, by weight percentage, is 90-95% of the mixed polyurethane material and 5-10% of the vinyl epoxy silicone co-crosslinking agent.
9. The process for preparing a water-based polyurethane printing ink according to claim 4, characterized in that: The preparation method of the vinyl epoxy silicone co-crosslinking agent is as follows: ethanol and deionized water are mixed at a weight ratio of 10:1 to obtain an ethanol aqueous solution; 3-[(2,3)-epoxypropoxy]propylmethyldimethoxysilane and dimethylethoxyvinylsilane are added to the ethanol aqueous solution, stirred for 10-15 minutes, heated to 70-80°C, added with a catalyst dibutyltin dilaurate while maintaining the temperature, reacted for 3-4 hours, and after reduced pressure rotary evaporation, the product was mixed with 1,1,3,3-tetramethyldisiloxane, a Custer catalyst was added, and the temperature was maintained at 60-70°C under a nitrogen environment for 48-52 hours to obtain the vinyl epoxy silicone co-crosslinking agent.
10. The process for preparing a water-based polyurethane printing ink according to claim 9, characterized in that: The molar ratio of 3-[(2,3)-glycidoxy]propylmethyldimethoxysilane, dimethylethoxyvinylsilane, and 1,1,3,3-tetramethyldisiloxane is 2:4:1.
Citation Information
Patent Citations
Environmentally friendly hydrophobic polyurethane ink and preparation method thereof
CN106009907A
Environment-friendly acrylate modified waterborne polyurethane printing ink and preparation method thereof
CN112029341A
Water-based UV ink and preparation method thereof
CN116179012A
High-wear-resistance super-fast-drying ink and preparation method thereof
CN116656173A
Environment-friendly printing process for environment-friendly packaging box
CN116715991A
Cited By
Weather-resistant waterborne polyurethane ink and preparation method thereof
CN119799065A
High-adhesion varnished wire priming paint and preparation method thereof
CN120173498A
A primer paint for enameled wire with high adhesion and its preparation method
CN120173498B
Low-smoke halogen-free flame-retardant polyolefin sheath environment-friendly cable and preparation method thereof
CN120484366A
Low-smoke halogen-free flame-retardant polyolefin sheath environmental protection cable and preparation method thereof
CN120484366B