Antibacterial antistatic cellulose blended yarn and preparation method thereof

By blending antibacterial and antistatic polyester fibers in cellulose blended yarn and using modified components, the antistatic, antibacterial and flame retardant properties of cellulose blended yarn are improved, and the problem of insufficient performance of traditional cellulose blended yarns is solved. , achieving efficient and lasting versatility.

CN118979320AInactive Publication Date: 2024-11-19DEZHOU HUANYUAN ECOLOGICAL TECH
View PDF 0 Cites 10 Cited by

Patent Information

Application Number
CN202411459018.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional cellulose blended yarns have poor antistatic properties, antibacterial properties and flame retardancy, which easily absorb dust and bacteria in the air, and lack of hydrophilicity, resulting in reduced comfort and limited application areas. Conventional antistatic agents and Polyester has poor compatibility and is difficult to maintain performance for a long time.

Method used

It uses Tencel fiber and antibacterial and antistatic polyester fiber, and uses modified carbon nanotubes, composite antibacterial agents and flame retardants to modify melamine polyphosphate, composite essential oil microcapsule powder and modified chitosan. Improve the antistatic, antibacterial and flame retardant properties of cellulose blended yarns, and improve mechanical strength and comfort through modification treatment.

Benefits of technology

It realizes the stable and efficient flame retardant, antibacterial and antistatic properties of cellulose blended yarns, maintains good mechanical strength and comfort, extends the durability of performance, and is suitable for multifunctional textiles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of cellulose blended yarns, in particular to an antibacterial and antistatic cellulose blended yarn and a preparation method thereof. The antibacterial and antistatic cellulose blended yarn is prepared by blending tencel fibers and antibacterial and antistatic polyester fibers according to the mass part ratio of 1: 5, and the antibacterial and antistatic polyester fibers comprise, by mass, 10-30 parts of tencel fibers and 10-30 parts of antibacterial and antistatic polyester fibers. The preparation raw materials comprise 85-90 parts of polyester chips, 8-12 parts of modified carbon nanotubes, 3-4 parts of a composite antibacterial agent, 3-4 parts of a flame retardant, and 0.5-0.7 part of a flame retardant synergist, and the composite antibacterial agent is prepared by mixing composite essential oil microcapsule powder and modified chitosan according to a mass part ratio of 5: 3. The antibacterial and antistatic cellulose blended yarn has stable and efficient flame retardance, hygroscopicity, antibacterial property and antistatic property, is high in mechanical strength and comfort level, and has important application value in the technical field of cellulose blended yarns.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of cellulose blended yarns, and in particular to an antibacterial and antistatic cellulose blended yarn and a preparation method thereof. Background Art

[0002] Polyester, also known as polyester fiber, is a synthetic fiber made from organic dibasic acids and diols through chemical condensation. It is the simplest and cheapest of the three major synthetic fiber processes. It has the advantages of high strength, wear resistance, good elasticity, not easy to deform, corrosion resistance, light resistance, good chemical resistance, easy to wash and quick drying, etc. It is widely used in the fields of civil textiles (such as clothing, bedding, decorative fabrics, etc.) and industrial fiber products (such as filter materials, insulation materials, tire cord, etc.).

[0003] With the advancement of modern science and technology and the improvement of people's living standards, society has higher and higher functional requirements for textile fabrics. However, traditional cellulose blended yarns have poor antistatic, antibacterial and flame retardancy. When processed into fabrics and used, they will be subjected to physical effects such as friction and extrusion to generate static electricity. Static electricity can easily absorb dust particles in the air, and dust contains a variety of viruses, bacteria and other substances harmful to the human body. Static electricity can easily cause local release of small sparks, resulting in itchy and uncomfortable electric shocks. In addition, in the hot summer, people tend to sweat after activities. Ordinary cellulose blended yarns have poor hydrophilicity and weak moisture absorption capacity. Sweat is not easy to discharge. After long-term use, there will be a feeling of stuffiness, which reduces the comfort of wearing. In addition, it is easier to breed bacteria under humid conditions, which seriously limits the application field of cellulose blended yarns.

[0004] At present, antistatic agents, flame retardants and antibacterial agents are often added to improve the performance of cellulose blended yarns, but conventional antistatic agents, flame retardants and antibacterial agents have poor compatibility with polyester and are easily lost after multiple washings, resulting in loss of performance and difficulty in long-term use. Therefore, there is an urgent need to invent a cellulose blended yarn with antibacterial, antistatic and flame retardant properties and long-term stable performance to meet the higher demands in the field of cellulose blended yarn technology. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present application provides an antibacterial and antistatic cellulose blended yarn and a preparation method thereof. The antibacterial and antistatic cellulose blended yarn of the present application has stable and efficient flame retardancy, hygroscopicity, antibacterial and antistatic properties, and has high mechanical strength and comfort, and has important application value in the field of cellulose blended yarn technology.

[0006] In the first aspect, the present application provides an antibacterial and antistatic cellulose blended yarn, which adopts the following technical solution: The invention discloses an antibacterial and antistatic cellulose blended yarn. The cellulose blended yarn is prepared by blending tencel fiber and antibacterial and antistatic polyester fiber in a weight ratio of 1:5. The antibacterial and antistatic polyester fiber is prepared by raw materials including, by weight, 85-90 parts of polyester chips, 8-12 parts of modified carbon nanotubes, 3-4 parts of composite antibacterial agents, 3-4 parts of flame retardants, and 0.5-0.7 parts of flame retardant synergist. The composite antibacterial agent is prepared by mixing composite essential oil microcapsule powder and modified chitosan in a weight ratio of 5:3.

[0007] By adopting the above technical scheme, polyester chips are used as the basic raw material of cellulose blended yarn to provide the strength and structural basis of the yarn. Modified carbon nanotubes are grafted with organic molecular chains through chemical bonding, which improves the interfacial compatibility with the matrix, reduces agglomeration and promotes uniform dispersion. This not only improves the antistatic performance, but also enhances the mechanical properties of the matrix. Functional groups such as hydroxyl groups, polyethylene glycol, and quaternary ammonium salts on the organic molecular chains further enhance the hydrophilicity, antibacterial and antistatic properties. The composite antibacterial agent is prepared by mixing composite essential oil microcapsule powder and modified chitosan in a mass ratio of 5:3. Among them, the composite essential oil microcapsule powder forms microcapsule wall materials through the reaction of the N=C bond in the characteristic group NCO of isophorone diisocyanate and the NH bond in polyglutamic acid benzyl ester after breaking, which improves the dispersibility and compatibility of the microcapsules and enhances the antibacterial properties. Modified chitosan has excellent antibacterial properties, can change the permeability of bacterial cell membranes and inhibit the DNA transcription process inside microbial cells, achieving high-efficiency antibacterial properties. The antibacterial property of chitosan modified with tannic acid is improved, and its catechol group can form strong hydrogen bonds with hydroxyl radicals on the surface of polyester to improve compatibility. The synergistic effect of the two significantly improves the antibacterial property and stability of cellulose blended yarn. Flame retardants can release flame-flaming gases such as phosphoric acid during combustion, forming a protective layer to slow down the combustion rate, prevent the spread of flames, and improve flame retardant properties. Flame retardant synergists enhance the flame retardant effect and improve the flame retardant efficiency. In summary, the present invention achieves multiple functions of cellulose blended yarns such as antibacterial, antistatic, flame retardant, and hygroscopicity by carefully selecting and proportioning various components, while maintaining good mechanical strength and comfort, and has important application value.

[0008] Preferably, the flame retardant is modified melamine polyphosphate, and the preparation method of the modified melamine polyphosphate comprises the following steps: S21, according to the mass ratio, 20 parts of hydrotalcite with a particle size of 0.5 micrometer and 30 parts of water are prepared into an aqueous suspension; S22, dispersing 200 parts of melamine polyphosphate in a solution consisting of 8 parts of 3-aminopropyltriethoxysilane, 200 parts of ethanol and 60 parts of water according to parts by mass to obtain a mixed solution; S23. Slowly add the aqueous suspension to the mixed solution, heat to 5°C, stir at 300 rpm, react for 30 minutes, filter, and vacuum dry at 80°C for 24 hours, grind and sieve to obtain modified melamine polyphosphate with a particle size of 1-3 μm.

[0009] By adopting the above technical scheme, in the preparation process of modified melamine polyphosphate, hydrotalcite and water are first prepared into an aqueous suspension, and then melamine polyphosphate is dispersed in a solution consisting of 3-aminopropyltriethoxysilane, ethanol and water to obtain a mixed solution. Then, the aqueous suspension is slowly added dropwise to the mixed solution, heated to 5°C, the stirring rate is 300rpm, and after reacting for 30min, it is filtered, and after vacuum drying at 80°C for 24h, it is ground and sieved to obtain a modified melamine polyphosphate with a particle size of 1-3μm. The melamine polyphosphate modified by the coupling agent has good compatibility with polyester, which is conducive to improving the dispersibility of the flame retardant in polyester fiber, thereby improving its flame retardant properties. In addition, the modified melamine polyphosphate can release flame-retardant gases such as phosphoric acid during combustion, and these gases can form a protective layer, effectively slowing down the combustion rate and preventing the spread of flames.

[0010] Preferably, the method for preparing the composite essential oil microcapsule powder comprises the following steps: S31, according to the mass parts, 6 parts of sandalwood essential oil, 4 parts of clove essential oil and 3 parts of isophorone diisocyanate were uniformly mixed to obtain an oil phase; S32. According to the mass fractions, add the oil phase into 20 parts of 6% sodium lignin sulfonate aqueous solution, stir continuously at 45°C and 10000r / min for 20 minutes, then heat to 73°C, add 0.4 parts of polyglutamate benzyl ester and continue stirring for 2.5 hours, filter, wash and dry to obtain composite essential oil microcapsule powder with a particle size of 2-3 microns.

[0011] By adopting the above technical scheme, a composite essential oil microcapsule powder is prepared: after the N=C bond in the characteristic group -NCO of isophorone diisocyanate and the NH bond in polybenzyl glutamate are broken, the active hydrogen in polybenzyl glutamate is connected to N, and the rest of the polybenzyl glutamate is connected to C. As the polymerization reaction proceeds, the molecular chain of the prepolymer becomes longer and longer, and the product gradually deposits on the surface of the essential oil, eventually forming the wall material of the microcapsule; the microcapsules are modified by polybenzyl glutamate, thereby improving the dispersibility and compatibility of the microcapsules, thereby improving the antibacterial properties of the cellulose blended yarn.

[0012] Preferably, the preparation method of the modified chitosan is: adding 20g of chitosan to 200ml of acetic acid solution with a mass concentration of 3%, stirring and dissolving to obtain a chitosan solution; adding 70g of tannic acid to 500ml of methanol, stirring and dissolving to obtain a tannic acid solution; adjusting the temperature of the chitosan solution to 36°C, adding the tannic acid solution and 6g of a carboxyl activator while stirring, stirring and reacting for 24h, and after the reaction is completed, dialyzing and freeze-drying to obtain the modified chitosan.

[0013] By adopting the above technical scheme, chitosan has excellent antibacterial properties, and can achieve high antibacterial properties by changing the permeability of bacterial cell membranes and inhibiting the DNA transcription process inside microbial cells; at the same time, chitosan is also modified by tannic acid, and the antibacterial properties of chitosan after phenol modification are improved to a certain extent. The catechol groups contained therein can also form strong hydrogen bonds with the hydroxyl radicals contained on the surface of polyester, thereby improving the compatibility of modified chitosan with the matrix, thereby improving the antibacterial properties of cellulose blended yarn. There is a synergistic effect between modified chitosan and composite essential oil microcapsule powder, which can significantly improve the antibacterial properties and stability of cellulose blended yarn, and it is long-lasting and efficient.

[0014] Preferably, the carboxyl activator is composed of N-hydroxysuccinimide and 1-ethyl-(3-dimethylaminopropyl)carbodiimide in a mass ratio of 3:2.

[0015] Preferably, the method for preparing the modified carbon nanotubes comprises the following steps: S61, placing 40 g of carbon nanotubes in a conical flask, then adding 1.5 L of 98% concentrated sulfuric acid and 0.5 L of 98% concentrated hydrochloric acid, and ultrasonically treating in a 65°C water bath for 10 h, adding deionized water to dilute the mixture after it is cooled to room temperature, centrifuging, and washing with anhydrous ethanol and deionized water for 5 times in sequence, drying, and grinding to obtain carboxylated carbon nanotubes; S62, in a reactor equipped with a stirring device, 25.2 g of diethylenetriamine, 100 g of methoxypolyethylene glycol aldehyde, 30 mL of piperidine and 200 mL of pyridine were stirred and mixed uniformly, the temperature was raised to 42° C., and the reaction was kept warm for 10 hours. After the reaction was completed, the reaction was naturally cooled, the solvent was removed by rotary evaporation, and then purified by column chromatography and rotary evaporation to obtain intermediate 1; S63. In a reactor equipped with a stirring device, 20 g of carboxylated carbon nanotubes were mixed with 200 mL of N,N-dimethylformamide, and magnetically stirred for 3 h to evenly disperse the carboxylated carbon nanotubes. Then, 40 g of intermediate 1, 2.5 g of dicyclohexylcarbodiimide and 0.7 g of 4-dimethylaminopyridine were added in sequence. After uniform stirring, the mixture was placed in a 43°C water bath for 5 h of ultrasonic treatment. The water bath was then removed and magnetically stirred for 12 h at room temperature. After the reaction was completed, the mixture was filtered, washed with anhydrous ethanol 4 times, dried and ground to obtain intermediate 2. S64. Under nitrogen protection, mix 20 g of intermediate 2 with 200 mL of N,N-dimethylformamide in a reactor equipped with a stirring device. After magnetic stirring for 70 minutes, add 30 g of 6-chloro-1-hexanol and 15 g of potassium carbonate. Control the reaction temperature to 78°C and stir the reaction for 14 hours. After the reaction is completed, filter and wash with anhydrous ethanol three times, dry and grind to obtain modified carbon nanotubes.

[0016] By adopting the above technical scheme, the prepared modified carbon nanotubes are grafted with organic molecular chains through chemical bonding, that is, an organic layer is formed on the surface of the modified carbon nanotubes, which can greatly improve the interface compatibility between the carbon nanotubes and the matrix, reduce the agglomeration of the carbon nanotubes, thereby promoting the uniform dispersion of the modified carbon nanotubes in the matrix, giving full play to the antistatic properties of the carbon nanotubes, and also strengthening the matrix; not only that, the carbon nanotubes are grafted with organic molecular chains, which can effectively prevent the migration and seepage of organic molecules and ensure the durability of various properties; in addition, the organic molecular chains contain hydroxyl groups, polyethylene glycol, and quaternary ammonium salts, among which the hydroxyl groups can not only produce chemical bonding with the polyester molecular chains during the melt spinning process to improve the interaction force with the matrix, The organic molecular chains are not easy to fall off during rinsing, thus improving the durability of performance; the introduction of hydrophilic chain polyethylene glycol structure can greatly improve the hydrophilic properties of the matrix, and the polyethylene glycol is a flexible chain segment that can further improve the mechanical properties of the matrix; the introduction of quaternary ammonium salt ions will produce strong electrostatic interactions between the positively charged and negatively charged bacteria, and will have a strong adsorption effect on the bacteria, effectively improving the antibacterial and antistatic properties of the matrix.

[0017] Preferably, the flame retardant synergist consists of manganese glycerophosphate and polyborosiloxane in a mass ratio of 4:3.

[0018] By adopting the above technical scheme, manganese glycerophosphate, as an effective flame retardant synergist, can release phosphate ions during the combustion process. These ions can react with the hydroxyl groups in polyester to form phosphate esters, thereby forming a protective phosphate layer on the surface of the polyester fiber. This phosphate layer can effectively isolate oxygen, slow down the combustion rate, and improve the flame retardant properties of the material. Polyborosiloxane is a polymer compound containing boron and silicon elements, which has excellent thermal stability and flame retardant properties. During the combustion process, polyborosiloxane can decompose to produce substances such as boric acid and silicate, which can form a dense protective layer on the fiber surface to prevent the spread of flames and improve the flame retardant properties of the material. The synergistic effect between manganese glycerophosphate and polyborosiloxane is manifested in that the two can promote each other during the combustion process and jointly improve the flame retardant properties of polyester fibers. The phosphate ions released by manganese glycerophosphate can interact with substances such as boric acid and silicate produced by the decomposition of polyborosiloxane to form a more stable and dense protective layer, thereby more effectively preventing the spread of flames and improving the flame retardant properties of the material.

[0019] In a second aspect, the present application provides a method for preparing an antibacterial and antistatic cellulose blended yarn, using the following technical solution: As a general technical concept, the present application also provides a method for preparing the above-mentioned antibacterial and antistatic cellulose blended yarn, comprising the following steps: S91. According to the mass fractions, polyester chips, modified carbon nanotubes, composite antibacterial agent, flame retardant, flame retardant synergist and coupling agent are sequentially added into a high-speed mixer for mixing, and then extruded into granules through a twin-screw extruder, and then melt-spun through a high-speed spinning machine to obtain antibacterial and antistatic polyester fibers, wherein the process temperatures of melt spinning are 250° C. in zone 1, 260° C. in zone 2; 275° C. in zone 3, and 270° C. in zone 4; the spinning speed is 5000 m / min, and the draft ratio is 3 times; S92. According to the mass fractions, the antibacterial and antistatic polyester fiber and the Tencel fiber are combined on a drawing frame to make slivers, which are drawn and twisted on a roving frame, further drawn and twisted on a spinning frame, wound and finally combined to obtain antibacterial and antistatic cellulose blended yarn.

[0020] In summary, the present application includes at least one of the following beneficial technical effects: 1. Highly effective flame retardancy: The introduction of modified melamine polyphosphate can release flame retardant gases such as phosphoric acid during combustion, forming a protective layer, effectively slowing down the combustion speed and preventing the spread of flames. In addition, the use of coupling agents improves the dispersion of flame retardants in polyester fibers, further enhancing flame retardancy.

[0021] 2. Excellent antibacterial property: The composite antibacterial agent is made by mixing composite essential oil microcapsule powder and modified chitosan, which have a synergistic effect. Composite essential oil microcapsule powder has good dispersibility, compatibility and antibacterial properties; while modified chitosan achieves high antibacterial efficiency by changing the permeability of bacterial cell membranes and inhibiting the DNA transcription process inside microbial cells. Tannic acid-modified chitosan further improves the antibacterial property and enhances compatibility with the matrix.

[0022] 3. Antistatic performance: After the modified carbon nanotubes are grafted with organic molecular chains, the interfacial compatibility with the matrix is ​​greatly improved, the agglomeration phenomenon is reduced, the uniform dispersion is promoted, and the antistatic performance of the carbon nanotubes is fully exerted. At the same time, the introduction of quaternary ammonium salt ions also helps to improve the antistatic performance.

[0023] 4. High mechanical strength and comfort: The modified melamine polyphosphate and modified carbon nanotubes have good compatibility with polyester, which is beneficial to improve the dispersion of flame retardants and antistatic agents in polyester fibers, thereby improving their flame retardant and antistatic properties; at the same time, after chitosan is modified with tannic acid, the catechol groups contained in it can also form strong hydrogen bonds with the hydroxyl radicals contained on the surface of polyester, thereby improving the compatibility of modified chitosan with the matrix, thereby improving the antibacterial properties and mechanical strength of cellulose blended yarns.

[0024] 5. Long-lasting and stable performance: Carbon nanotubes grafted onto organic molecular chains can effectively prevent the migration and seepage of organic molecules, ensuring the durability of various performance properties; in addition, the organic molecular chains contain functional groups such as hydroxyl, polyethylene glycol, and quaternary ammonium salts, which can produce chemical bonds with polyester molecular chains, enhance the interaction force with the matrix, and make the organic molecular chains less likely to fall off during rinsing, thereby improving the durability of performance. DETAILED DESCRIPTION

[0025] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0026] In the following examples and preparation examples, 1 portion means 200 g.

[0027] Preparation Example 1 Preparation of modified melamine polyphosphate The preparation method of modified melamine polyphosphate comprises the following steps: S21, according to the mass ratio, 20 parts of hydrotalcite with a particle size of 0.5 micrometer and 30 parts of water are prepared into an aqueous suspension; S22, dispersing 200 parts of melamine polyphosphate in a solution consisting of 8 parts of 3-aminopropyltriethoxysilane, 200 parts of ethanol and 60 parts of water according to parts by mass to obtain a mixed solution; S23. Slowly add the aqueous suspension to the mixed solution, heat to 5°C, stir at 300 rpm, react for 30 minutes, filter, and vacuum dry at 80°C for 24 hours, grind and sieve to obtain modified melamine polyphosphate with a particle size of 1-3 μm.

[0028] Preparation Example 2 Preparation of composite essential oil microcapsule powder The preparation method of composite essential oil microcapsule powder comprises the following steps: S31, according to the mass parts, 6 parts of sandalwood essential oil, 4 parts of clove essential oil and 3 parts of isophorone diisocyanate were uniformly mixed to obtain an oil phase; S32. According to the mass fractions, add the oil phase into 20 parts of 6% sodium lignin sulfonate aqueous solution, stir continuously at 45°C and 10000r / min for 20 minutes, then heat to 73°C, add 0.4 parts of polyglutamate benzyl ester and continue stirring for 2.5 hours, filter, wash and dry to obtain composite essential oil microcapsule powder with a particle size of 2-3 microns.

[0029] Preparation Example 3 Preparation of modified chitosan The preparation method of modified chitosan is as follows: adding 20g of chitosan to 200ml of acetic acid solution with a mass concentration of 3%, stirring and dissolving to obtain a chitosan solution; adding 70g of tannic acid to 500ml of methanol, stirring and dissolving to obtain a tannic acid solution; adjusting the temperature of the chitosan solution to 36°C, adding the tannic acid solution and 6g of a carboxyl activator (the carboxyl activator is composed of N-hydroxysuccinimide and 1-ethyl-(3-dimethylaminopropyl)carbodiimide in a mass ratio of 3:2) while stirring, stirring and reacting for 24h, and after the reaction is completed, dialyzing and freeze-drying to obtain the modified chitosan.

[0030] Preparation Example 4 Preparation of modified carbon nanotubes The method for preparing modified carbon nanotubes comprises the following steps: S61, placing 40 g of carbon nanotubes in a conical flask, then adding 1.5 L of 98% concentrated sulfuric acid and 0.5 L of 98% concentrated hydrochloric acid, and ultrasonically treating in a 65°C water bath for 10 h, adding deionized water to dilute the mixture after it is cooled to room temperature, centrifuging, and washing with anhydrous ethanol and deionized water for 5 times in sequence, drying, and grinding to obtain carboxylated carbon nanotubes; S62, in a reactor equipped with a stirring device, 25.2 g of diethylenetriamine, 100 g of methoxypolyethylene glycol aldehyde, 30 mL of piperidine and 200 mL of pyridine were stirred and mixed uniformly, the temperature was raised to 42° C., and the reaction was kept warm for 10 hours. After the reaction was completed, the reaction was naturally cooled, the solvent was removed by rotary evaporation, and then purified by column chromatography and rotary evaporation to obtain intermediate 1; S63. In a reactor equipped with a stirring device, 20 g of carboxylated carbon nanotubes were mixed with 200 mL of N,N-dimethylformamide, and magnetically stirred for 3 h to evenly disperse the carboxylated carbon nanotubes. Then, 40 g of intermediate 1, 2.5 g of dicyclohexylcarbodiimide and 0.7 g of 4-dimethylaminopyridine were added in sequence. After uniform stirring, the mixture was placed in a 43°C water bath for 5 h of ultrasonic treatment. The water bath was then removed and magnetically stirred for 12 h at room temperature. After the reaction was completed, the mixture was filtered, washed with anhydrous ethanol 4 times, dried and ground to obtain intermediate 2. S64. Under nitrogen protection, mix 20 g of intermediate 2 with 200 mL of N,N-dimethylformamide in a reactor equipped with a stirring device. After magnetic stirring for 70 minutes, add 30 g of 6-chloro-1-hexanol and 15 g of potassium carbonate. Control the reaction temperature to 78°C and stir the reaction for 14 hours. After the reaction is completed, filter and wash with anhydrous ethanol three times, dry and grind to obtain modified carbon nanotubes.

[0031] Example 1

[0032] An antibacterial and antistatic cellulose blended yarn, the cellulose blended yarn is made by blending tencel fiber and antibacterial and antistatic polyester fiber in a mass ratio of 1:5, the antibacterial and antistatic polyester fiber is prepared by raw materials including, by mass, 85 parts of polyester chips, 8 parts of modified carbon nanotubes, 3 parts of composite antibacterial agent, 3 parts of flame retardant, and 0.5 parts of flame retardant synergist, wherein the composite antibacterial agent is made by mixing composite essential oil microcapsule powder and modified chitosan in a mass ratio of 5:3, the flame retardant is modified melamine polyphosphate, and the flame retardant synergist is composed of manganese glycerophosphate and polyborosiloxane in a mass ratio of 4:3; The method for preparing the antibacterial and antistatic cellulose blended yarn comprises the following steps: S91. According to the mass fractions, polyester chips, modified carbon nanotubes, composite antibacterial agent, flame retardant, flame retardant synergist and coupling agent are sequentially added into a high-speed mixer for mixing, and then extruded into granules through a twin-screw extruder, and then melt-spun through a high-speed spinning machine to obtain antibacterial and antistatic polyester fibers, wherein the process temperatures of melt spinning are 250° C. in zone 1, 260° C. in zone 2; 275° C. in zone 3, and 270° C. in zone 4; the spinning speed is 5000 m / min, and the draft ratio is 3 times; S92. According to the mass fractions, the antibacterial and antistatic polyester fiber and the Tencel fiber are combined on a drawing frame to make slivers, which are drawn and twisted on a roving frame, further drawn and twisted on a spinning frame, wound and finally combined to obtain antibacterial and antistatic cellulose blended yarn.

[0033] Example 2

[0034] An antibacterial and antistatic cellulose blended yarn, the cellulose blended yarn is made by blending tencel fiber and antibacterial and antistatic polyester fiber in a mass ratio of 1:5, the antibacterial and antistatic polyester fiber is prepared by raw materials including, by mass, 90 parts of polyester chips, 12 parts of modified carbon nanotubes, 4 parts of composite antibacterial agents, 4 parts of flame retardants, and 0.7 parts of flame retardant synergists, wherein the composite antibacterial agent is made by mixing composite essential oil microcapsule powder and modified chitosan in a mass ratio of 5:3, the flame retardant is modified melamine polyphosphate, and the flame retardant synergist is composed of manganese glycerophosphate and polyborosiloxane in a mass ratio of 4:3; The method for preparing the antibacterial and antistatic cellulose blended yarn comprises the following steps: S91. According to the mass fractions, polyester chips, modified carbon nanotubes, composite antibacterial agent, flame retardant, flame retardant synergist and coupling agent are sequentially added into a high-speed mixer for mixing, and then extruded into granules through a twin-screw extruder, and then melt-spun through a high-speed spinning machine to obtain antibacterial and antistatic polyester fibers, wherein the process temperatures of melt spinning are 250° C. in zone 1, 260° C. in zone 2; 275° C. in zone 3, and 270° C. in zone 4; the spinning speed is 5000 m / min, and the draft ratio is 3 times; S92. According to the mass fractions, the antibacterial and antistatic polyester fiber and the Tencel fiber are combined on a drawing frame to make slivers, which are drawn and twisted on a roving frame, further drawn and twisted on a spinning frame, wound and finally combined to obtain antibacterial and antistatic cellulose blended yarn.

[0035] Example 3

[0036] An antibacterial and antistatic cellulose blended yarn, the cellulose blended yarn is made by blending tencel fiber and antibacterial and antistatic polyester fiber in a mass ratio of 1:5, the antibacterial and antistatic polyester fiber is prepared by raw materials including, by mass, 88 parts of polyester chips, 10 parts of modified carbon nanotubes, 3.5 parts of composite antibacterial agent, 3.5 parts of flame retardant, and 0.6 parts of flame retardant synergist, wherein the composite antibacterial agent is made by mixing composite essential oil microcapsule powder and modified chitosan in a mass ratio of 5:3, the flame retardant is modified melamine polyphosphate, and the flame retardant synergist is composed of manganese glycerophosphate and polyborosiloxane in a mass ratio of 4:3; The method for preparing the antibacterial and antistatic cellulose blended yarn comprises the following steps: S91. According to the mass fractions, polyester chips, modified carbon nanotubes, composite antibacterial agent, flame retardant, flame retardant synergist and coupling agent are sequentially added into a high-speed mixer for mixing, and then extruded into granules through a twin-screw extruder, and then melt-spun through a high-speed spinning machine to obtain antibacterial and antistatic polyester fibers, wherein the process temperatures of melt spinning are 250° C. in zone 1, 260° C. in zone 2; 275° C. in zone 3, and 270° C. in zone 4; the spinning speed is 5000 m / min, and the draft ratio is 3 times; S92. According to the mass fractions, the antibacterial and antistatic polyester fiber and the Tencel fiber are combined on a drawing frame to make slivers, which are drawn and twisted on a roving frame, further drawn and twisted on a spinning frame, wound and finally combined to obtain antibacterial and antistatic cellulose blended yarn.

[0037] Comparative Example 1 The same as Example 3, except that an equal amount of melamine polyphosphate is used instead of the flame retardant.

[0038] Comparative Example 2 The same as Example 3, except that: the composite antibacterial agent is composite essential oil microcapsule powder.

[0039] Comparative Example 3 The same as Example 3, except that: the composite antibacterial agent is modified chitosan.

[0040] Comparative Example 4 The same as Example 3, except that an equal amount of carbon nanotubes are used instead of modified carbon nanotubes.

[0041] Comparative Example 5 The same as Example 3, except that: the flame retardant synergist is manganese glycerophosphate.

[0042] Comparative Example 6 The same as Example 3, except that: the flame retardant synergist is polyborosiloxane.

[0043] Performance testing The antibacterial and antistatic cellulose blended yarns prepared in Examples 1 to 3 and Comparative Examples 1 to 6 were respectively measured for breaking elongation according to the national standard GB / T14344-93 "Test method for breaking strength and breaking elongation of synthetic filaments and textured yarns"; the test results are shown in Table 1; The antibacterial and antistatic cellulose blended yarns prepared in Examples 1 to 3 and Comparative Examples 1 to 6 were respectively made into fabrics using a circular knitting method, and were cut into test samples according to different test standards, and the following performance tests were performed: Flame retardant test: The test method is GB / T5455-2014 Textile combustion performance - Determination of vertical damage length, smoldering and afterflaming time; the test results are shown in Table 1; Antistatic: The national standard GB / T 12703.2-2009 "Textile electrostatic test method Part 2: Charge surface density" is used to measure the charge surface density of the fabric (uC / m 2 ), thereby testing the antistatic performance (the smaller the charge surface density, the better the antistatic performance); the test results are shown in Table 1; Water absorption rate: The water absorption rate was measured using the national standard GB / T 21655.1-2008 "Evaluation of moisture absorption and quick-drying properties of textiles Part 1: Single combination test method"; the test results are shown in Table 1; Antibacterial rate: The antibacterial rate of Escherichia coli and Staphylococcus aureus was determined using the national standard GB / T 20944.2-2007 "Evaluation of antibacterial properties of textiles - Part 2: Absorption method"; the test results are shown in Table 1; Durability: The flame retardant, antistatic and antibacterial properties of the samples were measured before and after washing 50 times using the same standard. The test results are shown in Table 2.

[0044] Table 1 Performance test

[0045] Table 2 Durability test

[0046] Analyzing the data in Table 1 and Table 2, we can see that: 1) The antibacterial and antistatic cellulose blended yarns prepared in Examples 1 to 3 have stable and efficient flame retardancy, hygroscopicity, antibacterial and antistatic properties, and high mechanical strength and comfort, and have important application value in the field of cellulose blended yarn technology.

[0047] 2) The comparative analysis of the performance of the antibacterial and antistatic cellulose blended yarns prepared in Example 3 and Comparative Example 1 shows that the modified melamine polyphosphate prepared in the present application has good compatibility with polyester, which is beneficial to improve the dispersibility of melamine polyphosphate in polyester fiber, thereby improving its flame retardant properties. In addition, the modified melamine polyphosphate can release flame-retardant gases such as phosphoric acid during combustion, and these gases can form a protective layer to effectively slow down the combustion speed and prevent the spread of flames.

[0048] 3) The performance comparison analysis of the antibacterial and antistatic cellulose blended yarns prepared in combination with Example 3 and Comparative Examples 2-3 shows that the composite antibacterial agent is prepared by mixing composite essential oil microcapsule powder and modified chitosan in a mass ratio of 5:3, and the composite essential oil microcapsule powder has good dispersibility, compatibility and antibacterial properties; while the modified chitosan achieves high-efficiency antibacterial properties by changing the permeability of bacterial cell membranes and inhibiting the DNA transcription process inside microbial cells, and the chitosan modified with tannic acid further improves the antibacterial properties and enhances the compatibility with the matrix. The composite essential oil microcapsule powder and modified chitosan work synergistically to significantly improve the comprehensive properties of cellulose blended yarns, especially the antibacterial properties.

[0049] 4) The comparative analysis of the performance of the antibacterial and antistatic cellulose blended yarns prepared in Example 3 and Comparative Example 4 shows that the modified carbon nanotubes prepared in the present application are grafted with organic molecular chains through chemical bonding, that is, an organic layer is formed on the surface thereof, which can greatly improve the interfacial compatibility between the carbon nanotubes and the matrix, reduce the agglomeration of the carbon nanotubes, thereby promoting the uniform dispersion of the modified carbon nanotubes in the matrix, giving full play to the antistatic properties of the carbon nanotubes, and also enhancing the matrix; not only that, the carbon nanotubes are grafted with organic molecular chains, which can effectively prevent the migration and seepage of organic molecules and ensure the durability of various properties; in addition, the organic molecular chains contain hydroxyl groups, polyethylene glycol, and quaternary ammonium salts, wherein the hydroxyl groups can not only produce chemical bonding with the polyester molecular chains during the melt spinning process, thereby improving the interaction force with the matrix, The organic molecular chains are not easy to fall off during rinsing, thus improving the durability of performance; the introduction of hydrophilic chain polyethylene glycol structure can greatly improve the hydrophilic properties of the matrix, and the polyethylene glycol is a flexible chain segment that can further improve the mechanical properties of the matrix; the introduction of quaternary ammonium salt ions will produce strong electrostatic interactions between the positively charged and negatively charged bacteria, and will have a strong adsorption effect on the bacteria, effectively improving the antibacterial and antistatic properties of the matrix.

[0050] 5) The performance comparison analysis of the antibacterial and antistatic cellulose blended yarns prepared in combination with Example 3 and Comparative Examples 5-6 shows that the flame retardant synergist is composed of manganese glycerophosphate and polyborosiloxane in a mass ratio of 4:3. The synergistic effect between manganese glycerophosphate and polyborosiloxane can promote each other during the combustion process and jointly improve the flame retardant properties of polyester fibers. The phosphate ions released by manganese glycerophosphate can interact with substances such as boric acid and silicate produced by the decomposition of polyborosiloxane to form a more stable and dense protective layer, thereby more effectively preventing the spread of flames and improving the flame retardant properties of the material.

[0051] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation methods of the present application can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the protection scope of the present application.

Claims

1. An antibacterial and antistatic cellulose blended yarn, characterized in that: The cellulose blended yarn is prepared by blending tencel fiber and antibacterial and antistatic polyester fiber in a mass ratio of 1:

5. The antibacterial and antistatic polyester fiber is prepared by raw materials including, by mass, 85-90 parts of polyester chips, 8-12 parts of modified carbon nanotubes, 3-4 parts of composite antibacterial agents, 3-4 parts of flame retardants, and 0.5-0.7 parts of flame retardant synergist. The composite antibacterial agent is prepared by mixing composite essential oil microcapsule powder and modified chitosan in a mass ratio of 5:

3. The preparation method of the composite essential oil microcapsule powder comprises the following steps: S31, according to the mass parts, 6 parts of sandalwood essential oil, 4 parts of clove essential oil and 3 parts of isophorone diisocyanate were uniformly mixed to obtain an oil phase; S32. According to the mass fractions, add the oil phase into 20 parts of 6% sodium lignin sulfonate aqueous solution, stir continuously at 45°C and 10000r / min for 20 minutes, then heat to 73°C, add 0.4 parts of polyglutamate benzyl ester and continue stirring for 2.5 hours, filter, wash and dry to obtain composite essential oil microcapsule powder with a particle size of 2-3 microns.

2. The antibacterial and antistatic cellulose blended yarn according to claim 1, characterized in that: The flame retardant is modified melamine polyphosphate, and the preparation method of the modified melamine polyphosphate comprises the following steps: S21, according to the mass ratio, 20 parts of hydrotalcite with a particle size of 0.5 micrometer and 30 parts of water are prepared into an aqueous suspension; S22, dispersing 200 parts of melamine polyphosphate in a solution consisting of 8 parts of 3-aminopropyltriethoxysilane, 200 parts of ethanol and 60 parts of water according to parts by mass to obtain a mixed solution; S23. Slowly add the aqueous suspension to the mixed solution, heat to 5°C, stir at 300 rpm, react for 30 minutes, filter, and vacuum dry at 80°C for 24 hours, grind and sieve to obtain modified melamine polyphosphate with a particle size of 1-3 μm.

3. The antibacterial and antistatic cellulose blended yarn according to claim 1, characterized in that: The preparation method of the modified chitosan is as follows: adding 20g of chitosan to 200ml of acetic acid solution with a mass concentration of 3%, stirring and dissolving to obtain a chitosan solution; adding 70g of tannic acid to 500ml of methanol, stirring and dissolving to obtain a tannic acid solution; adjusting the temperature of the chitosan solution to 36°C, adding the tannic acid solution and 6g of a carboxyl activator while stirring, stirring and reacting for 24h, and after the reaction is completed, dialyzing and freeze-drying to obtain the modified chitosan.

4. The antibacterial and antistatic cellulose blended yarn according to claim 3, characterized in that: The carboxyl activator is composed of N-hydroxysuccinimide and 1-ethyl-(3-dimethylaminopropyl)carbodiimide in a mass ratio of 3:

2.

5. The antibacterial and antistatic cellulose blended yarn according to claim 1, characterized in that: The method for preparing the modified carbon nanotubes comprises the following steps: S61, placing 40 g of carbon nanotubes in a conical flask, then adding 1.5 L of 98% concentrated sulfuric acid and 0.5 L of 98% concentrated hydrochloric acid, and ultrasonically treating in a 65°C water bath for 10 h, adding deionized water to dilute the mixture after it is cooled to room temperature, centrifuging, and washing with anhydrous ethanol and deionized water for 5 times in sequence, drying, and grinding to obtain carboxylated carbon nanotubes; S62, in a reactor equipped with a stirring device, 25.2 g of diethylenetriamine, 100 g of methoxypolyethylene glycol aldehyde, 30 mL of piperidine and 200 mL of pyridine were stirred and mixed uniformly, the temperature was raised to 42° C., and the reaction was kept warm for 10 hours. After the reaction was completed, the reaction was naturally cooled, the solvent was removed by rotary evaporation, and then purified by column chromatography and rotary evaporation to obtain intermediate 1; S63. In a reactor equipped with a stirring device, 20 g of carboxylated carbon nanotubes were mixed with 200 mL of N,N-dimethylformamide, and magnetically stirred for 3 h to evenly disperse the carboxylated carbon nanotubes. Then, 40 g of intermediate 1, 2.5 g of dicyclohexylcarbodiimide and 0.7 g of 4-dimethylaminopyridine were added in sequence. After uniform stirring, the mixture was placed in a 43°C water bath for 5 h of ultrasonic treatment. The water bath was then removed and magnetically stirred for 12 h at room temperature. After the reaction was completed, the mixture was filtered, washed with anhydrous ethanol 4 times, dried and ground to obtain intermediate 2. S64. Under nitrogen protection, mix 20 g of intermediate 2 with 200 mL of N,N-dimethylformamide in a reactor equipped with a stirring device. After magnetic stirring for 70 minutes, add 30 g of 6-chloro-1-hexanol and 15 g of potassium carbonate. Control the reaction temperature to 78°C and stir the reaction for 14 hours. After the reaction is completed, filter and wash with anhydrous ethanol three times, dry and grind to obtain modified carbon nanotubes.

6. The antibacterial and antistatic cellulose blended yarn according to claim 1, characterized in that: The flame retardant synergist consists of manganese glycerophosphate and polyborosiloxane in a mass ratio of 4:

3.

7. A method for preparing an antibacterial and antistatic cellulose blended yarn according to any one of claims 1 to 6, characterized in that: The following steps are involved: S81. According to the mass fractions, polyester chips, modified carbon nanotubes, composite antibacterial agent, flame retardant and flame retardant synergist are sequentially added into a high-speed mixer for mixing, and then extruded into granules through a twin-screw extruder, and then melt-spinned through a high-speed spinning machine to obtain antibacterial and antistatic polyester fibers, wherein the process temperatures of melt spinning are 250° C. in zone 1, 260° C. in zone 2; 275° C. in zone 3, and 270° C. in zone 4; the spinning speed is 5000 m / min, and the draft ratio is 3 times; S82. According to the mass fractions, the antibacterial and antistatic polyester fiber and the tencel fiber are combined on a drawing frame to make slivers, which are then drawn and twisted on a roving frame, further drawn and twisted on a spinning frame, wound and finally combined to obtain antibacterial and antistatic cellulose blended yarns.

Citation Information

Cited By

  • Environment-friendly breathable polyester silk fabric and preparation process thereof

    CN119392504A

  • Antibacterial breathable yarn and antibacterial breathable socks thereof

    CN119736740A

  • Composite short fiber and preparation method thereof

    CN119913635A

  • Composite short fiber and preparation method thereof

    CN119913635B

  • Preparation method of environment-friendly wood-plastic composite material

    CN119931181A