Sagger for positive electrode material of lithium ion battery and preparation method of sagger

By constructing a kyanite-KAlSi2O6 core-shell structure, it blocks the contact between the lithium-ion battery cathode material and the sagger, solves the problem of erosion and thermal shock resistance of the sagger material during the calcination process of the lithium-ion battery cathode material, and improves the resistance of the sagger. Aggressive and high temperature mechanical properties.

CN118754688APending Publication Date: 2024-10-11ZHENGZHOU NON FERROUS METALS RES INST CO LTD OF CHALCO

Patent Information

Application Number
CN202410991585.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

During the calcination process of lithium-ion battery cathode materials, the sagger material is eroded by the lithium-ion battery cathode material and suffers from thermal expansion mismatch, resulting in structural damage and reduced thermal shock resistance. Potassium aluminate is introduced into the existing technology to improve corrosion resistance but mechanical properties. decline.

Method used

Using raw materials such as kyanite, potassium carbonate, silica, industrial alumina, tabular corundum and activated α-alumina, the kyanite-KAlSi2O6 core-shell structure is constructed to prevent the positive electrode material from contacting the sagger and improve high-temperature mechanics. performance.

Benefits of technology

It effectively improves the corrosion resistance and high-temperature mechanical properties of the sagger used for lithium-ion battery cathode materials, avoids corrosion reactions, and enhances high-temperature flexural strength and thermal shock resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754688A_ABST
    Figure CN118754688A_ABST
Patent Text Reader

Abstract

The invention provides a sagger for a positive electrode material of a lithium ion battery and a preparation method, and belongs to the field of refractory materials. The sagger comprises the following raw materials in percentage by mass: 65%-75% of kyanite, 0.5%-3% of potassium carbonate, 0.5%-2% of silicon dioxide, 1%-5% of industrial aluminum oxide, 12%-20% of tabular corundum and 4%-8% of active alpha-aluminum oxide. By reasonably designing the raw material composition of the sagger, a kyanite-KAlSi2O6 core-shell structure is constructed, and KAlSi2O6 coats the surfaces of kyanite particles, so that the contact between the positive electrode material and kyanite in the sagger is effectively prevented, and the erosion reaction is avoided; meanwhile, KAlSi2O6 has good sinterability and forms tight connection with a surrounding matrix at a high temperature, and the high-temperature mechanical property of the sagger is improved. Therefore, the erosion resistance and the high-temperature mechanical property of the sagger for the lithium ion battery positive electrode material are improved at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of refractory materials, and in particular to a sagger for positive electrode materials of lithium-ion batteries and a preparation method thereof. Background Art

[0002] Due to its advantages such as high specific energy, long cycle life, high operating voltage and no pollution, lithium-ion batteries have become a widely used energy storage power source in industries such as portable electronic devices and new energy vehicles. The positive electrode material is the most critical component of lithium batteries. Among them, the positive electrode material of lithium-ion batteries has become the mainstream material for the current research and application of positive electrode materials due to its higher energy density, excellent stability and large capacity. The positive electrode material of lithium-ion batteries is mainly prepared by calcining its precursor mixed powder at 900-1100℃. During the calcination process, the sagger is not only subjected to the thermal stress shock caused by the rapid temperature change, but also eroded by the positive electrode material of the lithium-ion battery, which seriously affects the service life of the sagger material.

[0003] At present, mullite and cordierite are mostly used to prepare saggers. However, because the lithium ions in the positive electrode materials of lithium batteries are extremely active at the calcination temperature and have strong permeability, they react with the aluminum silicon components in the sagger materials to form low-melting point compounds, which cause the sagger materials to dissolve, and then cause the sagger material structure to be damaged; at the same time, the compounds generated by the reaction do not match the thermal expansion coefficient of the sagger materials, which reduces the thermal shock resistance of the sagger materials, causes cracking and peeling of the saggers, and also causes the sagger structure to be damaged. In order to increase the service life of the sagger materials, the prior art introduces potassium aluminate (K 2 O.Al 2 O 3 ), potassium aluminate basically does not react with the positive electrode material of the lithium-ion battery, and can improve the corrosion resistance of the sagger. However, after the introduction of potassium aluminate, the mechanical properties of the sagger material decrease, and the thermal shock resistance tends to weaken. Due to its negative effect on the mechanical properties, the amount of potassium aluminate introduced cannot be too much. Therefore, during the calcination process, the aluminum silicon components in the sagger material, such as mullite, will still contact with the positive electrode material of the lithium-ion battery, and it is difficult to completely avoid the sagger from being corroded and damaged. In view of this, it is necessary to provide a sagger for lithium-ion battery positive electrode materials and a preparation method thereof to overcome the above-mentioned defects. Summary of the invention

[0004] The present application provides a sagger for lithium-ion battery positive electrode materials and a preparation method thereof, in order to solve the following technical problem: how to simultaneously improve the corrosion resistance and high-temperature mechanical properties of the sagger for lithium-ion battery positive electrode materials.

[0005] In a first aspect, the present application provides a sagger for positive electrode materials of lithium-ion batteries. The sagger comprises the following raw materials, measured by mass fraction: kyanite: 65%-75%, potassium carbonate: 0.5%-3%, silicon dioxide: 0.5%-2%, industrial alumina: 1%-5%, plate-like corundum: 12%-20%, and active α-alumina: 4%-8%.

[0006] Optionally, in terms of mass fraction, in the chemical composition of the kyanite, Al 2 O 3 ≥57.0%,SiO 2 ≤39.0%,TiO 2 ≤0.4%,Fe 2 O 3 ≤1.2%, CaO≤0.4%, MgO≤0.3%, K 2 O≤0.2%,Na 2 O≤0.1%.

[0007] Optionally, the model of the kyanite is D57 kyanite.

[0008] Optionally, the particle size of the kyanite is 0-1mm; the particle size of the potassium carbonate is 0-0.044mm; the particle size of the silicon dioxide is 0-0.044mm; the particle size of the industrial alumina is 0-0.044mm; the particle size of the plate-like corundum is 0-0.044mm; and the particle size of the activated α-alumina is 0-0.005mm.

[0009] Optionally, in terms of mass fraction, in the chemical composition of potassium carbonate, K 2 CO 3 ≥99.9; in terms of mass fraction, the chemical composition of the silicon dioxide is SiO 2 ≥99.9%; in terms of mass fraction, the chemical composition of the industrial alumina is Al 2 O 3 ≥99%; in terms of mass fraction, in the chemical composition of the plate-like corundum, Al 2 O 3 ≥99.6%; in terms of mass fraction, the chemical composition of the active α-alumina is Al 2 O 3 ≥99.8%,Na 2 O≤0.2%.

[0010] Optionally, the sagger further comprises the following raw materials: a binder, wherein the binder is yellow dextrin.

[0011] Optionally, the sagger meets at least one of the following properties: bulk density ≥ 2.46 g / cm 3, apparent porosity ≥ 20.8%, high temperature flexural strength ≥ 5.6MPa, flexural strength retention rate ≥ 54%.

[0012] In a second aspect, the present application provides a method for preparing a sagger according to any one embodiment of the first aspect, the method comprising:

[0013] Kyanite, potassium carbonate, silicon dioxide, industrial alumina and additives are mixed in proportion, and then pressed to obtain a green body;

[0014] The green body is first dried, first calcined and crushed to obtain kyanite-KAlSi 2 O 6 Composite materials;

[0015] The kyanite-KAlSi 2 O 6 The composite material, plate-shaped corundum, active α-alumina and additives are mixed in proportion, and then pressed and formed to obtain a sagger body;

[0016] The sagger blank is subjected to a second drying and a second calcination to obtain a sagger.

[0017] Optionally, the first drying temperature is 100°C-120°C, and the first drying time is 12h-24h; and / or the first calcination temperature is 1200°C-1400°C, and the first calcination time is 6h-8h.

[0018] Optionally, the temperature of the first drying is 100°C-120°C, and the time of the first drying is 12h-24h; and / or the temperature of the first calcination is 1300°C-1500°C, and the time of the first calcination is 3h-5h.

[0019] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0020] The present application provides a sagger for positive electrode materials of lithium-ion batteries. The sagger includes the following raw materials by mass fraction: kyanite: 65%-75%, potassium carbonate: 0.5%-3%, silicon dioxide: 0.5%-2%, industrial alumina: 1%-5%, plate-shaped corundum: 12%-20%, and active α-alumina: 4%-8%. By rationally designing the raw material composition of the sagger, a kyanite-KAlSi 2 O 6 Core-shell structure, KAlSi 2 O 6 Coated on the surface of kyanite particles, it effectively hinders the contact between the positive electrode material and the kyanite in the sagger, avoiding the occurrence of corrosion reaction; at the same time, KAlSi 2 O6 It has good sintering properties and forms a close connection with the surrounding matrix at high temperature, which improves the high-temperature mechanical properties of the sagger. Thereby, the corrosion resistance and high-temperature mechanical properties of the sagger used for lithium-ion battery positive electrode materials are also improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0022] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0023] Figure 1 The present invention is a flow chart of a method for preparing a sagger for positive electrode materials of lithium-ion batteries provided in an embodiment of the present application. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0025] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0026] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.

[0027] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0028] The present application provides a sagger for positive electrode materials of lithium-ion batteries. The sagger comprises the following raw materials, measured by mass fraction: kyanite: 65%-75%, potassium carbonate: 0.5%-3%, silicon dioxide: 0.5%-2%, industrial alumina: 1%-5%, plate-like corundum: 12%-20%, and active α-alumina: 4%-8%.

[0029] In an embodiment of the present application, the content of kyanite is controlled to be 65-75wt%. When it is less than 65%, the content of alumina is too low and the content of silica is too high, which is not conducive to the corrosion resistance of the sagger. When it is greater than 75%, the amount of plate-shaped corundum added is too small, which is not conducive to the high-temperature stability of the sagger. The content of potassium carbonate is controlled to be 0.5-3wt%. When it is less than 0.5%, the content of potassium aluminosilicate prepared is too low, and the ability to improve the corrosion resistance is limited. When it is greater than 3%, the content of potassium aluminosilicate prepared is too high, which is not conducive to the strength of the sagger. The content of silica is controlled to be 0.5-2wt%. When it is less than 0.5%, the content of potassium aluminosilicate prepared is too low, and the ability to improve the corrosion resistance is limited. When it is greater than 2%, the content of The prepared potassium aluminosilicate content is too high, which is not conducive to the strength of the sagger; the content of industrial alumina is controlled to be 1-5wt%, when the content of potassium aluminosilicate is less than 1%, the prepared potassium aluminosilicate content is too low, and the ability to improve the corrosion resistance is limited; when the content of potassium aluminosilicate is greater than 5%, the prepared potassium aluminosilicate content is too high, which is not conducive to the strength of the sagger; the content of plate-like corundum is controlled to be 12-20wt%, when it is less than 12%, the amount of plate-like corundum added is too small, which is not conducive to the high-temperature stability of the sagger, and when it is greater than 20%, the amount of plate-like corundum added is too much, which is not conducive to the thermal shock resistance of the sagger; the content of active α-alumina is controlled to be 4-8wt%, when it is less than 4%, it is not conducive to the sintering performance of the sagger, and when it is greater than 8%, it has little effect on the performance and increases the cost. Exemplarily, the mass fraction of kyanite can be 65%, 67%, 69%, 70%, 72%, 75%, etc., the mass fraction of potassium carbonate can be 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, etc., the mass fraction of silicon dioxide can be 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%, etc., the mass fraction of industrial alumina can be 1%, 2%, 3%, 4%, 5%, etc., the mass fraction of plate corundum can be 12%, 14%, 16%, 18%, 20%, etc., and the mass fraction of activated α-alumina can be 4%, 5%, 6%, 7%, 8%, etc.

[0030] In some embodiments, in terms of mass fraction, the chemical composition of the kyanite is composed of Al 2 O 3 ≥57.0%,SiO 2 ≤39.0%,TiO 2 ≤0.4%,Fe 2 O 3 ≤1.2%, CaO≤0.4%, MgO≤0.3%, K 2 O≤0.2%,Na 2 O≤0.1%.

[0031] In the above embodiment, the selected kyanite has a higher aluminum oxide content and a lower silicon dioxide content, which is beneficial to improving the corrosion resistance of the sagger.

[0032] In some embodiments, the model of the kyanite is D57 kyanite. D57 kyanite has the highest content of aluminum oxide, which is beneficial to improving the corrosion resistance of the sagger.

[0033] In some embodiments, the particle size of the kyanite is 0-1 mm; the particle size of the potassium carbonate is 0-0.044 mm; the particle size of the silicon dioxide is 0-0.044 mm; the particle size of the industrial alumina is 0-0.044 mm; the particle size of the plate-like corundum is 0-0.044 mm; and the particle size of the activated α-alumina is 0-0.005 mm.

[0034] In the above embodiment, the raw material particle size selected for preparing potassium aluminosilicate is relatively small, which is conducive to the full combination between particles and is completely converted into potassium aluminosilicate through solid phase reaction at high temperature.

[0035] In some embodiments, in terms of mass fraction, the chemical composition of potassium carbonate is K 2 CO 3 ≥99.9; in terms of mass fraction, the chemical composition of the silicon dioxide is SiO 2 ≥99.9%; in terms of mass fraction, the chemical composition of the industrial alumina is Al 2 O 3 ≥99%; in terms of mass fraction, in the chemical composition of the plate-like corundum, Al 2 O 3 ≥99.6%; in terms of mass fraction, the chemical composition of the active α-alumina is Al 2 O 3 ≥99.8%,Na 2 O≤0.2%.

[0036] In some embodiments, the sagger further comprises the following raw materials: a binder, which is yellow dextrin, and the added mass of the binder accounts for 3% of the total mass of kyanite, potassium carbonate, silicon dioxide, industrial alumina, plate-shaped corundum, and active α-alumina.

[0037] In the above embodiment, by adding a binder and controlling the amount of the binder, it is ensured that the raw materials can be tightly combined during the process of pressing the green body.

[0038] In some embodiments, the sagger meets at least one of the following properties: bulk density ≥ 2.46 g / cm 3 , apparent porosity ≥ 20.8%, high temperature flexural strength ≥ 5.6MPa, flexural strength retention rate ≥ 54%.

[0039] Figure 1 The present invention is a flow chart of a method for preparing a sagger for positive electrode materials of lithium-ion batteries provided in an embodiment of the present application.

[0040] Based on a general inventive concept, see Figure 1 The present application provides a method for preparing a sagger as described in any one of the above embodiments, the method comprising:

[0041] S1, kyanite, potassium carbonate, silicon dioxide, industrial alumina and additives are mixed in proportion, and then pressed to obtain a green body;

[0042] S2, the green body is first dried, first calcined and crushed to obtain kyanite-KAlSi 2 O 6 Composite materials;

[0043] In some embodiments, the first drying temperature is 100°C-120°C, and the first drying time is 12h-24h; and / or the first calcination temperature is 1200°C-1400°C, and the first calcination time is 6h-8h.

[0044] In the above embodiment, by controlling the parameters of the first drying, the moisture in the green body can be completely removed. By controlling the process parameters of the first calcination, the complete phase transition of potassium aluminosilicate is ensured. Exemplarily, the temperature of the first drying can be 100°C, 105°C, 110°C, 115°C, 120°C, etc., and the time of the first drying can be 12h, 14h, 16h, 18h, 20h, 22h, 24h, etc. The temperature of the first calcination can be 1200°C, 1250°C, 1300°C, 1350°C, 1400°C, etc., and the time of the first calcination can be 6h, 6.5h, 7h, 7.5h, 8h, etc.

[0045] In some embodiments, kyanite-KAlSi 2 O 6 The particle size of the composite material is 0-1 mm.

[0046] S3, the kyanite-KAlSi 2 O 6 The composite material, plate-shaped corundum, active α-alumina and additives are mixed in proportion, and then pressed and formed to obtain a sagger body;

[0047] In some embodiments, the pressing pressure of the sagger blank is 90 MPa-120 MPa.

[0048] In the above embodiment, the pressure of the pressing molding is controlled to ensure that the sagger blank has good formability.

[0049] S4, subjecting the sagger blank to a second drying and a second calcination to obtain a sagger.

[0050] In some embodiments, the first drying temperature is 100°C-120°C, and the first drying time is 12h-24h; and / or the first calcination temperature is 1300°C-1500°C, and the first calcination time is 3h-5h.

[0051] In the above embodiment, by controlling the parameters of the second drying, the moisture in the green body can be completely removed. By controlling the process parameters of the second calcination, the sintering performance is guaranteed to meet the requirements. Exemplarily, the temperature of the first drying can be 100°C, 105°C, 110°C, 115°C, 120°C, etc., and the time of the first drying can be 12h, 14h, 16h, 18h, 20h, 22h, 24h, etc. The temperature of the first calcination can be 1300°C, 1350°C, 1400°C, 1450°C, 1500°C, etc., and the time of the first calcination can be 3h, 3.5h, 4h, 4.5h, 5h, etc.

[0052] The product prepared by the method for preparing a sagger for positive electrode materials of lithium ion batteries is the above-mentioned sagger for positive electrode materials of lithium ion batteries. The raw material composition and performance of the sagger for positive electrode materials of lithium ion batteries prepared by the method for preparing a sagger for positive electrode materials of lithium ion batteries can refer to the above-mentioned embodiment. Since the method for preparing a sagger for positive electrode materials of lithium ion batteries adopts part or all of the technical solutions of the embodiment of the sagger for positive electrode materials of lithium ion batteries, it at least has all the beneficial effects brought by the technical solutions of the embodiment of the sagger for positive electrode materials of lithium ion batteries, which will not be repeated here one by one.

[0053] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.

[0054] Example 1

[0055] (1) According to Table 1, kyanite, potassium carbonate, silicon dioxide and industrial alumina are weighed, and appropriate amounts of yellow dextrin and water are added and mixed evenly, and then molded under a hydraulic press to obtain a green body, wherein the amount of yellow dextrin added accounts for 3% of the total weight of the raw materials.

[0056] Table 1 The raw material formula required for preparing the sagger in Example 1

[0057]

[0058]

[0059] (2) Place the green body in a drying oven at a drying temperature of 110°C for 24 hours.

[0060] (3) The dried green body was placed in an electric furnace and calcined at a temperature of 1300°C for 6 hours to obtain kyanite-KAlSi 2 O 6 Composite materials.

[0061] (4) Prepare kyanite-KAlSi 2 O 6 The composite material is crushed to obtain 1-0 mm particles for later use.

[0062] (5) Weigh kyanite-KAlSi according to Table 1 2 O 6 The composite material, plate-shaped corundum, active alpha-alumina, 3% yellow dextrin accounting for the total weight of the raw materials and water are added and mixed evenly, and then a sagger body is obtained by molding with a hydraulic press, and the molding pressure is 100 MPa.

[0063] (6) The sagger body is sent to a drying kiln for heat treatment at a drying temperature of 110°C and a drying time of 24 hours.

[0064] (7) The heat-treated sagger body is sent into a tunnel kiln and calcined at a high temperature of 1450°C for 3 hours.

[0065] Example 2

[0066] (1) According to Table 2, kyanite, potassium carbonate, silicon dioxide and industrial alumina were weighed, and appropriate amounts of yellow dextrin and water were added and mixed evenly, and then molded under a hydraulic press to obtain a green body, wherein the amount of yellow dextrin added accounted for 3% of the total weight of the raw materials.

[0067] Table 2 The raw material formula required for preparing the sagger in Example 2

[0068]

[0069] (2) Place the green body in a drying oven at a drying temperature of 110°C for 24 hours.

[0070] (3) The dried green body was placed in an electric furnace and calcined at a temperature of 1300°C for 6 hours to obtain kyanite-KAlSi 2 O 6 Composite materials.

[0071] (4) Prepare kyanite-KAlSi 2 O 6 The composite material is crushed to obtain 1-0 mm particles for later use.

[0072] (5) Weigh kyanite-KAlSi according to Table 2 2 O6 The composite material, plate-shaped corundum, active alpha-alumina, 3% yellow dextrin accounting for the total weight of the raw materials and water are added and mixed evenly, and then a sagger body is obtained by molding with a hydraulic press, and the molding pressure is 100 MPa.

[0073] (6) The sagger body is sent to a drying kiln for heat treatment at a drying temperature of 110°C and a drying time of 24 hours.

[0074] (7) The heat-treated sagger body is sent into a tunnel kiln and calcined at a high temperature of 1450°C for 3 hours.

[0075] Example 3

[0076] According to Table 3, kyanite, potassium carbonate, silicon dioxide and industrial alumina were weighed, and appropriate amounts of yellow dextrin and water were added and mixed evenly, and then molded under a hydraulic press to obtain a green body, wherein the amount of yellow dextrin added accounted for 3% of the total weight of the raw materials.

[0077] Table 3 Raw material formula required for preparing sagger in Example 3

[0078]

[0079] (2) Place the green body in a drying oven at a drying temperature of 110°C for 24 hours.

[0080] (3) The dried green body was placed in an electric furnace and calcined at a temperature of 1300°C for 6 hours to obtain kyanite-KAlSi 2 O 6 Composite materials.

[0081] (4) Prepared kyanite-KAlSi 2 O 6 The composite material is crushed to obtain 1-0 mm particles for later use.

[0082] (5) Weigh kyanite-KAlSi according to Table 3 2 O 6 The composite material, plate-shaped corundum, active alpha-alumina, 3% yellow dextrin accounting for the total weight of the raw materials and water are added and mixed evenly, and then a sagger body is obtained by molding with a hydraulic press, and the molding pressure is 100 MPa.

[0083] (6) The sagger body is sent to a drying kiln for heat treatment at a drying temperature of 110°C and a drying time of 24 hours.

[0084] (7) The heat-treated sagger body is sent into a tunnel kiln and calcined at a high temperature of 1450°C for 3 hours.

[0085] Comparative Example 1

[0086] (1) According to Table 4, kyanite, potassium carbonate, silicon dioxide and industrial alumina were weighed, and appropriate amounts of yellow dextrin and water were added and mixed evenly, and then molded under a hydraulic press to obtain a green body, wherein the amount of yellow dextrin added accounted for 3% of the total weight of the raw materials.

[0087] Table 4 Raw material formula required for preparing sagger in comparative example 1

[0088]

[0089] (2) Place the green body in a drying oven at a drying temperature of 110°C for 24 hours.

[0090] (3) The dried green body was placed in an electric furnace and calcined at a temperature of 1300°C for 6 hours to obtain kyanite-KAlSi 2 O 6 Composite materials.

[0091] (4) Prepared kyanite-KAlSi 2 O 6 The composite material is crushed to obtain 1-0 mm particles for later use.

[0092] (5) Weigh kyanite-KAlSi according to Table 3 2 O 6 The composite material, plate-shaped corundum, active alpha-alumina, 3% yellow dextrin accounting for the total weight of the raw materials and water are added and mixed evenly, and then a sagger body is obtained by molding with a hydraulic press, and the molding pressure is 100 MPa.

[0093] (6) The sagger body is sent to a drying kiln for heat treatment at a drying temperature of 110°C and a drying time of 24 hours.

[0094] (7) The heat-treated sagger body is sent into a tunnel kiln and calcined at a high temperature of 1450°C for 3 hours.

[0095] Comparative Example 2

[0096] (1) Weigh the raw materials according to Table 5, add appropriate amount of yellow dextrin and water and mix evenly, then form the sagger body under a hydraulic press, wherein the amount of yellow dextrin added accounts for 3% of the total weight of the raw materials.

[0097] Table 5: Raw material formula required for preparing sagger in comparative example

[0098]

[0099] (2) The sagger body is sent to a drying kiln for heat treatment at a drying temperature of 110°C and a drying time of 24 hours.

[0100] (3) The heat-treated sagger body is sent into a tunnel kiln and calcined at a high temperature of 1450°C for 3 hours.

[0101] Comparative Example 3

[0102] (1) Weigh the raw materials according to Table 6, add appropriate amount of yellow dextrin and water and mix evenly, then form the sagger body under a hydraulic press, wherein the amount of yellow dextrin added accounts for 3% of the total weight of the raw materials.

[0103] Table 6: Raw material formula required for preparing sagger in comparative example

[0104]

[0105] (2) The sagger body is sent to a drying kiln for heat treatment at a drying temperature of 110°C and a drying time of 24 hours.

[0106] (3) The heat-treated sagger body is sent into a tunnel kiln and calcined at a high temperature of 1450°C for 3 hours.

[0107] The following tests were performed on the saggers for lithium ion battery positive electrode materials prepared in Examples 1-3 and Comparative Examples 1-3:

[0108] 1) Bulk density and apparent porosity test: Using Archimedes principle, the bulk density and apparent porosity are tested by the drainage method.

[0109] 2) High temperature flexural strength test: The sagger was kept at 1100°C for 1 hour, and the high temperature flexural strength of the sagger was tested at high temperature using the three-point bending method.

[0110] 3) Thermal shock resistance test: The water cooling method is used for testing. The sagger is quickly placed in a muffle furnace with a temperature of 1100°C and kept warm for 30 minutes. After being taken out, it is quickly placed in room temperature water for cooling. The cooled sagger is placed in a drying oven for drying, and the flexural strength after thermal shock is measured and the flexural strength retention rate is calculated. The flexural strength retention rate of the sagger can represent the quality of its thermal shock resistance.

[0111] 4) Slag resistance test: The static crucible method was used to carry out corrosion resistance test at 1100°C for 20 hours. The results are shown in Table 5:

[0112] Table 5 Performance test results of saggers prepared in Examples 1-3 and Comparative Examples

[0113]

[0114] The results show that compared with the saggers prepared in the comparative example, the corrosion resistance and high temperature strength of the saggers prepared in Examples 1-3 are significantly improved, and the thermal shock resistance does not change much. In addition, compared with the saggers prepared in Comparative Examples 1-3 using kyanite D45, mullite and cordierite as the main raw materials, the saggers prepared in Examples 1-3 using kyanite as the raw material have the advantages of low pollution, low energy consumption and low cost.

[0115] In addition, one or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:

[0116] In the embodiment of the present invention, kyanite-KAlSi 2 O 6 Core-shell structure, KAlSi 2 O 6 Coated on the surface of kyanite, it effectively blocks the contact between lithium ions in the positive electrode material of the lithium battery and the aluminum silicon components in the sagger, avoiding the occurrence of corrosion reactions.

[0117] In the embodiment of the present invention, KAlSi 2 O 6 It has good sintering properties and forms a close connection with the surrounding matrix at high temperatures, thus improving the high-temperature mechanical properties of the sagger.

[0118] In the embodiment of the present invention, kyanite is a natural refractory raw material and can be used without calcination. Using kyanite to prepare saggers can reduce pollution and save energy consumption.

[0119] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A sagger for lithium-ion battery positive electrode material, characterized in that: The sagger comprises the following raw materials by mass fraction: kyanite: 65%-75%, potassium carbonate: 0.5%-3%, silicon dioxide: 0.5%-2%, industrial alumina: 1%-5%, plate-like corundum: 12%-20%, and active α-alumina: 4%-8%.

2. The sagger according to claim 1, characterized in that: Calculated by mass fraction, the chemical composition of the kyanite is as follows: Al2O3≥57.0%, SiO2≤39.0%, TiO2≤0.4%, Fe2O3≤1.2%, CaO≤0.4%, MgO≤0.3%, K2O≤0.2%, and Na2O≤0.1%.

3. The sagger according to claim 2, characterized in that: The model of the kyanite is D57 kyanite.

4. The sagger according to claim 1, characterized in that: The particle size of the kyanite is 0-1mm; the particle size of the potassium carbonate is 0-0.044mm; the particle size of the silicon dioxide is 0-0.044mm; the particle size of the industrial alumina is 0-0.044mm; the particle size of the plate-like corundum is 0-0.044mm; and the particle size of the active α-alumina is 0-0.005mm.

5. The sagger according to claim 4, characterized in that: In terms of mass fraction, in the chemical composition of the potassium carbonate, K2CO3≥99.9%; in terms of mass fraction, in the chemical composition of the silicon dioxide, SiO2≥99.9%; in terms of mass fraction, in the chemical composition of the industrial alumina, Al2O3≥99%; in terms of mass fraction, in the chemical composition of the plate-like corundum, Al2O3≥99.6%; in terms of mass fraction, in the chemical composition of the active α-alumina, Al2O3≥99.8%, Na2O≤0.2%.

6. The sagger according to claim 1, characterized in that: The sagger also includes the following raw materials: a binder, which is yellow dextrin.

7. The sagger according to claim 1, characterized in that: The sagger meets at least one of the following properties: bulk density ≥ 2.46 g / cm 3 , apparent porosity ≥ 20.8%, high temperature flexural strength ≥ 5.6MPa, flexural strength retention rate ≥ 54%.

8. A method for preparing a sagger according to any one of claims 1 to 7, characterized in that: The method comprises: Kyanite, potassium carbonate, silicon dioxide, industrial alumina and additives are mixed in proportion, and then pressed to obtain a green body; The green body is first dried, first calcined and crushed to obtain a kyanite-KAlSi2O6 composite material; The kyanite-KAlSi2O6 composite material, plate-shaped corundum, active α-alumina and additives are mixed in proportion, and then pressed to obtain a sagger blank; The sagger blank is subjected to a second drying and a second calcination to obtain a sagger.

9. The method according to claim 8, characterized in that The temperature of the first drying is 100° C.-120° C., and the time of the first drying is 12 h-24 h; and / or the temperature of the first calcination is 1200° C.-1400° C., and the time of the first calcination is 6 h-8 h.

10. The method according to claim 8, characterized in that The first drying temperature is 100° C.-120° C., and the first drying time is 12 h-24 h; and / or the first calcination temperature is 1300° C.-1500° C., and the first calcination time is 3 h-5 h.

Citation Information

Patent Citations

  • Energy-saving type high-temperature high-thermal shock resistance kiln furnace structural material prepared by using waste fireproof kiln furniture and method for preparing same

    CN101792321A

  • Refractory castable and preparation method thereof

    CN116675544A

  • Ceramics made of zeolite wherein high density leusite and / or porsite are incorporated as main ingredients

    JP1993155657A

  • Flux combination of barium oxide and potassium feldspar for high-strength alumina porcelain electric insulators

    US4332913A

Cited By

  • Container for cathode active materials

    EP4741363A1