High-strength electric porcelain as well as preparation method and application thereof
By adjusting the chemical formula and spraying process of the electric porcelain base glaze and coating, the problems of insufficient surface strength, heat resistance and corrosion resistance of electric porcelain in harsh environments were solved. High-strength electric porcelain was prepared and realized in UHV equipment. good performance.
Patent Information
- Application Number
- CN202410968383.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-18
AI Technical Summary
Existing electroceramics have insufficient surface strength, poor heat resistance, and weak corrosion resistance in harsh environments, which limits their application in UHV equipment.
By adjusting the chemical raw material formula of the base glaze and coating, combined with the atmospheric plasma spraying process, and optimizing the surface roughness of the base glaze body and spraying parameters, a high-strength electric porcelain was prepared, including base glaze and coating, using 50 parts of α-Al2O3, The base glaze of 16 to 20 parts of SiO2, 3 to 7 parts of CaO and other chemical raw materials, and the coating of 50 parts of γ-Al2O3, 25 to 33 parts of Y2O3 and other chemical raw materials ensure excellent bonding between the base glaze and the coating.
The surface strength, heat resistance and corrosion resistance of electric porcelain are significantly improved, allowing it to maintain structural integrity under extreme temperatures and harsh environments, meet the high standard requirements of UHV equipment, and broaden the application scope of electric porcelain in complex environments.
Smart Images

Figure BDA0004952383140000091 
Figure BDA0004952383140000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electric porcelain, and in particular relates to a high-strength electric porcelain and a preparation method and application thereof. Background Art
[0002] The research on UHV insulators is currently focused on improving the comprehensive performance of insulators by adjusting the inorganic raw material formula based on high-aluminum porcelain. However, due to the compatibility issues between chemical raw materials and the complexity of the interaction between multiple raw materials, the formulation research and development process faces great challenges.
[0003] Existing ordinary insulators have many shortcomings, such as insufficient surface strength, poor heat resistance and weak corrosion resistance, which limit their application in harsh environments. In order to overcome these problems, it is particularly important to develop an insulator that has both high strength and good heat resistance and corrosion resistance.
[0004] The present invention proposes a new solution that can significantly improve the surface properties of insulators, while also effectively improving their heat resistance and corrosion resistance. These characteristics enable the insulator products of the present invention to maintain the integrity of their structure and function in extreme temperature changes and harsh corrosive environments, meeting the high standards required of UHV power equipment for insulator materials, thereby broadening the application range of insulators in complex environments. Summary of the invention
[0005] The present invention overcomes at least one of the following problems of insufficient surface strength, poor heat resistance and weak corrosion resistance of the prior art insulators. Therefore, a high-strength insulator and a preparation method and application thereof are provided, wherein the high-strength insulator has high strength and excellent heat resistance and corrosion resistance.
[0006] The present invention solves the above technical problems through the following technical solutions.
[0007] The present invention provides a high-strength electrical porcelain, comprising a base glaze and a coating;
[0008] The base glaze comprises the following chemical raw materials in parts by weight: 50 parts of α-Al2O3, 16-20 parts of SiO2, 3-7 parts of CaO, 1-3 parts of MgO, 2-5 parts of K2O, 0.5-2.8 parts of Na2O, 3-7 parts of ZrO2, and 2-6 parts of TiO2;
[0009] The coating comprises the following chemical raw materials in parts by weight: 50 parts of γ-Al2O3, 25 to 33 parts of Y2O3, 2 to 4 parts of MoSi2 and 7 to 15 parts of α-Si3N4.
[0010] Furthermore, the base glaze contains the following chemical raw materials in parts by weight: 50 parts of α-Al2O3, 17.3 to 19.4 parts of SiO2, 3.3 to 6.5 parts of CaO, 1.58 to 2.7 parts of MgO, 2.45 to 4.56 parts of K2O, 0.62 to 2.31 parts of Na2O, 3.4 to 6.6 parts of ZrO2, and 2.7 to 5.6 parts of TiO2.
[0011] Furthermore, the coating comprises the following chemical raw materials in parts by weight: 50 parts of γ-Al2O3, 26 to 31 parts of Y2O3, 2.2 to 3.8 parts of MoSi2 and 7.9 to 13.5 parts of α-Si3N4.
[0012] Among the chemical raw materials for the coating in the present invention, γ-Al2O3 is selected due to its good compatibility with the base glaze and excellent dispersion and adhesion. On the other hand, γ-Al2O3 can be stably converted into α-Al2O3 with better thermal stability at high temperatures; Y2O3 has good chemical inertness, corrosion resistance and wear resistance, and MoSi2 has excellent high-temperature oxidation resistance. The addition of the two can enable the electrical porcelain to be used in extreme environments, but the thermal expansion coefficients of the two are high and they are usually not directly applied to the ceramic matrix; α-Si3N4 has a lower thermal expansion coefficient, which not only helps to reduce the thermal expansion of the overall material, but also can further enhance the overall performance of the material by controlling the growth and refinement of its grains.
[0013] In the present invention, the particle size of the α-Al2O3 (CAS No.: 1344-28-1) is 0.2-0.4 μm.
[0014] In the present invention, the particle size of the γ-Al2O3 is ≤50nm.
[0015] In the present invention, the particle size of the α-Si3N4 (CAS No.: 12033-89-5) is 10 to 50 nm, for example, 20 nm.
[0016] In the present invention, the thickness of the base glaze is 0.3-0.45 mm, preferably 0.35-0.4 mm.
[0017] In the present invention, the thickness of the coating is 0.2-0.3 mm, preferably 0.22-0.26 mm.
[0018] In the present invention, the thermal expansion coefficient of the base glaze is 5.05 to 5.18×10 -6 / K, preferably 5.11~5.13×10 -6 / K.
[0019] In the present invention, the thermal expansion coefficient of the coating is 5.21 to 5.28×10 -6 / K.
[0020] In the present invention, the thermal shock resistance temperature of the high-strength electrical porcelain is 250-270°C.
[0021] In the present invention, the bending strength of the high-strength electrical porcelain is 485-497Mpa.
[0022] The present invention also provides a method for preparing the above-mentioned high-strength electrical porcelain, comprising the following steps:
[0023] S1. Preparation of base glaze slurry: After the chemical raw materials of the base glaze are prepared according to the above formula, they are ball-milled, sieved and blended to obtain the base glaze slurry;
[0024] S2. Base glaze treatment: the body is dipped in base glaze slurry and then sintered to obtain a base glaze body;
[0025] The sintering temperature is set at 1050-1150°C, preferably 1070-1130°C;
[0026] The surface roughness Ra of the base glaze body is 28-43 μm;
[0027] S3. Preparation of coating powder: The chemical raw materials of the coating are prepared according to the above formula, and then ground and sieved to obtain coating powder;
[0028] S4. Coating treatment: The coating powder is sprayed on the surface of the base glaze body by atmospheric plasma to obtain high-strength electrical porcelain.
[0029] In S1, the mesh size of the sieving is 250-300 meshes.
[0030] In S1, the specific gravity of the glaze slurry is 1.45-1.47 g / cm 3 .
[0031] In S2, the base glaze blank also needs to be cleaned, polished and sandblasted to make the surface roughness Ra of the base glaze blank 28 to 43 μm, preferably 30 to 43 μm. The surface roughness of the base glaze blank has a significant effect on the adhesion and growth of the coating. If the base glaze surface is too smooth, the bonding force between the coating and the base glaze will be weakened, resulting in weak adhesion of the coating; on the contrary, if the surface roughness is too large, the growth of the coating may become uneven, affecting the overall quality and performance of the coating.
[0032] In S2, the heating rate of the sintering is 15-30°C / min.
[0033] In S2, the sintering heat preservation time is 6 to 10 hours.
[0034] In S3, the mesh size of the sieving is 500-800 meshes.
[0035] In S4, the argon gas flow rate of the atmospheric plasma spraying is 30 to 40 L min -1 .
[0036] In S4, the hydrogen flow rate of the atmospheric plasma spraying is 3 to 7 L min -1 .
[0037] In S4, the set current value of the atmospheric plasma spraying is 350-380A. If the current value is set too high, the coating may become too dense, resulting in reduced porosity, which may increase the brittleness of the coating and reduce its toughness. If the current value is too low, the porosity of the coating may increase, affecting the density and overall strength of the coating.
[0038] In S4, the atmospheric plasma spraying is followed by heat preservation at 1100-1200° C. for 15-24 hours. If the heat preservation temperature is too high, the coating will grow fast and local stress concentration may increase pores and further induce cracks.
[0039] The present invention also provides the use of the high-strength electrical porcelain as described above in high-voltage transmission lines, substations and converter stations, aerospace, chemical and petroleum industries or marine and offshore facilities.
[0040] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] 1. The present invention ensures excellent bonding between the base glaze and the coating by adjusting the formula of the base glaze and the coating and exploring the reasonable range of the surface roughness of the base glaze blank. This optimization not only improves the surface quality of the electrical porcelain, but also enhances its overall performance.
[0043] 2. The present invention explores the influence of atmospheric plasma spraying process on coating growth and successfully prepares an electric porcelain with high strength, excellent thermal shock resistance and salt spray corrosion resistance by precisely controlling the spraying parameters. DETAILED DESCRIPTION
[0044] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and carefully in combination with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.
[0045] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0046] The "range" disclosed in the present invention is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of a particular range. The range defined in this way can be inclusive or exclusive of end values, and can be combined arbitrarily, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60-120 and 80-110 is listed for a specific parameter, it is understood that the range of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present invention, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" represents that all real numbers between "0-5" have been fully listed herein, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0047] If not otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form a new technical solution.
[0048] Unless otherwise specified, all technical features and optional technical features of the present invention can be combined with each other to form a new technical solution.
[0049] If not otherwise specified, all steps of the present invention may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0050] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0051] If not specifically stated, in the present invention, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0052] Detailed information of the chemical raw materials used in the following examples and comparative examples is shown in Table 1;
[0053] Table 1
[0054] Chemical raw materials CAS Number Manufacturer, model or specification Specification <![CDATA[α-Si3N4]]> 12033-89-5 Guangzhou Wengjiang Particle size 20nm <![CDATA[α-Al2O3]]> 1344-28-1 Beijing Puxitang Particle size 0.2~0.4μm <![CDATA[γ-Al2O3]]> 1344-28-1 Beijing Puxitang Particle size 20nm
[0055] Example 1
[0056] 1. The high-strength electrical porcelain of this embodiment includes a base glaze and a coating:
[0057] The base glaze is composed of the following chemical raw materials in parts by weight: 50 parts of α-Al2O3, 17.8 parts of SiO2, 4.7 parts of CaO, 1.58 parts of MgO, 4.56 parts of K2O, 0.62 parts of Na2O, 5.22 parts of ZrO2, and 3.9 parts of TiO2.
[0058] The coating is composed of the following chemical raw materials by weight: 50 parts of γ-Al2O3, 27.4 parts of Y2O3, 2.6 parts of MoSi2 and 10.1 parts of α-Si3N4.
[0059] The thickness of the base glaze is 0.37mm and the coating thickness is 0.25mm.
[0060] 2. The preparation method of the high-strength electrical porcelain of this embodiment is as follows:
[0061] S1. Preparation of base glaze slurry: After the chemical raw materials of base glaze are prepared according to the above formula, they are ball-milled, sieved through a 250-mesh sieve and mixed to obtain base glaze slurry. The specific gravity of the glaze slurry is 1.46 g / cm 3 ;
[0062] S2. Base glaze treatment: the body is dipped in base glaze slurry and then sintered to obtain a base glaze body;
[0063] The set sintering temperature is 1100° C., the sintering heating rate is 15° C. / min, and the temperature is heated to 1100° C. and then kept at that temperature for 8 hours.
[0064] The base glaze body was cleaned, polished and sandblasted to a surface roughness Ra of 34 μm;
[0065] S3. Preparation of coating powder: The chemical raw materials of the coating are prepared according to the above formula, and then ground and sieved through a 600-mesh sieve to obtain a coating powder;
[0066] S4. Coating treatment: The coating powder is sprayed on the surface of the base glaze blank by atmospheric plasma spraying, with an argon flow rate of 35L·min -1 , hydrogen flow rate is 5L·min -1 , set the current value to 375A, and keep warm at 1100℃ for 20h after spraying; high-strength electrical porcelain can be obtained.
[0067] Example 2
[0068] The difference between this embodiment and embodiment 1 is that:
[0069] 1. The high-strength electrical porcelain of this embodiment includes a base glaze and a coating:
[0070] The base glaze is composed of the following chemical raw materials in parts by weight: 50 parts of α-Al2O3, 19.4 parts of SiO2, 3.3 parts of CaO, 2.3 parts of MgO, 2.58 parts of K2O, 2.3 parts of Na2O, 6.1 parts of ZrO2, and 2.7 parts of TiO2.
[0071] The coating is composed of the following chemical raw materials by weight: 50 parts of γ-Al2O3, 29 parts of Y2O3, 3.3 parts of MoSi2 and 13.5 parts of α-Si3N4.
[0072] The thickness of the base glaze is 0.35mm and the coating thickness is 0.22mm.
[0073] Example 3
[0074] The difference between this embodiment and embodiment 1 is that:
[0075] 2. The preparation method of the high-strength electrical porcelain of this embodiment is as follows:
[0076] In S2, the base glaze body is cleaned, polished and sandblasted to have a surface roughness Ra of 30 μm.
[0077] In S4, the set current value of atmospheric plasma spraying is 380A, and the atmospheric plasma spraying is followed by keeping at 1150°C for 18h.
[0078] Example 4
[0079] The difference between this embodiment and embodiment 1 is that:
[0080] 2. The preparation method of the high-strength electrical porcelain of this embodiment is as follows:
[0081] In S2, the base glaze body is cleaned, polished and sandblasted to have a surface roughness Ra of 43 μm.
[0082] In S4, the set current value of the atmospheric plasma spraying is 350A, and the atmospheric plasma spraying is followed by keeping at 1100°C for 24h.
[0083] Comparative Example 1
[0084] The difference between this comparative example and Example 1 is:
[0085] 1. The high-strength electrical porcelain of this comparative example includes a base glaze and a coating:
[0086] The coating is composed of the following chemical raw materials by weight: 50 parts of γ-Al2O3, 30.5 parts of Y2O3, 9.7 parts of MoSi2 and 6.4 parts of α-Si3N4.
[0087] The high-strength electrical porcelain obtained in this comparative example has cracks and bulges on its surface in many places.
[0088] Comparative Example 2
[0089] The difference between this comparative example and Example 1 is:
[0090] 1. The high-strength electrical porcelain of this comparative example includes a base glaze and a coating:
[0091] The coating is composed of the following chemical raw materials by weight: 50 parts of γ-Al2O3, 26 parts of Y2O3, 0 parts of MoSi2 and 9.7 parts of α-Si3N4.
[0092] The surface of the high-strength electric porcelain prepared in this comparative example is uneven, showing multiple concave and convex shapes.
[0093] Comparative Example 3
[0094] The difference between this comparative example and Example 1 is:
[0095] 2. The preparation method of the high-strength electrical porcelain of this embodiment is as follows:
[0096] In S2, the surface roughness Ra of the ground glaze body was 25 μm.
[0097] The high-strength insulator obtained in this comparative example has slight bulging on its surface.
[0098] Comparative Example 4
[0099] The difference between this embodiment and embodiment 1 is that:
[0100] 2. The preparation method of the high-strength electrical porcelain of this embodiment is as follows:
[0101] In S4, the set current value of the atmospheric plasma spraying is 300A, and the atmospheric plasma spraying is followed by keeping the temperature at 1300°C for 10 hours.
[0102] The high-strength electric porcelain obtained in this comparative example has a small amount of relatively wide cracks (width between 0.08 and 0.17 mm) on its surface.
[0103] Effect Example
[0104] The above embodiments and comparative examples were tested for performance, see Table 2.
[0105] Thermal stability test method: refer to GB / T 3298-2022 thermal shock resistance test method for daily-use ceramics. According to the national standard test procedure, the temperature is usually gradually increased at intervals of 20°C. In order to improve the test accuracy, the temperature is actually gradually increased at intervals of 10°C. The thermal shock resistance temperature in the table below refers to the thermal shock resistance temperature before cracks appear.
[0106] Thermal expansion coefficient test method: refer to GB / T 3810.8-2016 Ceramic Tile Test Method Part 8: Determination of Linear Thermal Expansion, and test the surface of the base glaze body obtained by S2 and the high-strength electrical porcelain obtained by S4 after peeling.
[0107] Bending strength determination method: GB / T 6569 Fine ceramics bending strength test method, three-point bending method.
[0108] Salt spray resistance time test method: refer to GB / T 10125-2021 artificial atmosphere corrosion test salt spray test (neutral salt spray test), test time 800h.
[0109] Table 2
[0110]
[0111]
[0112] As can be seen from Table 2, the coating of Comparative Example 1 contains a large amount of MoSi2, but a small amount of α-Si3N4. The large thermal expansion coefficient of the coating will cause compressive stress in the coating, which will lead to poor apparent quality of the insulator, uneven surface, multiple cracks and bulges, and obvious peeling on the surface after the salt spray test. MoSi2 is not added to the coating of Comparative Example 2, so the corrosion resistance of the insulator is poor and the surface is seriously powdered. The surface roughness of the base glaze blank of Comparative Example 3 is small, the bonding between the coating and the base glaze is not good, and slight bulges appear on the surface of the high-strength insulator. After the salt spray test, there are many surface cracks and bulges. The atmospheric ion spraying current value of Comparative Example 4 is too small and the insulation temperature is high. There are many pores in the coating and the coating grows too fast, resulting in local stress concentration, which further induces cracks.
[0113] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods. The specific embodiments described above further describe the purpose, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high-strength electrical porcelain, characterized in that: Includes base glaze and coating; The base glaze comprises the following chemical raw materials in parts by weight: 50 parts of α-Al2O3, 16-20 parts of SiO2, 3-7 parts of CaO, 1-3 parts of MgO, 2-5 parts of K2O, 0.5-2.8 parts of Na2O, 3-7 parts of ZrO2, and 2-6 parts of TiO2; The coating comprises the following chemical raw materials in parts by weight: 50 parts of γ-Al2O3, 25 to 33 parts of Y2O3, 2 to 4 parts of MoSi2 and 7 to 15 parts of α-Si3N4.
2. The high-strength electrical porcelain according to claim 1, characterized in that: Satisfy at least one of the following conditions (1) to (2): (1) The base glaze comprises the following chemical raw materials in parts by weight: 50 parts of α-Al2O3, 17.3-19.4 parts of SiO2, 3.3-6.5 parts of CaO, 1.58-2.7 parts of MgO, 2.45-4.56 parts of K2O, 0.62-2.31 parts of Na2O, 3.4-6.6 parts of ZrO2, and 2.7-5.6 parts of TiO2; (2) The coating comprises the following chemical raw materials in parts by weight: 50 parts of γ-Al2O3, 26 to 31 parts of Y2O3, 2.2 to 3.8 parts of MoSi2 and 7.9 to 13.5 parts of α-Si3N4.
3. The high-strength electrical porcelain according to claim 1, characterized in that: The chemical raw material satisfies at least one of the following conditions (1) to (3); (1) The particle size of the α-Al2O3 is 0.2 to 0.4 μm; (2) The particle size of the γ-Al2O3 is ≤50nm; (3) The particle size of the α-Si3N4 is 10 to 50 nm.
4. The high-strength electrical porcelain according to claim 1, characterized in that: Satisfy at least one of the following conditions (1) to (2): (1) The thickness of the base glaze is 0.30 to 0.45 mm; (2) The thickness of the coating is 0.2 to 0.3 mm.
5. The high-strength electrical porcelain according to claim 1, characterized in that: Satisfy at least one of the following conditions (1) to (2): (1) The thermal expansion coefficient of the base glaze is 5.05 to 5.18 × 10 -6 / K; (2) The thermal expansion coefficient of the coating is 5.21 to 5.28 × 10 -6 / K.
6. The high-strength electric porcelain according to claim 1, characterized in that: Satisfy at least one of the following conditions (1) to (2): (1) The thermal shock resistance temperature of the high-strength electric porcelain is 250-270°C; (2) The flexural strength of the high-strength electrical porcelain is 485-497 MPa.
7. The method for preparing high-strength electrical porcelain according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. Preparation of base glaze slurry: After the chemical raw materials of the base glaze are prepared according to the above formula, they are ball-milled, sieved and blended to obtain the base glaze slurry; S2. Base glaze treatment: the body is dipped in base glaze slurry and then sintered to obtain a base glaze body; The sintering temperature is set at 1050-1150°C; The surface roughness Ra of the base glaze body is 28-43 μm; S3. Preparation of coating powder: The chemical raw materials of the coating are prepared according to the above formula, and then ground and sieved to obtain coating powder; S4. Coating treatment: The coating powder is sprayed on the surface of the base glaze body by atmospheric plasma to obtain high-strength electrical porcelain.
8. The method for preparing high-strength electrical porcelain according to claim 7, characterized in that: Satisfy at least one of the following conditions (1) to (5): (1) In S1, the mesh size of the sieving is 250-300 mesh; (2) In S1, the specific gravity of the glaze slurry is 1.45-1.47 g / cm 3 ; (3) In S2, the heating rate of the sintering is 15 to 30°C / min; (4) In S2, the sintering holding time is 6 to 10 hours; (5) In S3, the mesh size of the sieving is 500 to 800 meshes.
9. The method for preparing high-strength electrical porcelain according to claim 7, characterized in that: The atmospheric plasma spraying satisfies at least one of the following conditions (1) to (4): (1) The argon gas flow rate of the atmospheric plasma spraying is 30 to 40 L min -1 ; (2) The hydrogen flow rate of the atmospheric plasma spraying is 3 to 7 L min -1 ; (3) The set current value of the atmospheric plasma spraying is 350-380A; (4) After the atmospheric plasma spraying, the material is kept at 1100-1200° C. for 15-24 hours.
10. Use of the high-strength insulators as claimed in claims 1 to 6 in high-voltage transmission lines, transformer substations and converter stations, aerospace, chemical and petroleum industries or marine and offshore facilities.
Citation Information
Patent Citations
Ceramic tile ground coat, ceramic tile and preparation method of ceramic tile ground coat
CN115974411A
Method for joining
CN1466557A
Heattresistant covering material
JP1977043825A
Ceramic panel and its production
JP1997020578A
Aluminium oxide coated body and method for the production thereof
WO2011020739A1