Green water-based emulsion with high activity, zero residue and excellent anti-yellowing performance and preparation method thereof

By introducing and modifying rod-shaped metal oxide nanoparticles, the formaldehyde released by the initiator after catalysis is oxidized into harmless substances, solving the problems of monomer residue and yellowing in aqueous emulsions, and achieving high activity, zero residue and anti-yellowing. Green water-based emulsion preparation improves product performance and environmental friendliness.

CN118755013AInactive Publication Date: 2024-10-11ZHEJIANG SATELLITE PETRO CHEM CO LTD +1

Patent Information

Application Number
CN202410828642.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing water-based emulsion preparation technology, unreacted monomer residue and yellowing problems are difficult to effectively solve, affecting product performance and environmental safety.

Method used

Rod-shaped metal oxide nanoparticles are introduced and modified, and their metal d orbital Lewis acid sites are used to catalyze the formaldehyde released by the initiator to oxidize to carbon dioxide and water to increase the polymerization rate, reduce residues, and avoid yellowing.

Benefits of technology

A highly active, zero-residue, anti-yellowing green water-based emulsion has been achieved, which improves the polymerization rate and product performance, reduces formaldehyde residue, and improves environmental friendliness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755013A_ABST
    Figure CN118755013A_ABST
Patent Text Reader

Abstract

The invention provides a green water-based emulsion with high activity, zero residue and excellent yellowing resistance and a preparation method thereof, and relates to the field of green environment-friendly water-based emulsions. The water-based emulsion is a composite emulsion of rod-like metal oxide nanoparticles prepared by emulsion polymerization and a vinyl monomer. The invention overcomes the defects in the prior art, provides a green and environment-friendly water-based emulsion, and introduces rod-like metal oxide nanoparticles to oxidize formaldehyde released by the post-initiator sodium formaldehyde sulfoxylate into formic acid, so that the formic acid is decomposed into carbon dioxide and water along with temperature rise. The comprehensive performance of the waterborne emulsion in the aspects of accelerating the polymerization rate, reducing the yellowing of a latex film, reducing residual monomers, being free of formaldehyde and the like is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aqueous emulsion preparation, and in particular to a green aqueous emulsion with high activity, zero residue and excellent anti-yellowing performance and a preparation method thereof. Background Art

[0002] Aqueous emulsions are made by emulsion polymerization of vinyl monomers. Water-based emulsion polymers (resins) can be made by adding an emulsifier (made by emulsion polymerization) or monomers containing hydrophilic groups and directly using free radical emulsion polymerization.

[0003] In recent years, due to the country's restrictions on VOC, water-based emulsions have become a research hotspot in the adhesive, coating and ink industries because of their excellent corrosion resistance, weather resistance, water resistance, alkali resistance, good film-forming properties, good color retention, no pollution to the environment, and safe use. However, the monomers cannot be 100% converted in the production of polymer emulsions, and it is inevitable that there are certain unreacted monomers in the emulsion. Commonly used monomers are generally compounds containing unsaturated double bonds C=C, such as vinyl chloride, styrene, vinyl acetate, acrylic acid and its ester compounds. These compounds have adverse effects on the environment, and most of them have strong irritating odors and varying degrees of toxicity, which will damage the health of users, such as causing skin allergies, breathing difficulties, headaches, etc. In addition, the residue of unreacted monomers will affect the final use performance of polymer products, such as mechanical properties and chemical resistance. Lung CY et al. (Minimization of the inevitable residual monomer in denturebase acrylic. Dent Mater. 2005, 21 (12): 1119-1128) reported a method for removing methyl methacrylate (MMA) monomer from polymethyl methacrylate (PMMA). The residual MMA monomer content was studied at treatment temperatures of 95°C and 100°C and treatment times of 5h to 192h. It was found that the MMA content could be reduced to between 0.07% and 0.25%. Although the temperature increase method is simple and effective and does not require the addition of other chemicals, it is time-consuming, energy-consuming and inefficient, and has not been widely used. The method that is used more commercially is the post-polymerization method, which uses a redox initiation system with relatively mild reaction conditions. A typical redox system is composed of an oxidant such as persulfate, hydroperoxide, etc. and a reducing agent such as ascorbic acid, sodium formaldehyde sulfoxylate, sodium pyrosulfite, etc. However, ascorbic acid will be oxidized into yellowish 2,3-diketogulonic acid, which makes the final emulsion yellow. Although sodium formaldehyde sulfoxylate has obvious effect in reducing residual units, it is gradually banned from use because it produces formaldehyde. Sodium metabisulfite will produce irritating SO2 when heated. If the human body ingests excessive sulfur dioxide, it is easy to cause allergies, which may cause symptoms such as difficulty breathing, diarrhea, vomiting, and may also cause varying degrees of damage to the brain and other tissues.

[0004] The post-polymerization method in the water-based emulsion industry widely uses hydrogen peroxide / sodium formaldehyde sulfoxylate as an initiator to eliminate residual forms, but formaldehyde is very harmful and the overall performance of the emulsion cannot be balanced. Therefore, it is crucial to develop a new type of green and environmentally friendly water-based emulsion to improve the overall performance of the emulsion. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a green aqueous emulsion with high activity, zero residue and excellent anti-yellowing performance and a preparation method thereof, wherein rod-shaped metal oxide nanoparticles are introduced and their surfaces are modified, and in the post-polymerization process, oxygen vacancies at the Lewis acid sites of the metal d orbital catalytically oxidize the formaldehyde released by the post-initiator sodium formaldehyde sulfoxylate into formic acid, which is then decomposed into carbon dioxide and water as the temperature rises, so that the comprehensive performance of the aqueous emulsion in terms of accelerating the polymerization rate, reducing the yellowing of the latex film, reducing residual monomers and eliminating formaldehyde is greatly improved.

[0006] To achieve the above objectives, the technical solution of the present invention is implemented through the following technical solutions:

[0007] A green water-based emulsion with high activity, zero residue and excellent anti-yellowing performance is a composite latex formed by hybridization of silane-modified rod-shaped metal oxide nanoparticles and vinyl monomers through emulsion polymerization.

[0008] Preferably, the rod-shaped metal oxide nanoparticles in the silane-modified rod-shaped metal oxide nanoparticles are at least one of MnO2, SiO2, CeO2, TiO2, CdO, La2O3, and NiO, and the size of the rod-shaped metal oxide nanoparticles is 5-15 nm in diameter and 15-50 nm in length.

[0009] Preferably, the silane in the silane-modified rod-shaped metal oxide nanoparticles is at least one of methacrylic acid-modified silicone oil, γ-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane, vinyl-tri(2-methoxyethoxy)silane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and γ-methacryloxypropyltrimethoxysilane.

[0010] Preferably, the vinyl monomer is at least two of acrylic acid and acrylic acid esters, methacrylic acid and methacrylic acid esters, hydroxy acrylate, hydroxy methacrylate, styrene, vinyl acetate, acrylonitrile, and olefinically terminated fluorosilicone monomers.

[0011] The preparation method of the green aqueous emulsion comprises the following steps:

[0012] (1) Preparation of rod-shaped metal oxide nanoparticles: dissolving a metal compound in a solvent, adding an acid or a base and transferring to an autoclave, heat treating at 90-180° C. for 5-24 hours, then filtering and washing the obtained mixture, drying at 50-120° C. for 10-36 hours, and then maintaining at 350-600° C. for 2-6 hours, thereby obtaining rod-shaped metal oxide nanoparticles;

[0013] (2) Surface modification with silane: The rod-shaped metal oxide nanoparticles and silane are dispersed in anhydrous ethanol and stirred in a constant temperature water bath at 60-120° C. for 0.5-3 hours, then washed with deionized water and filtered, and the solid part is dried in a vacuum drying oven for 12-48 hours to obtain silane-modified rod-shaped metal oxide nanoparticles;

[0014] (3) Preparation of composite emulsion: deionized water and a first initiator are used as a primer, and silane-modified rod-shaped metal oxide nanoparticles, a second initiator, deionized water and a vinyl monomer are mixed and sheared at high speed to obtain a pre-emulsion. After the primer becomes clear and transparent, the pre-emulsion is added dropwise in a semi-continuous manner for 4-6 hours. After the addition is completed, a rear initiator is added and the mixture is kept warm for 1-2 hours to obtain an aqueous emulsion, and the mass ratio of the primer to the pre-emulsion is 0.5-2:1.5-6.

[0015] Preferably, the metal compound in step (1) is at least one of KMnO4, tetraethyl orthosilicate, Ce(NO3)3, tetrabutyl titanate, Cd(CH3COO)2, La(OH)3, and NiSO4.

[0016] Preferably, the raw materials in the primer solution of step (3) are calculated by weight as follows: 10-50 parts of deionized water, 0.01-0.08 parts of the first initiator, and the first initiator is any one of ammonium persulfate, potassium persulfate, azobisisobutyronitrile or azobiscyanovaleric acid.

[0017] Preferably, the raw materials in the pre-emulsion of step (3) are calculated by weight as follows: 12-35 parts of vinyl monomer, 1.5-32 parts of rod-shaped metal oxide nanoparticles, 0.03-0.5 parts of second initiator, and 20-100 parts of deionized water, and the second initiator is at least one of a combination of hydrogen peroxide and ascorbic acid, hydrogen peroxide and sodium formaldehyde sulfoxylate, and hydrogen peroxide and sodium metabisulfite.

[0018] The present invention provides a green water-based emulsion with high activity, zero residue and excellent anti-yellowing performance, which has the following advantages over the prior art:

[0019] (1) The composite emulsion prepared by emulsion polymerization of the rod-shaped metal oxide nanoparticles prepared by the present invention and the vinyl monomer has a dumbbell-shaped structure. The rod-shaped metal oxide nanoparticles introduced have a small particle size (<50 nm) and a large specific surface area. The oxygen vacancies in the metal d-orbital Lewis acid sites catalyze the oxidation of formaldehyde released by the post-initiator sodium formaldehyde sulfoxylate into green carbon dioxide and water.

[0020] (2) The metal oxide nanoparticles prepared by the present invention have a rod-like morphology with higher oxygen vacancy density than spherical ones, and have higher catalytic oxidation activity, and can rapidly oxidize and decompose formaldehyde;

[0021] (3) The present invention modifies the surface of rod-shaped metal oxide nanoparticles by using silane, thereby increasing the dispersibility and polymerizability of the inorganic particles in water, avoiding particle agglomeration, enlargement and sedimentation, and improving the compatibility between the polymer and the inorganic substance to obtain a stable organic-inorganic composite emulsion. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 TEM image of rod-shaped MnO2 nanoparticles prepared in Example 1 of the present invention;

[0023] Figure 2 This is a TEM image of the dumbbell-shaped structure of the MnO2-polyacrylate composite latex latex particles prepared in Example 1 of the present invention. The dumbbell-shaped structure is obtained by copolymerization of MnO2 nanoparticles and acrylate monomers;

[0024] Figure 3 The XPS spectrum of the rod-shaped MnO2 nanoparticles modified with vinyl-tri(2-methoxyethoxy)silane prepared in Example 1 of the present invention shows the presence of C, O, Si, and Mn elements, indicating that the rod-shaped MnO2 nanoparticles have been successfully modified. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Embodiment 1:

[0027] Preparation of composite emulsion:

[0028] 1. Preparation of rod-shaped MnO2 nanoparticles:

[0029] KMnO4 was dissolved in hydrochloric acid and transferred to an autoclave, heat treated at 150°C for 14 hours, and then the obtained mixture was filtered, washed, dried at 110°C for 17 hours, and then kept at 400°C for 5 hours to obtain rod-shaped MnO2 nanoparticles;

[0030] 2. Surface modification of vinyl-tri(2-methoxyethoxy)silane:

[0031] Rod-shaped MnO2 nanoparticles and KH550 were dispersed in anhydrous ethanol and stirred in a constant temperature water bath at 65°C for 1.5 hours, then washed with deionized water and filtered, and the solid part was dried in a vacuum drying oven for 24 hours to obtain silane-modified rod-shaped MnO2 nanoparticles.

[0032] 3. Preparation of composite emulsion:

[0033] Deionized water and initiator APS are used as primers, and modified rod-shaped MnO2 nanoparticles, initiator APS, deionized water, methyl methacrylate (MMA) and butyl acrylate (BA) are mixed in a mass ratio of 1:1 and sheared at high speed to obtain a pre-emulsion. After the primer becomes clear and transparent, the pre-emulsion is added dropwise in a semi-continuous manner for 4 hours. After the addition is completed, the initiator tert-butyl peroxide and sodium formaldehyde sulfoxylate (mass percentage 4:1) are added and kept warm for another hour. The mass percentage of the primer and the pre-emulsion is 0.8:2 to obtain a composite emulsion.

[0034] Embodiment 2:

[0035] Preparation of composite emulsion:

[0036] 1. Preparation of rod-shaped TiO2 nanoparticles:

[0037] 10 mL C 16 H 36 O4Ti (tetrabutyl titanate) and 100mL oleic acid were added to a conical flask, and the mixture was vigorously stirred under magnetic stirring at room temperature for 1h. 4mL dodecylamine was injected into the conical flask with a syringe (1mL / min), and then vigorously stirred at room temperature for 24h to ensure that the components in the solution were evenly mixed. The prepared solution was transferred into a high-pressure reactor (Berghof BHL-800), and the reactor was quickly heated to 280℃. After keeping the temperature for 24h, the heating was stopped and the mixture was naturally cooled to room temperature to obtain rod-shaped TiO2 nanoparticles.

[0038] 2. Surface modification of γ-methacryloxypropyltrimethoxysilane (silane coupling agent KH570) silane;

[0039] The rod-shaped TiO2 nanoparticles and KH570 were dispersed in anhydrous ethanol and stirred in a constant temperature water bath at 125°C for 2.5 hours, then washed with deionized water and filtered, and the solid part was dried in a vacuum drying oven for 36 hours to obtain silane-modified rod-shaped TiO2 nanoparticles.

[0040] 3. Preparation of composite emulsion:

[0041] Deionized water and initiator KPS are used as primers, and modified rod-shaped TiO2 nanoparticles, initiator KPS, deionized water, styrene (St), and BA are mixed in a mass ratio of 1:1 and sheared at high speed to obtain a pre-emulsion. After the primer becomes clear and transparent, the pre-emulsion is added dropwise in a semi-continuous manner for 3.5 hours. After the addition is completed, the post-initiator tert-butyl peroxide and sodium formaldehyde sulfoxylate (mass percentage 4:1) are added and kept warm for another 1.5 hours. The mass percentage of the primer and the pre-emulsion is 0.7:1.9 to obtain a composite emulsion.

[0042] Embodiment 3:

[0043] Preparation of composite emulsion:

[0044] 1. Preparation of rod-shaped SiO2 nanoparticles:

[0045] Under ammonia conditions (pH = 9.5), using hexadecyltrimethylammonium bromide as a template, tetraethyl orthosilicate as a silicon source, and peregal Os-25 as an additive, monodisperse short rod-shaped nano-SiO2 particles with an axial size of about 30nm and a radial size in the range of 10-15nm were prepared;

[0046] 2. Surface modification of γ-aminopropyltriethoxysilane (silane coupling agent KH550) silane:

[0047] The rod-shaped SiO2 nanoparticles and vinyl-tri(2-methoxyethoxy)silane were dispersed in anhydrous ethanol and stirred in a constant temperature water bath at 95°C for 2 hours, then washed with deionized water and filtered, and the solid part was dried in a vacuum drying oven for 30 hours to obtain silane-modified rod-shaped SiO2 nanoparticles.

[0048] 3. Preparation of composite emulsion:

[0049] Deionized water and initiator ACVA are used as primers, and modified rod-shaped SiO2 nanoparticles, initiator ACVA, deionized water, vinyl acetate (EVA), and isooctyl hydroxymethylacrylate (OEHMA) are mixed in a mass ratio of 1:1 and sheared at high speed to obtain a pre-emulsion. After the primer becomes clear and transparent, the pre-emulsion is added dropwise in a semi-continuous manner for 3 hours. After the addition is completed, the post-initiator tert-butyl peroxide and sodium formaldehyde sulfoxylate (mass percentage 4:1) are added and kept warm for another 1.5 hours. The mass percentage of the primer and the pre-emulsion is 0.8:1.9 to obtain a composite emulsion.

[0050] Embodiment 4:

[0051] Preparation of composite emulsion:

[0052] (1) Preparation of rod-shaped CeO2 nanoparticles:

[0053] Ce(NO3)3 is dispersed in a sodium hydroxide aqueous solution, stirred at room temperature until a suspension mixture is formed, and then the suspension is placed in a reactor, subjected to a hydrothermal reaction at 120°C, centrifuged, washed, and dried to obtain a pre-product, and finally the pre-product is calcined at 500°C to obtain rod-shaped nano CeO2 particles;

[0054] (2) Surface modification of vinyltrimethoxysilane:

[0055] The rod-shaped CeO2 nanoparticles and vinyltrimethoxysilane were dispersed in anhydrous ethanol and stirred in a constant temperature water bath at 75°C for 2 hours, then washed with deionized water and filtered, and the solid part was dried in a vacuum drying oven for 15 hours to obtain silane-modified rod-shaped CeO2 nanoparticles.

[0056] (3) Preparation of composite emulsion:

[0057] Deionized water and initiator AIBN are used as primers, and modified rod-shaped CeO2 nanoparticles, initiator AIBN, deionized water, acrylonitrile (ACN) and isooctyl acrylate (HMA) are mixed in a mass ratio of 1:1 and sheared at high speed to obtain a pre-emulsion. After the primer becomes clear and transparent, the pre-emulsion is added dropwise in a semi-continuous manner for 3 hours. After the addition is completed, the post-initiator tert-butyl peroxide and sodium formaldehyde sulfoxylate (mass percentage 4:1) are added and kept warm for another 2 hours. The mass percentage of the primer and the pre-emulsion is 0.7:2 to obtain a composite emulsion.

[0058] Embodiment 5:

[0059] Preparation of composite emulsion:

[0060] 1. Preparation of rod-shaped CdO nanoparticles:

[0061] Prepare a 10% polyvinyl pyrrolidone (PVP) ethanol solution, add 0.08g Cd(CH3COO)2 and stir with a magnetic stirrer for 6h. After it is fully dissolved and mixed evenly, place it in a 5mL glass syringe, connect the electrospinning device, use aluminum foil as the receiving plate, the voltage is 15kV, the distance is 20cm, and the spun fiber membrane is placed in a vacuum drying oven at room temperature for 24h. Scrape off the prepared composite fiber, put it in a muffle furnace at 600℃ and calcine it for 4h, remove the template to obtain rod-shaped nano CdO particles;

[0062] 2. Surface modification of vinyltrimethoxysilane:

[0063] The rod-shaped CdO nanoparticles and vinyltrimethoxysilane were dispersed in anhydrous ethanol and stirred in a constant temperature water bath at 85°C for 2 hours, then washed with deionized water and filtered, and the solid part was dried in a vacuum drying oven for 20 hours to obtain silane-modified rod-shaped CdO nanoparticles.

[0064] 3. Preparation of composite emulsion:

[0065] Deionized water and initiator KPS are used as primers, and modified rod-shaped CdO nanoparticles, initiator KPS, deionized water, MMA and isooctyl acrylate (HMA) are mixed in a mass ratio of 1:1 and sheared at high speed to obtain a pre-emulsion. After the primer becomes clear and transparent, the pre-emulsion is added dropwise in a semi-continuous manner for 3 hours. After the addition is completed, the post-initiator tert-butyl peroxide and sodium formaldehyde sulfoxylate (mass percentage 4:1) are added and kept warm for another hour. The mass percentage of the primer and the pre-emulsion is 0.8:2 to obtain a composite emulsion.

[0066] Comparative Example 1:

[0067] Preparation of composite emulsion:

[0068] Deionized water and initiator KPS were used as primers. Initiator KPS, deionized water, MMA and BA were mixed in a mass ratio of 1:1 and sheared at high speed to obtain a pre-emulsion. After the primer became clear and transparent, the pre-emulsion was added dropwise in a semi-continuous manner for 3 hours. After the addition was completed, a rear initiator, tert-butyl peroxide and sodium formaldehyde sulfoxylate (mass percentage 4:1) were added and kept warm for another 1.5 hours. The mass percentage of the primer and the pre-emulsion was 0.8:1.9 to obtain a composite emulsion.

[0069] Detection:

[0070] 1. The composite emulsions prepared in Examples 1-5 and Comparative Example 1 were tested for residual monomers according to the industry standard SN / T 3342-2012 Determination of residual monomer content in acrylic resin - gas chromatography-mass spectrometry. The test results are shown in Table 1.

[0071] 2. The free formaldehyde content of the composite emulsions prepared in Examples 1-5 and Comparative Example 1 was tested according to the free formaldehyde content standard GB18583-2008. The test results are shown in Table 1;

[0072] 3. The composite emulsions prepared in Examples 1-5 and Comparative Example 1 were vacuum dried at 50°C for 10 hours and then dried at 120°C for 1 hour. The whiteness value of the obtained latex film was tested on a whiteness meter TC-BD48B. The test results are shown in Table 1.

[0073] 4. Take 1 ml of the composite emulsion prepared in Examples 1-5 and Comparative Example 1 every 20 minutes and test the sugar content with a sugar meter PAL-1. Record the time required when the sugar content of the composite emulsion does not change. The recorded results are shown in Table 1.

[0074] Table 1 Composite emulsion performance test data

[0075]

[0076]

[0077] It can be seen from the data in the table that the composite emulsion of copolymerization of rod-shaped metal oxide nanoparticles and vinyl monomers prepared by the method of the present invention, as can be seen from Comparative Example 1, the whiteness values ​​of the latex films in Examples 1-5 are all higher than those in Comparative Example 1, the residual monomer and formaldehyde contents are much lower than those in Comparative Example 1, and the time required for the completion of polymerization is lower than that in Comparative Example 1, indicating that the introduction of rod-shaped metal oxide nanoparticles improves the comprehensive performance of the aqueous emulsion.

[0078] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A green aqueous emulsion with high activity, zero residue and excellent anti-yellowing performance, characterized in that: The emulsion is a composite latex formed by hybridization of silane-modified rod-shaped metal oxide nanoparticles and vinyl monomers through emulsion polymerization.

2. The green aqueous emulsion according to claim 1, characterized in that: The rod-shaped metal oxide nanoparticles in the silane-modified rod-shaped metal oxide nanoparticles are at least one of MnO2, SiO2, CeO2, TiO2, CdO, La2O3, and NiO, and the size of the rod-shaped metal oxide nanoparticles is 5-15nm in diameter and 15-50nm in length.

3. The green aqueous emulsion according to claim 1, characterized in that: The silane in the silane-modified rod-shaped metal oxide nanoparticles is at least one of methacrylic acid-modified silicone oil, γ-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane, vinyl-tri(2-methoxyethoxy)silane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and γ-methacryloxypropyltrimethoxysilane.

4. The green aqueous emulsion according to claim 1, characterized in that: The vinyl monomers are at least two of acrylic acid and acrylic acid esters, methacrylic acid and methacrylic acid esters, hydroxy acrylic acid esters, hydroxy methacrylic acid esters, styrene, vinyl acetate, acrylonitrile, and olefinically terminated fluorosilicone monomers.

5. A method for preparing the green aqueous emulsion according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: (1) Preparation of rod-shaped metal oxide nanoparticles: dissolving a metal compound in a solvent, adding an acid or a base and transferring to an autoclave, heat treating at 90-180° C. for 5-24 hours, then filtering and washing the obtained mixture, drying at 50-120° C. for 10-36 hours, and then maintaining at 350-600° C. for 2-6 hours, thereby obtaining rod-shaped metal oxide nanoparticles; (2) Surface modification with silane: The rod-shaped metal oxide nanoparticles and silane are dispersed in anhydrous ethanol and stirred in a constant temperature water bath at 60-120° C. for 0.5-3 hours, then washed with deionized water and filtered, and the solid part is dried in a vacuum drying oven for 12-48 hours to obtain silane-modified rod-shaped metal oxide nanoparticles; (3) Preparation of composite emulsion: deionized water and a first initiator are used as a primer, and silane-modified rod-shaped metal oxide nanoparticles, a second initiator, deionized water and a vinyl monomer are mixed and sheared at high speed to obtain a pre-emulsion. After the primer becomes clear and transparent, the pre-emulsion is added dropwise in a semi-continuous manner for 4-6 hours. After the addition is completed, a rear initiator is added and the mixture is kept warm for 1-2 hours to obtain an aqueous emulsion, and the mass ratio of the primer to the pre-emulsion is 0.5-2:1.5-6.

6. The preparation method according to claim 5, characterized in that: The metal compound in step (1) is at least one of KMnO4, tetraethyl orthosilicate, Ce(NO3)3, tetrabutyl titanate, Cd(CH3COO)2, La(OH)3, and NiSO4.

7. The preparation method according to claim 5, characterized in that: The raw materials in the primer solution of step (3) are calculated by weight as follows: 10-50 parts of deionized water and 0.01-0.08 parts of a first initiator, and the first initiator is any one of ammonium persulfate, potassium persulfate, azobisisobutyronitrile or azobiscyanovaleric acid.

8. The preparation method according to claim 5, characterized in that: The raw materials in the pre-emulsion of step (3) are calculated by weight as follows: 12-35 parts of vinyl monomer, 1.5-32 parts of rod-shaped metal oxide nanoparticles, 0.03-0.5 parts of second initiator, and 20-100 parts of deionized water, and the second initiator is at least one of a combination of hydrogen peroxide and ascorbic acid, hydrogen peroxide and sodium formaldehyde sulfoxylate, and hydrogen peroxide and sodium pyrosulfite.

Citation Information

Patent Citations

  • Method for producing a nanocomposite dispersion comprising composite particles|of inorganic nanoparticles and organic polymers

    CN104603183A

  • Aqueous acrylic resin which can degrade formaldehyde by using visible light and preparation method of aqueous acrylic resin

    CN109851706A

  • Method of reducing the content of residual monomers in emulsion polymers

    KR100569219B1

  • Redox system and process

    US20020099156A1

Cited By

  • Water-based anti-corrosion finishing paint emulsion for offshore wind power blade and preparation method of water-based anti-corrosion finishing paint emulsion

    CN119081495A