Nanoparticle self-assembled modified cationic waterborne polyurethane elastomer as well as preparation method and application thereof

By loading nanoparticles in cationic water-based polyurethane and using electrostatic force to combine, the problem of large particle size and insufficient mechanical properties of cationic water-based polyurethane emulsion is solved, a modified polymer with small particle size and good stability is realized, and its application is expanded. scope.

CN118755048APending Publication Date: 2024-10-11LIANHONG (JIANGSU) NEW MATERIALS RES INST CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411056992.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing cationic water-based polyurethane emulsions have problems such as excessive particle size, insufficient mechanical properties, and insufficient emulsion stability and solid content, which limits its application development.

Method used

By loading nanoparticles in cationic water-based polyurethane, electrostatic force binding is used to realize nanoparticle self-assembly, adjust the pH value of the water phase and the electrostatic binding force of nanoparticles, reduce interfacial tension, and improve solid content and mechanical properties.

Benefits of technology

A modified cationic water-based polyurethane emulsion with small particle size, excellent mechanical properties and good stability has been achieved, which improves the solid content and mechanical properties and expands its application prospects in textiles, leather and conductive polymer materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755048A_ABST
    Figure CN118755048A_ABST
Patent Text Reader

Abstract

The invention discloses a nanoparticle self-assembled modified cationic waterborne polyurethane elastomer and a preparation method and application thereof.According to the nanoparticle self-assembled modified cationic waterborne polyurethane elastomer and the preparation method and application thereof, nanoparticles are introduced into a cationic waterborne polyurethane emulsion through the electrostatic interaction of anions and cations, and the interfacial tension and the emulsion particle size of the cationic waterborne polyurethane emulsion are reduced through electrostatic force combination; the solid content of the emulsion is increased to 40-45%, and meanwhile, a continuous filler network is formed, so that the mechanical property of polyurethane is improved. In addition, the nanoparticle self-assembled modified cationic waterborne polyurethane provided by the invention forms a continuous filler network, so that the nanoparticle self-assembled modified cationic waterborne polyurethane has a wide application prospect in the aspect of conductive polymer preparation. According to the method, K + is further introduced into the nano-particles, and the nano-particles with negative electricity can generate electrostatic repulsion when being stacked on the interface, so that the nano-particles can be tightly stacked on the interface, and the interface assembly effect is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer material preparation, and specifically relates to a nanoparticle self-assembly modified cationic waterborne polyurethane elastomer and a preparation method and application thereof. Background Art

[0002] As an environmentally friendly material with water as a dispersant, waterborne polyurethane is divided into anionic waterborne polyurethane and cationic waterborne polyurethane according to the characteristics of its hydrophilic ions. The synthesis method of anionic waterborne polyurethane is simple and has developed rapidly, while cationic waterborne polyurethane has developed slowly due to the difficulty in synthesis regulation and control. However, due to the characteristics of cations as hydrophilic groups, cationic waterborne polyurethane has many excellent properties that anionic waterborne polyurethane does not have. In the textile field, cationic waterborne polyurethane has better wetting properties. In the leather field, cationic waterborne polyurethane has better adhesion to the negatively charged leather surface, so it can enhance the leather feel and improve the leather quality. In addition, cationic waterborne polyurethane can also be used under acidic conditions, so it complements anionic waterborne polyurethane.

[0003] As society's requirements for environmental protection increase, waterborne polyurethane has broad application prospects due to its excellent properties such as safety, non-toxicity, non-flammability, and environmental friendliness. In addition, cationic waterborne polyurethane also has antistatic and antibacterial characteristics. However, the current cationic waterborne polyurethane emulsion has problems such as large particle size, insufficient mechanical properties, insufficient emulsion stability and solid content, which limits its application development. Summary of the invention

[0004] In order to improve the above technical problems, the present invention provides a modified cationic waterborne polyurethane, comprising a cationic waterborne polyurethane and nanoparticles supported on the cationic waterborne polyurethane.

[0005] According to an embodiment of the present invention, the nanoparticles are bound to the cationic waterborne polyurethane by electrostatic force. Preferably, the nanoparticles are bound to the cationic waterborne polyurethane by electrostatic force between positive and negative charges. Exemplarily, the nanoparticles are bound to the cationic waterborne polyurethane by COO - With NH3 + The electrostatic adsorption force between them is combined with the cationic water-based polyurethane.

[0006] According to an embodiment of the present invention, the modified cationic waterborne polyurethane may also contain K + Preferably, the K + Provided by potassium salts, such as KBr, KCl, etc.

[0007] According to an embodiment of the present invention, in the modified cationic waterborne polyurethane, the mass percentage of the cationic waterborne polyurethane may be 40% to 45%.

[0008] According to an embodiment of the present invention, in the modified cationic waterborne polyurethane, the mass percentage of nanoparticles may be 0.055% to 1.1%.

[0009] According to an embodiment of the present invention, in the modified cationic waterborne polyurethane, K + The mass percentage can be 1.9% to 4.2%.

[0010] According to an embodiment of the present invention, the modified cationic waterborne polyurethane may optionally contain a dispersant, for example, water.

[0011] According to an embodiment of the present invention, the sum of the mass percentages of the components in the modified cationic waterborne polyurethane is 100%.

[0012] According to an embodiment of the present invention, the cationic waterborne polyurethane has the definition described below.

[0013] According to an embodiment of the present invention, the nanoparticles should be negatively charged, preferably negatively charged nanoparticles that can be dispersed in water. For example, the nanoparticles are selected from the following negatively charged nanoparticles: one, two or more of carbon nanotubes, graphene, graphene oxide, MXene nanosheets, silicon dioxide, cellulose nanocrystals, etc. Preferably, the particle size of the nanoparticles is 10 to 1000 nm.

[0014] In one embodiment of the present invention, the nanoparticles contain carboxyl groups. Preferably, the nanoparticles are selected from at least one of carboxyl-modified carbon nanotubes (carboxyl content 1-5 wt%), graphene oxide, carboxyl-modified nanosilica ions (carboxyl content 1-5 wt%) and cellulose nanocrystals.

[0015] According to an embodiment of the present invention, the average particle size of the modified cationic waterborne polyurethane is 40 to 100 nm, exemplified by 40 nm, 41 nm, 46 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm.

[0016] According to an embodiment of the present invention, the modified cationic waterborne polyurethane is in the form of an emulsion. Preferably, the Zeta potential of the modified cationic waterborne polyurethane emulsion is higher than 25 mv, preferably 29 to 50 mv, exemplified by 29.1 mv, 39.8 mv, 43.8 mv, 45.1 mv or 45.9 mv.

[0017] According to an embodiment of the present invention, the modified cationic waterborne polyurethane is a nanoparticle self-assembled modified cationic waterborne polyurethane.

[0018] The present invention also provides a method for preparing the modified cationic waterborne polyurethane, which comprises mixing and reacting the cationic waterborne polyurethane with nanoparticles to obtain the modified cationic waterborne polyurethane.

[0019] According to an embodiment of the present invention, the nanoparticles are added to the reaction system in the form of an aqueous dispersion. Preferably, the concentration of the nanoparticle aqueous dispersion is 0.001 to 200.0 mg / mL, preferably 0.1 to 20.0 mg / mL, more preferably 1.0 to 20.0 mg / mL, and exemplarily 1.0 mg / mL. Further, the pH value of the nanoparticle aqueous dispersion is 0 to 7, preferably 3 to 5, and exemplarily 3.5, 4.0, 4.5 or 5.0.

[0020] According to an embodiment of the present invention, the mixing mass ratio of the cationic waterborne polyurethane to the nanoparticle aqueous dispersion is (0.66-0.81):1, exemplified by 0.66:1, 0.7:1, 0.75:1, and 0.8:1.

[0021] According to an embodiment of the present invention, the cationic waterborne polyurethane is prepared from raw materials including diisocyanate and diol by polycondensation reaction under the action of a catalyst and a chain extender.

[0022] In one embodiment of the present invention, the molar ratio of the diisocyanate to the diol is 0.5:1-5:1, exemplified by 0.5:1, 1:1, 2:1, 3:1, 4:1, 5:1.

[0023] According to an embodiment of the present invention, the diisocyanate is selected from at least one of p-toluenesulfonyl isocyanate (TSI), isophorone diisocyanate (IPDI), 4-methylphenyl isocyanate (MPI), 4-methoxyphenyl isocyanate (MOPI), phenyl isothiocyanate (PITC), benzoyl isocyanate (BI), isopropyl isothiocyanate (IPIT), hexyl isocyanate (HI) and other isocyanates and isothiocyanates.

[0024] According to an embodiment of the present invention, the diol is at least one of PEG, PBA and PBT. Preferably, the water content of the diol is controlled below 500 ppm.

[0025] In one embodiment of the present invention, the catalyst is selected from dibutyltin dilaurate, for example. Preferably, the amount of the catalyst is 0.1-0.5% of the total mass of the diol and the diisocyanate, exemplified by 0.1%, 0.2%, 0.3%, 0.4%, 0.5%.

[0026] In one embodiment of the present invention, the amount of the chain extender is 5-10% of the total mass of the diol and the diisocyanate, and exemplary amounts are 5%, 6%, 7%, 8%, 9%, and 10%.

[0027] According to an embodiment of the present invention, the chain extender includes a chain extender with nitrogen atoms on the main chain and a chain extender with nitrogen atoms on the side chain, preferably a chain extender with nitrogen atoms on the side chain. For example, the chain extender with nitrogen atoms on the main chain is N-methyldiethanolamine; the chain extender with nitrogen atoms on the side chain is at least one of 3-imidazole-1-ylpropane-1,2-diol and 2,2-dimethylamino-1,3-propanediol.

[0028] In one embodiment of the present invention, the preparation of the cationic waterborne polyurethane is carried out in a solvent system. For example, diisocyanate, diol and catalyst are sequentially mixed and reacted, and then a solvent and a chain extender are added. For example, the solvent is a polar solvent such as acetone, acetophenone or propiophenone.

[0029] According to an embodiment of the present invention, in order to reduce the electrostatic repulsion between the nanoparticles and enable the nanoparticles to be densely packed at the interface, the nanoparticle aqueous dispersion may further contain K + Preferably, the K + The concentration of K is 0.5 to 2 mol / L, exemplarily 1.0 mol / L. + Provided by potassium salts, such as KBr, KCl, etc.

[0030] According to an embodiment of the present invention, the preparation method of the modified cationic waterborne polyurethane comprises the following steps:

[0031] (1) Synthesis of cationic waterborne polyurethane: Mix diisocyanate and diol, add catalyst (such as dibutyltin dilaurate), carry out polycondensation reaction (react at 60-100°C for 0.5-6.0h), cool down (to 30°C), add solvent (stir for 0.2-2.0h), add chain extender for reaction (react at 40-60°C for 2-5h); add 1,4-butanediol to control isocyanate index, continue reaction (react at 40-70°C for 1-6h), and finally cool down (to 20-40°C) to remove solvent;

[0032] (2) adding the nanoparticle aqueous dispersion to the cationic waterborne polyurethane obtained in step (1), stirring, and obtaining a nanoparticle-modified cationic waterborne polyurethane emulsion.

[0033] Furthermore, the nanoparticle-modified cationic aqueous polyurethane emulsion obtained by the above steps (1) and (2) has the following properties: Figure 1 The structure shown (taking carbon nanotubes as an example).

[0034] According to an embodiment of the present invention, in step (1), 1,4-butanediol is added to control the isocyanate index to 0.85 to 0.95, exemplarily 0.9.

[0035] The present invention also provides an adhesive film, which contains the modified cationic waterborne polyurethane or is prepared from the modified cationic waterborne polyurethane.

[0036] According to an embodiment of the present invention, the tensile strength of the adhesive film is higher than 14 MPa, preferably 15 to 25 MPa, and exemplified by 17 MPa, 18.3 MPa, 19.8 MPa, 20.9 MPa, and 23 MPa.

[0037] The present invention also provides a method for preparing the above-mentioned adhesive film, which comprises: preparing the modified cationic waterborne polyurethane by adopting the above-mentioned method for preparing the modified cationic waterborne polyurethane.

[0038] Furthermore, the modified cationic waterborne polyurethane emulsion is prepared.

[0039] According to an embodiment of the present invention, the method for preparing the adhesive film may further include: casting the modified cationic waterborne polyurethane emulsion onto a (polytetrafluoroethylene) template, drying to constant weight after standing (such as at room temperature for three days) to obtain the adhesive film.

[0040] According to an embodiment of the present invention, the drying temperature is 20 to 150° C., exemplarily 50° C.; the drying time is, for example, 1 to 24 hours, exemplarily 24 hours.

[0041] The present invention also provides application of the modified cationic waterborne polyurethane in the fields of textiles, leather and conductive polymers.

[0042] The present invention also provides a product, which contains the modified cationic waterborne polyurethane and / or is prepared from the modified cationic waterborne polyurethane.

[0043] According to an embodiment of the present invention, the product may be a textile, leather or a conductive polymer material.

[0044] The present invention also provides a method for improving the wetting performance of textiles, comprising using the modified cationic waterborne polyurethane for preparing textiles.

[0045] The present invention also provides a method for improving leather quality, comprising using the modified cationic waterborne polyurethane for leather preparation.

[0046] Beneficial effects of the present invention:

[0047] (1) The present invention provides a modified cationic waterborne polyurethane, specifically a modified cationic waterborne polyurethane emulsion, which has the advantages of small particle size, excellent mechanical properties, good stability and high solid content, and has broad application prospects.

[0048] (2) The present invention realizes the self-assembly of nanoparticles on the surface of the emulsion particles by introducing nanoparticles into the water phase and adjusting the pH value of the water phase to control the electrostatic binding force between the polyurethane segments and the nanoparticles. The self-assembly of hydrophilic nanoparticles at the interface reduces the interfacial tension, thereby reducing the emulsion particle size of the cationic waterborne polyurethane, and enhancing the stability of the emulsion, achieving the effect of increasing the solid content. At the same time, the nanoparticles can form a filler network in the film, thereby improving the mechanical properties of the cationic waterborne polyurethane. Specifically:

[0049] The invention introduces nanoparticles (such as carbon nanotubes) into cationic waterborne polyurethane emulsion through the electrostatic action of anions and cations, reduces the interfacial tension and emulsion particle size of the cationic waterborne polyurethane emulsion through electrostatic force combination, increases the solid content of the emulsion to 40-45%, and forms a continuous filler network, thereby improving the mechanical properties of the polyurethane. In addition, the nanoparticle self-assembly modified cationic waterborne polyurethane of the invention has a wide application prospect in the preparation of conductive polymer materials because a continuous filler network is formed.

[0050] (3) The present invention further introduces K into nanoparticles (such as carbon nanotubes) + , since negatively charged nanoparticles will generate electrostatic repulsion when they are deposited at the interface, it is not conducive to the close accumulation of nanoparticles. + The addition of shields the electrostatic repulsion, allowing the nanoparticles to accumulate tightly on the interface, thereby further improving the effect of interface assembly.

[0051] (4) Since the power source of the interface assembly is to use electrostatic attraction to increase the adsorption energy of the nanoparticles at the interface, thereby making the adsorption energy greater than the energy of the thermal motion of the nanoparticles, the nanoparticles can be firmly anchored on the interface. The electrostatic attraction comes from the electrostatic interaction between the protonated nitrogen atoms and the ionized carboxylic acid radicals of the cationic waterborne polyurethane. In order to ensure the coexistence of the protonation of the nitrogen atoms and the ionization of the carboxylic acid, the present invention controls the pH of the nanoparticles (such as carbon nanotubes) to increase the adsorption energy of the nanoparticles at the interface, thereby allowing the nanoparticles to be firmly anchored on the interface.

[0052] (5) The present invention uses a chain extender with nitrogen atoms in the side chain to reduce the steric hindrance of the electrostatic interaction between the protonated nitrogen atoms and the carboxylate groups, thereby enabling the nanoparticles to be firmly anchored on the interface. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 Schematic diagram of the assembly of cationic waterborne polyurethane and nanoparticle aqueous dispersion.

[0054] Figure 2 This is a TEM image of the modified cationic waterborne polyurethane product prepared in Example 1 (taking carbon nanotubes as an example). DETAILED DESCRIPTION

[0055] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0056] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0057] Zeta potential test: According to the standard GB / Z 42353-2023 "Zeta potential determination operation guide", dynamic light scattering (Nanobrook Omni, USA) is used for measurement (the potential reflects the stability of the emulsion, and the higher the potential, the better the stability).

[0058] Tensile strength test: According to the standard GB / T528-1998Y "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber", all the specimens to be stretched were cut into dumbbell-shaped specimens, and a uniaxial tensile test was carried out at room temperature at a tensile rate of 500 mm / min using a universal material testing machine.

[0059] Example 1

[0060] A preparation method of a nanoparticle self-assembly modified cationic waterborne polyurethane elastomer comprises the following steps: placing 300g of dehydrated polyethylene glycol (PEG600) into a four-necked flask equipped with a stirring device, a condensation reflux device and a thermometer, opening the reflux device and the stirrer, heating the flask to 70°C, dripping 222g of IPDI (the molar ratio of IPDI to PEG600 is 2:1) into the flask, and completing the dripping in 1h, then adding 2.61g of dibutyltin dilaurate, cooling the temperature to 30°C after reacting for 1h, adding 26.1g of acetone, heating the temperature to 50°C, adding 52.2g of a chain extender N-methyldiethanolamine at one time, and finally adding 15.54g of 1,4-butanediol to control the isocyanate index to be 0.9 (isocyanate index=isocyanate mole number / hydroxyl mole number), and reacting at 50°C for 3h. Acetone was removed by vacuum distillation at 30°C, 900 mL of a 1.0 mg / mL, pH 3.5 carbon nanotube aqueous dispersion (purchased from Pioneer Nano, low-purity carboxylated single-walled carbon nanotubes, model: XFS07, diameter 1-2 nm, carboxyl content 2.73 wt%) was added, and an emulsion was obtained after stirring at 50°C for 1 hour. The emulsion had a solid content of 45% and an average particle size of 50 nm. The emulsion was cast on a horizontal PTFE plate, placed at room temperature for 3 days, and then transferred to a 50°C forced air oven for drying for 24 hours to obtain a modified cationic waterborne polyurethane product.

[0061] The Zeta potential of the emulsion prepared in this example is 39.8 mv, and the tensile strength of the finished modified cationic waterborne polyurethane is 17 MPa.

[0062] Figure 2 This is a TEM image of the finished modified cationic waterborne polyurethane prepared in Example 1 (taking carbon nanotubes as an example). It can be seen from the figure that the carbon nanotubes are evenly dispersed in the cationic waterborne polyurethane film, forming a continuous filler network, which helps to improve the mechanical properties of the cationic waterborne polyurethane.

[0063] Example 2

[0064] A preparation method of a nanoparticle self-assembled modified cationic waterborne polyurethane elastomer, comprising: placing 300g of dehydrated polyethylene glycol (PEG600) into a four-necked flask equipped with a stirrer, a condensation reflux device and a thermometer. The reflux device and the stirrer are turned on, the temperature is raised to 70°C, 222g of IPDI (the molar ratio of IPDI to PEG600 is 2:1) is added dropwise to the flask, and the addition is completed in 1h, then 2.61g of dibutyltin dilaurate is added, the temperature is lowered to 30°C after reaction for 1h, 26.1g of acetone is added, the temperature is raised to 50°C, 52.2g of chain extender N-methyldiethanolamine is added at one time, 15.54g of 1,4-butanediol is added to control the isocyanate index to 0.9, and the reaction is carried out at 50°C for 3h. Acetone is removed by reduced pressure distillation at 30°C, and 900mL of a 1.0mg / mL, pH 3.5, K + A 1.0 mol / L carbon nanotube aqueous dispersion (purchased from Pioneer Nano, low-purity carboxylated single-walled carbon nanotubes, model: XFS07, diameter 1-2 nm, carboxyl content 2.73 wt %; wherein K + The method is to add KBr to the carbon nanotube aqueous dispersion and stir at 50°C for 1 hour to obtain an emulsion. The solid content of the emulsion is 45%, and the average particle size is 46nm. The emulsion is cast on a horizontal polytetrafluoroethylene plate, placed at room temperature for 3 days, and then transferred to a 50°C forced air oven for drying for 24 hours to obtain a modified cationic waterborne polyurethane product.

[0065] The Zeta potential of the emulsion prepared in this example is 43.8 mv, and the tensile strength of the finished modified cationic waterborne polyurethane is 19.8 MPa.

[0066] Example 3

[0067] A preparation method of a nanoparticle self-assembly modified cationic waterborne polyurethane elastomer comprises the following steps: placing 300 g of dehydrated polyethylene glycol (PEG600) into a four-necked flask equipped with a stirring device, a condensation reflux device and a thermometer, opening the reflux device and the stirrer, heating to 70°C, dripping 222 g of IPDI (the molar ratio of IPDI to PEG600 is 2:1) into the flask, and completing the dripping in 1 hour, adding 2.61 g of dibutyltin dilaurate, reacting for 1 hour, cooling to 30°C, adding 26.1 g of acetone, and heating to 50°C, adding 52.2 g of a chain extender 2,2-dimethylamino-1,3-propylene glycol at one time, adding 15.52 g of 1,4-butanediol to control the isocyanate index to 0.9, and reacting at 50°C for 3 hours. Acetone was removed by vacuum distillation at 30°C, and 900 mL of a carbon nanotube aqueous dispersion (purchased from Pioneer Nano, low-purity carboxylated single-walled carbon nanotubes, model: XFS07, diameter 1-2 nm, carboxyl content 2.73 wt%) with a concentration of 1.0 mg / mL and a pH of 3.5 was added, and an emulsion was obtained after stirring. The solid content of the emulsion was 45%, and the average particle size was 41 nm. The emulsion was cast on a horizontal PTFE plate, placed at room temperature for 3 days, and then transferred to a 50°C forced air oven and dried for 24 hours to obtain a modified cationic waterborne polyurethane product.

[0068] The Zeta potential of the emulsion prepared in this example is 45.1 mv, and the tensile strength of the finished modified cationic waterborne polyurethane is 20.9 MPa.

[0069] Example 4

[0070] A preparation method of a nanoparticle self-assembled modified cationic waterborne polyurethane elastomer comprises the following steps: placing 300 g of dehydrated polyethylene glycol (PEG600) into a four-necked flask equipped with a stirring device, a condensation reflux device and a thermometer. The reflux device and the stirrer are turned on, the temperature is raised to 70°C, 222 g of IPDI (the molar ratio of IPDI to PEG600 is 2:1) is added dropwise to the flask, and the addition is completed within 1 hour. Then, 2.61 g of dibutyltin dilaurate is added, the temperature is lowered to 30°C after reaction for 1 hour, 26.1 g of acetone is added, the temperature is raised to 50°C, 52.2 g of a chain extender 2,2-dimethylamino-1,3-propylene glycol is added at one time, and finally 15.52 g of 1,4-butanediol is added to control the isocyanate index to 0.9, and the reaction is carried out at 50°C for 3 hours. Acetone is removed by vacuum distillation at 30°C, and 900 mL of 1.0 mg / mL, pH 3.5, and K + A 1.0 mol / L carbon nanotube aqueous dispersion (purchased from Pioneer Nano, low-purity carboxylated single-walled carbon nanotubes, model: XFS07, diameter 1-2 nm, carboxyl content 2.73 wt%; wherein K +The method is to add KBr to the carbon nanotube aqueous dispersion and stir at 50°C for 1 hour to obtain an emulsion. The solid content of the emulsion is 45% and the average particle size is 40nm. The emulsion is cast on a horizontal polytetrafluoroethylene plate, placed at room temperature for 3 days, and then transferred to a 50°C forced air oven for drying for 24 hours to obtain a modified cationic waterborne polyurethane product.

[0071] The Zeta potential of the emulsion prepared in this example is 45.9 mv, and the tensile strength of the finished modified cationic waterborne polyurethane is 23 MPa.

[0072] Example 5

[0073] A preparation method of a nanoparticle self-assembly modified cationic waterborne polyurethane elastomer comprises the following steps: placing 300 g of dehydrated polyethylene glycol (PEG600) into a four-necked flask equipped with a stirring device, a condensation reflux device and a thermometer, opening the reflux device and the stirrer, heating to 70°C, dripping 222 g of IPDI (the molar ratio of IPDI to PEG600 is 2:1) into the flask, and completing the dripping in 1 hour, then adding 2.61 g of dibutyltin dilaurate, reacting for 1 hour, cooling to 30°C, adding 26.1 g of acetone, heating to 50°C, adding 52.2 g of a chain extender 2,2-dimethylamino-1,3-propylene glycol at one time, and finally adding 15.52 g of 1,4-butanediol to control the isocyanate index to 0.9, and reacting at 50°C for 3 hours. Acetone was removed by vacuum distillation at 30°C, and 900 mL of a carbon nanotube aqueous dispersion (purchased from Pioneer Nano, low-purity carboxylated single-walled carbon nanotubes, model: XFS07, diameter 1-2 nm, carboxyl content 2.73 wt%) with a concentration of 1.0 mg / mL and a pH of 5.0 was added, and an emulsion was obtained after stirring. The solid content of the emulsion was 45%, and the average particle size was 100 nm. The emulsion was cast on a horizontal polytetrafluoroethylene plate, placed at room temperature for 3 days, and then transferred to a 50°C forced air oven and dried for 24 hours to obtain a modified cationic waterborne polyurethane product.

[0074] The Zeta potential of the emulsion prepared in this example is 29.1 mv, and the tensile strength of the finished modified cationic waterborne polyurethane is 18.3 MPa.

[0075] Comparative Example 1

[0076] A method for preparing a cationic waterborne polyurethane elastomer comprises the following steps: placing 300 g of dehydrated polyethylene glycol (PEG600) into a four-necked flask equipped with a stirring device, a condensation reflux device and a thermometer. The reflux device and the stirrer are turned on, the temperature is raised to 70°C, 222 g of IPDI (the molar ratio of IPDI to PEG600 is 2:1) is added dropwise to the flask, the addition is completed within 1 hour, 2.61 g of dibutyltin dilaurate is added, the temperature is lowered to 30°C after reaction for 1 hour, 26.1 g of acetone is added, the temperature is raised to 50°C, 52.2 g of a chain extender N-methyldiethanolamine is added at one time, and finally 15.54 g of 1,4-butanediol is added to control the isocyanate index to 0.9, and the reaction is carried out at 50°C for 3 hours. Acetone is removed by vacuum distillation at 30°C, 900 mL of a deionized HCl solution with a pH of 3.5 is added, and an emulsion is obtained after stirring. The solid content of the emulsion was 45% and the average particle size was 150 nm. The emulsion was cast on a horizontal polytetrafluoroethylene plate, placed at room temperature for 3 days, and then transferred to a 50°C forced air oven for drying for 24 hours to obtain a finished cationic waterborne polyurethane product.

[0077] The Zeta potential of the emulsion prepared in this comparative example is 23.4 mv, and the tensile strength of the finished cationic waterborne polyurethane is 14 MPa.

[0078] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A modified cationic waterborne polyurethane, It is characterized in that The modified cationic waterborne polyurethane comprises cationic waterborne polyurethane and nanoparticles supported on the cationic waterborne polyurethane.

2. The modified cationic waterborne polyurethane according to claim 1, It is characterized in that The nanoparticles are bonded to the cationic waterborne polyurethane through electrostatic force. Preferably, the nanoparticles are - With NH 3 + The electrostatic adsorption force between them is combined with the cationic water-based polyurethane. Preferably, the modified cationic waterborne polyurethane may also contain K + . Preferably, the modified cationic waterborne polyurethane is in the form of an emulsion. Preferably, the Zeta potential of the modified cationic aqueous polyurethane emulsion is higher than 25 mv.

3. The method for preparing the modified cationic waterborne polyurethane according to claim 1 or 2, It is characterized in that The preparation method comprises the steps of mixing and reacting cationic waterborne polyurethane with nanoparticles to obtain the modified cationic waterborne polyurethane.

4. The preparation method according to claim 3, It is characterized in that The nanoparticles are added into the reaction system in the form of water dispersion. Preferably, the concentration of the nanoparticle aqueous dispersion is 0.001 to 200.0 mg / mL. Preferably, the mixing mass ratio of the cationic waterborne polyurethane to the nanoparticle aqueous dispersion is (0.66-0.81):

1. Preferably, the nanoparticle aqueous dispersion may also contain K + Preferably, the K + The concentration is 0.5~2mol / L.

5. A film, It is characterized in that The modified cationic waterborne polyurethane contains the modified cationic waterborne polyurethane according to claim 1 or 2 or is prepared from the modified cationic waterborne polyurethane according to claim 1 or 2.

6. The method for preparing the adhesive film according to claim 5, It is characterized in that The preparation method comprises: preparing the modified cationic waterborne polyurethane by adopting the preparation method of the modified cationic waterborne polyurethane according to claim 3 or 4. Preferably, a modified cationic aqueous polyurethane emulsion is prepared. Preferably, the method for preparing the adhesive film may further include: casting the modified cationic waterborne polyurethane emulsion into a template, and drying the template to a constant weight after standing.

7. Application of the modified cationic waterborne polyurethane according to claim 1 or 2 in the fields of textiles, leather and conductive polymers.

8. A product, It is characterized in that It contains the modified cationic waterborne polyurethane described in claim 1 or 2 and / or is prepared from the modified cationic waterborne polyurethane described in claim 1 or 2.

9. A method for improving the wetting properties of textiles, It is characterized in that The method comprises using the modified cationic waterborne polyurethane according to claim 1 or 2 for preparing textiles.

10. A method for improving leather quality, It is characterized in that The method comprises using the modified cationic waterborne polyurethane according to claim 1 or 2 for the preparation of leather.

Citation Information

Cited By

  • Antibacterial functionalized nano silicon dioxide modified polyurethane coating and preparation method thereof

    CN119371888A

  • Water-soluble engineering plastic reinforced cationic waterborne polyurethane material and preparation method thereof

    CN119639217A