Degradable high-resilience foaming packaging material and preparation method thereof
By using the blend modification of thermoplastic biodegradable plastics and thermoplastic elastomers and plant fiber fillers in biodegradable foam packaging materials, combined with the collaborative foaming technology of physical foaming agents and chemical foaming agents, we solve the problem of existing materials. Issues of performance and cost, achieving high resilience and good biodegradability.
Patent Information
- Application Number
- CN202410964635.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-11
AI Technical Summary
Existing biodegradable foam packaging materials have limitations in terms of cost, technology and performance, making it difficult to prepare foam packaging materials that are degradable and have excellent performance.
Thermoplastic biodegradable plastics and thermoplastic elastomers are used as matrix materials, combined with plant fiber fillers, and through collaborative foaming technology of physical foaming agents and chemical foaming agents to prepare high-resilience degradable foam packaging materials. Specifically, it includes the blending modification of polybutylene adipate/terephthalate (PBAT) and polyurethane thermoplastic elastomer (TPU), as well as the use of wood powder as filler and nucleating agent, combined with a one-step molding method. processing.
It improves the expandability and resilience of the material, reduces the cost, simplifies the preparation process, and achieves efficient foaming effect and good biodegradability.
Smart Images

Figure CN118755239A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of packaging materials, and in particular to a degradable high-resilience foaming packaging material and a preparation method thereof. Background Art
[0002] Foam packaging materials are widely used in food, electronic products, furniture and other industries due to their light weight, heat insulation, sound absorption, shock absorption and other characteristics. However, they have attracted widespread attention due to environmental issues such as difficulty in degradation, recycling, resource waste, environmental pollution and microplastic residue. As more and more countries and regions have successively issued plastic restrictions, plastic bans and related regulations, packaging materials are also developing towards biodegradable materials. Biodegradable foam materials have the characteristics of light weight, high porosity, good flexibility, high efficiency in energy absorption and heat insulation, and excellent biodegradability. They have great application prospects in cushioning packaging, logistics and transportation, aerospace, sports and leisure and other fields.
[0003] At present, there are still limitations in terms of cost, process and performance for preparing foam packaging materials from biodegradable plastics. Therefore, preparing biodegradable foam packaging materials with excellent performance is one of the problems to be solved in this technical field. Summary of the invention
[0004] In order to solve at least one aspect of the above problems and defects in the prior art, the present invention provides a degradable high-resilience foam packaging material and a preparation method thereof, which can prepare a degradable high-resilience foam packaging material.
[0005] The first aspect of the present invention provides a degradable high-resilience foam packaging material, comprising:
[0006] It includes a base material, a foaming agent and a catalyst; the composition and mass percentage of the base material are:
[0007] Biodegradable polymer 70%~90%,
[0008] Plant fiber filler 10% to 30%;
[0009] The foaming agent is a mixed foaming agent, including a physical foaming agent and a chemical foaming agent;
[0010] The catalyst includes zinc oxide.
[0011] Specifically, according to the degradable high-resilience foam packaging material of the first aspect, the biodegradable polymer includes a first biodegradable polymer and a second biodegradable polymer;
[0012] The first biodegradable polymer includes one or a mixture of polybutylene adipate / terephthalate (PBAT), polybutylene succinate (PBS), polylactic acid (PLA), polyhydroxyalkanoate (PHA), polycaprolactone (PCL), thermoplastic starch (TPS), and polycarbonate (PPC);
[0013] The second biodegradable polymer includes one or a mixture of styrene-based thermoplastic elastomer, polyurethane-based thermoplastic elastomer (TPU), polyolefin-based thermoplastic elastomer, polyamide-based thermoplastic elastomer (TPEA), ester-based thermoplastic elastomer (TPEE), organic fluorine-based thermoplastic elastomer (TPF), organic silicon-based thermoplastic elastomer or ethylene-based thermoplastic elastomer.
[0014] Furthermore, the composition and mass percentage of the first biodegradable polymer and the second biodegradable polymer are as follows:
[0015] The first biodegradable polymer is polybutylene adipate / terephthalate (PBAT) 40% to 80%;
[0016] The second biodegradable polymer is polyurethane thermoplastic elastomer (TPU) 10% to 50%.
[0017] Specifically, according to the degradable high-resilience foam packaging material described in the first aspect, the plant fiber filler includes one or a mixture of wood powder, bamboo powder, straw or waste plant fibers.
[0018] Preferably, the mass percentage of the plant fiber filler is 20%; the mesh number of the plant fiber filler is 40-200 meshes, preferably the mesh number of the plant fiber filler is 100 meshes;
[0019] Preferably, the plant fiber filler is wood powder.
[0020] Specifically, according to the degradable high-resilience foam packaging material described in the first aspect, the chemical foaming agent includes one or a mixture of azobisisobutyronitrile (AIBN), azodicarbonamide (AC), hydrazine hydrogen sulfate (HSCN) and dimethyl sulfate (DMS), isopentyl nitrite (IIPN), sodium bicarbonate, aluminum hydroxide, magnesium hydroxide or melamine.
[0021] Specifically, according to the degradable high-resilience foam packaging material described in the first aspect, the mixed foaming agent accounts for 2% to 8% of the weight percentage of the base material, preferably 2%; the physical foaming agent accounts for 1% to 4% of the total weight of the mixed foaming agent, preferably 2%; the chemical foaming agent accounts for 1% to 3% of the weight percentage of the base material, preferably 2%.
[0022] Furthermore, the physical foaming agent includes a microsphere expansion agent and / or a microsphere foaming agent.
[0023] Specifically, according to the degradable high-resilience foam packaging material described in the first aspect, the catalyst accounts for 1% to 3% by weight of the base material, preferably 2%; the weight ratio of the chemical foaming agent to the catalyst is 4:1 to 1:1.
[0024] The second aspect of the present invention provides a method for preparing a degradable foam packaging material, comprising:
[0025] Step 1: According to a certain ratio, weigh a certain amount of biodegradable polymer and put it into a high-speed mixer to mix evenly;
[0026] Step 2: Spread the plant fiber filler evenly on the tray, dry it, weigh a certain amount of the dried plant fiber filler, add it into the high-speed mixer and continue to mix it evenly;
[0027] Step 3: Weigh a certain amount of chemical foaming agent and catalyst, mix them evenly, then add them into a high-speed mixer and continue to mix evenly;
[0028] Step 4: Weigh a certain amount of physical foaming agent and add it into a high-speed mixer and continue to mix evenly to obtain the final mixed material;
[0029] Step 5: Spread the final mixed material in a mold and put it into an oven for processing; the processing includes two stages, the first stage processing temperature is 140-150° C., the time is 10-20 minutes; the second stage processing temperature is 160-170° C., the time is 10-20 minutes;
[0030] Step 6: Take out the mold and cool it to room temperature. The material is cooled and solidified to obtain a foaming packaging material.
[0031] Further, the drying temperature in step 2 is 100° C. to 110° C., preferably 103° C.;
[0032] The first stage processing temperature in step 5 is preferably 145° C. and the time is 15 minutes; the second stage processing temperature is preferably 165° C. and the time is 15 minutes.
[0033] The degradable high-resilience foam packaging material and the preparation method thereof according to the first and second aspects of the present invention have at least one of the following advantages:
[0034] 1. The present invention uses thermoplastic biodegradable plastics and thermoplastic elastomers as matrix materials, especially polybutylene adipate / terephthalate (PBAT) and polyurethane thermoplastic elastomer (TPU) as matrix materials. Compared with traditional plastics, the packaging material of the present invention is biodegradable; when polybutylene adipate / terephthalate (PBAT) and polyurethane thermoplastic elastomer (TPU) are blended, the melt strength of the blend is improved, and it has a strong recoverable elastic deformation, which can bind more foaming gas, reduce the escape of foaming gas, increase the diffusion rate of foaming gas, and increase the biaxial tensile force of the cell wall to withstand the cell growth, so it is beneficial to the formation of bubble nuclei, bubble growth, and stable solidification of bubbles, and greatly improves the expandability of the blend.
[0035] Second, the present invention uses plant fibers from a wide range of sources, especially wood powder, as fillers and nucleating agents, and plastic reduction can reduce costs. Plant fibers as fillers can increase melt strength, but cannot melt in the plastic homogeneous system to play a heterogeneous nucleation role, which is conducive to the formation and diffusion of uniform bubble nuclei, and the material foaming is more uniform.
[0036] 3. The present invention uses physical foaming agents and chemical foaming agents for synergistic foaming, and the prepared material has high resilience.
[0037] Fourth, the preparation method of the present invention adopts a one-step molding method. There is no need to modify the materials before preparation. The raw materials are mixed evenly and then placed in a mold and heated at high temperature. The preparation process is simple and efficient. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] These and / or other aspects and advantages of the present invention will become apparent and readily understood from the following description of the preferred embodiments in conjunction with the accompanying drawings, in which:
[0039] Figure 1 This is a flow chart of the preparation process of a specific embodiment of the present invention;
[0040] Figure 2 This is a front view of a degradable high-resilience foam packaging material prepared according to a specific embodiment of the present invention;
[0041] Figure 3 A side view of a degradable high-resilience foam packaging material prepared in one specific embodiment of the present invention;
[0042] Figure 4 This is a cell morphology diagram of a degradable high-resilience foam packaging material prepared in a specific embodiment of the present invention;
[0043] Figure 5 This is a diameter size distribution diagram of a degradable high-resilience foam packaging material prepared in a specific embodiment of the present invention;
[0044] Figure 6This is a ten-cycle compression curve of a degradable high-resilience foam packaging material prepared in a specific embodiment of the present invention. DETAILED DESCRIPTION
[0045] The technical solution of the present invention is further specifically described below by examples and in conjunction with the accompanying drawings. In the specification, the same or similar reference numerals indicate the same or similar components. The following description of the embodiments of the present invention with reference to the accompanying drawings is intended to explain the overall inventive concept of the present invention and should not be construed as a limitation of the present invention.
[0046] In recent years, biodegradable foam materials have the characteristics of light weight, high porosity, good flexibility, efficient energy absorption and heat insulation, and excellent biodegradability, and have great application prospects in the fields of cushioning packaging, logistics and transportation, aerospace, sports and leisure, etc. However, there are still limitations in the cost, process and performance of biodegradable plastics for preparing foam packaging materials. Therefore, using biodegradable materials to prepare foam packaging materials with excellent performance is one of the problems to be solved in this technical field.
[0047] Therefore, we proposed a degradable high-resilience foam packaging material and a preparation method thereof, which can prepare a degradable foam packaging material with high resilience.
[0048] The first aspect of the present invention discloses a degradable high-resilience foam packaging material, comprising a base material, a foaming agent and a catalyst; the composition and mass percentage of the base material are:
[0049] Biodegradable polymer 70%~90%,
[0050] Plant fiber filler 10% to 30%;
[0051] The foaming agent is a mixed foaming agent, including a microsphere expansion agent and a chemical foaming agent;
[0052] The catalyst includes zinc oxide.
[0053] In one embodiment, the biodegradable polymer includes a first biodegradable polymer and a second biodegradable polymer;
[0054] The first biodegradable polymer includes one or a mixture of polybutylene adipate / terephthalate (PBAT), polybutylene succinate (PBS), polylactic acid (PLA), polyhydroxyalkanoate (PHA), polycaprolactone (PCL), thermoplastic starch (TPS), and polycarbonate (PPC);
[0055] The second biodegradable polymer includes one or a mixture of styrene thermoplastic elastomer, polyurethane thermoplastic elastomer (TPU), polyolefin thermoplastic elastomer, polyamide thermoplastic elastomer (TPEA), ester thermoplastic elastomer (TPEE), organic fluorine thermoplastic elastomer (TPF), organic silicon thermoplastic elastomer or ethylene thermoplastic elastomer.
[0056] In one embodiment, the composition and mass percentage of the first biodegradable polymer and the second biodegradable polymer are:
[0057] The first biodegradable polymer is polybutylene adipate / terephthalate (PBAT) 40% to 80%;
[0058] The second biodegradable polymer is 10% to 50% of polyurethane thermoplastic elastomer (TPU);
[0059] The plant fiber filler includes one or a mixture of wood powder, bamboo powder, straw or waste plant fibers.
[0060] In a specific embodiment, polybutylene adipate / terephthalate (PBAT), polybutylene succinate (PBS), polylactic acid (PLA), polyhydroxyalkanoate (PHA), polycaprolactone (PCL), thermoplastic starch (TPS), polycarbonate (PPC), etc. are thermoplastic biodegradable plastics, which are plastics that are both thermoplastic and can be decomposed by microorganisms under certain conditions. These thermoplastic biodegradable plastics maintain the processing convenience of traditional plastics while also having environmentally friendly characteristics.
[0061] Among them, polybutylene adipate / terephthalate (PBAT) has good ductility and elongation at break, as well as good heat resistance, impact resistance and excellent biodegradability. However, due to the relatively low molecular weight of polybutylene adipate / terephthalate (PBAT), the molecular chain is linear, and the degree of entanglement between molecular chains is low, so the melt strength is low. On the one hand, the binding effect on the foaming gas is small, and the foaming gas is easy to escape and cannot be stably present in the pore structure. On the other hand, the pore wall cannot withstand the tensile force of pore growth during the pore growth and shaping stage, and the pores are easy to collapse, merge and rupture, resulting in a larger pore size. At the same time, because polybutylene adipate / terephthalate (PBAT) is a semi-crystalline polymer, the solubility and diffusion rate of the foaming agent in the crystal region are low, the pore nucleation will be inhibited, and the crystal region is not easy to plastically deform, the pore growth is restricted, and the foaming properties such as pore morphology, foaming ratio, and buffering are all affected.
[0062] In order to improve the expandability of polybutylene adipate / terephthalate (PBAT), other polymers may be added to blend and modify it. As specifically described in the embodiments of the present invention, polybutylene adipate / terephthalate (PBAT) is blended and modified with a thermoplastic elastomer (TPE).
[0063] Thermoplastic elastomer (TPE) is a kind of material with rubber properties and plastic processing convenience. There are mainly the following types: styrene thermoplastic elastomer (SBS, SEBS, SIS, etc.), polyurethane thermoplastic elastomer (TPU), polyolefin thermoplastic elastomer (TPV, TPO), polyamide thermoplastic elastomer (TPEA), ester thermoplastic elastomer (TPEE), organic fluorine thermoplastic elastomer (TPF), silicone thermoplastic elastomer or ethylene thermoplastic elastomer, etc. Thermoplastic elastomer combines the dual properties of rubber and plastic, which can not only replace part of rubber, but also modify plastic, so it is widely used in rubber industry and plastic industry.
[0064] Among them, polyurethane thermoplastic elastomer (TPU) is a type of thermoplastic elastomer that can be plasticized by heating and dissolved by solvents. It has excellent comprehensive properties and processing properties such as high strength, high toughness, wear resistance, oil resistance, and temperature resistance. Polyurethane thermoplastic elastomer (TPU) can be reused after being discarded and can be degraded in a composting state.
[0065] In a specific embodiment, polybutylene adipate / terephthalate (PBAT) is added with polyurethane thermoplastic elastomer (TPU) for blending modification. When polybutylene adipate / terephthalate (PBAT) and polyurethane thermoplastic elastomer (TPU) are blended, polybutylene adipate / terephthalate (PBAT) and polyurethane thermoplastic elastomer (TPU) undergo an ester exchange reaction, the molecular chains are highly entangled with each other, the free movement of the molecular chains is reduced, the internal friction of the blend is increased, the melt strength of the blend is improved, the binding effect on the foaming gas is increased, and the escape of the foaming gas is reduced. Also due to the "solvent" effect of the polyurethane thermoplastic elastomer (TPU), part of the crystallization of polybutylene adipate / terephthalate (PBAT) is destroyed, and the diffusion rate of the foaming agent in the blend is increased, which is beneficial to the formation and diffusion of bubble nucleation; at the same time, the polyurethane thermoplastic elastomer (TPU) melt has a strong recoverable elastic deformation during flow, which is not only beneficial to the growth of bubbles, but also improves the biaxial tensile force of the bubble wall to withstand the growth of bubbles, thereby greatly improving the expandability of the blend.
[0066] In another specific embodiment, in order to improve the expandability of polybutylene adipate / terephthalate (PBAT), other polymers may be added to perform filling and modification, such as described in the embodiment of the present invention, polybutylene adipate / terephthalate (PBAT) is filled and modified by adding natural plant fibers.
[0067] After polybutylene adipate / terephthalate (PBAT) and polyurethane thermoplastic elastomer (TPU) are blended and melted, the melt is a homogeneous system, while the natural plant fiber filler cannot melt after heating and becomes a low potential energy point that is evenly dispersed in the homogeneous system. The gas generated by the decomposition of the foaming agent is easy to gather at the low potential energy point. When the gas gathering speed exceeds the dissolution and diffusion speed of the gas in the melt, bubble nuclei are formed. On the one hand, the natural plant fiber filler uniformly increases the number of bubble nuclei and plays a heterogeneous nucleation role. On the other hand, the polar groups contained in the natural plant fiber filler interact with the groups of polybutylene adipate / terephthalate (PBAT), hindering the movement of the polybutylene adipate / terephthalate (PBAT) molecular chain to a certain extent, increasing the melt viscosity, increasing the binding effect on the foaming gas, and reducing the escape of the foaming gas. Natural plant fiber fillers as solid particles hinder the diffusion and arrangement of polybutylene adipate / terephthalate (PBAT) molecular chain segments to the crystal nucleus, resulting in a decrease in the crystallization rate and an increase in the diffusion rate of the foaming agent, which is beneficial to the formation and diffusion of bubble nucleation.
[0068] In one embodiment, natural plant fiber fillers include wood powder (such as wood chips, sawdust, shavings, twigs, scraps, sanding powder, etc.), bamboo powder, straw and waste plant fibers. Because of their low cost, low density, renewable and degradable nature, they can avoid the pollution caused by the burning of abandoned crops and solve the problem of handling urban waste wood. They are an inevitable requirement for my country to develop a circular economy and build a conservation-oriented society, and are of great significance.
[0069] Furthermore, the mass percentage of the plant fiber filler is 20%; the mesh number of the plant fiber filler is 40-200 meshes, and preferably the mesh number of the plant fiber filler is 100 meshes.
[0070] In one embodiment, the 100-mesh plant fiber filler has good uniformity, processing performance, mechanical properties and other properties.
[0071] Specifically, the 100-mesh plant fiber filler has a uniform particle size, which helps to ensure the dispersibility and consistency of the plant fiber filler in the composite material, thereby obtaining more uniform physical and mechanical properties. The finer plant fiber filler particle size can increase its contact area with the biodegradable polymer, which helps to improve the adhesion between the plant fiber filler and the biodegradable polymer, thereby improving the overall performance of the composite material. In addition, due to its small particle size, the 100-mesh plant fiber filler can be more easily mixed and melted with the biodegradable polymer during processing, which helps to improve the processing performance of the composite material. Fine-grained plant fiber fillers can also better fill the voids in the composite material, which helps to improve the mechanical properties of the composite material, such as tensile strength, compressive strength and impact strength.
[0072] Furthermore, the use of 100-mesh plant fiber fillers can improve the surface quality of the composite material, making it smoother and improving the aesthetics of the product. Fine-grained plant fiber fillers may reduce the water absorption of the composite material because the smaller particle size helps to reduce the porosity in the material.
[0073] Furthermore, in one embodiment, the plant fiber filler is wood powder.
[0074] As a natural fiber, wood flour acts as a filler and nucleating agent. Due to its high rigidity, wood flour can improve melt strength, slow down melt deformation and mobility, thereby inhibiting excessive expansion of cells and controlling cell size. In addition to its good properties as a plant fiber filler, wood flour is more common in industrial applications, which can reduce costs and simplify the production process.
[0075] The invention uses thermoplastic biodegradable plastics and thermoplastic elastomers as matrix materials, especially polybutylene adipate / terephthalate (PBAT) and polyurethane thermoplastic elastomer (TPU) as matrix materials. Compared with traditional plastics, the packaging material of the invention is biodegradable. When polybutylene adipate / terephthalate (PBAT) and polyurethane thermoplastic elastomer (TPU) are blended, the melt strength of the blend is improved, and the blend has strong recoverable elastic deformation, can bind more foaming gas, reduce the escape of foaming gas, increase the diffusion rate of foaming gas, and increase the biaxial tensile force of the cell wall to withstand the cell growth, so it is beneficial to the formation of bubble nuclei, bubble growth, and stable solidification of bubbles, and greatly improves the expandability of the blend.
[0076] The present invention uses plant fibers from a wide range of sources, especially wood powder, as fillers and nucleating agents, and plastic reduction can reduce costs. Plant fibers as fillers can improve melt strength, but cannot be melted in a plastic homogeneous system to play a heterogeneous nucleation role, so it is conducive to the formation and diffusion of uniform bubble nuclei, and the material foaming is more uniform.
[0077] Furthermore, the present invention uses a physical foaming agent and a chemical foaming agent as a mixed foaming agent to achieve a synergistic foaming effect, so that the prepared degradable foaming packaging material has better resilience.
[0078] In the prior art, physical foaming is the use of physical principles to foam, such as dissolving gas or liquid in plastic and then expanding or vaporizing it. Chemical foaming is a method of using specially added chemical foaming agents to decompose under heat or chemical reactions between raw material components to produce gas, so that the plastic melt is filled with bubbles. However, the long saturation time in the physical foaming process will affect production efficiency, and rapid heating or rapid pressure relief has high requirements on energy and equipment safety. Chemical foaming agents are prone to produce more by-products when they decompose during the foaming process. For example, if the particle size is not fine enough, more by-products will be produced, resulting in the product having a taste and color deviation.
[0079] To solve the above problems, the present invention uses physical foaming agents and chemical foaming agents for synergistic foaming. The decomposition reaction of chemical foaming agents such as azodicarbonamide (AC) is an exothermic process with a fast decomposition rate. The heat suddenly released during the decomposition process causes local overheating of the melt, resulting in a decrease in the local viscosity of the melt. After the bubble is formed, since the pressure of the gas in the bubble is inversely proportional to the radius, the smaller the bubble, the higher the internal pressure. When two bubbles of different sizes approach, the gas diffuses from the small bubble to the large bubble to merge the bubbles, the bubble expansion expands the diameter of the pore, the pore wall membrane is thinned, the pore is easy to rupture, and the pore collapses. Physical foaming agents such as microsphere expansion agents (microsphere foaming agents) can absorb the heat released by the decomposition reaction of chemical foaming agents. When the microsphere expansion agent is heated, its thermoplastic shell softens, and at the same time, the volatile substances in its shell vaporize or decompose to form gas, which increases the internal pressure of the microspheres, causing the volume of the microspheres to expand, and the spherical cells formed in the shell. Because they are wrapped and fixed by the microsphere shell, the cells are closed cells with complete shape, small and uniform. When cooled, the thermoplastic shell hardens again, and the volume and shape of the microspheres are fixed. Therefore, the cells are not easy to merge and collapse, the equipment requirements are not high, the foaming process is simple, and the foamed material has good resilience.
[0080] In one embodiment, the chemical foaming agent includes one or a mixture of azobisisobutyronitrile (AIBN), azodicarbonamide (AC), hydrazine hydrogen sulfate (HSCN), dimethyl sulfate (DMS), isopentyl nitrite (IIPN), sodium bicarbonate, aluminum hydroxide, magnesium hydroxide or melamine.
[0081] The physical foaming agent can be a microsphere expansion agent and / or a microsphere foaming agent. The difference between different types of the physical foaming agent lies mainly in their different expansion temperatures. The required microsphere expansion agent can be determined according to the melting temperature of different materials.
[0082] Furthermore, the mixed foaming agent accounts for 2% to 8% of the weight of the base material, preferably 2%; the physical foaming agent accounts for 1% to 4% of the total weight of the mixed foaming agent, preferably the microsphere expansion agent is 2%; the chemical foaming agent accounts for 1% to 3% of the weight of the base material, preferably 2%.
[0083] Furthermore, the catalyst accounts for 1% to 3% of the weight of the base material, preferably 2%; the weight ratio of the chemical foaming agent to the catalyst is 4:1 to 1:1; preferably, the weight ratio of the chemical foaming agent azodicarbonamide (AC) to the catalyst zinc oxide (ZnO) is 1:1.
[0084] In a specific embodiment, when the weight ratio of the chemical foaming agent to the catalyst is 1:1, the decomposition temperature of the foaming agent is 160-175°C; when the weight ratio of the chemical foaming agent to the catalyst is 2:1, the decomposition temperature of the foaming agent is 170-180°C; when the weight ratio of the chemical foaming agent to the catalyst is 4:1, the decomposition temperature of the foaming agent is 180-190°C.
[0085] In specific implementation, different ratios of AC / ZnO have a great influence on the foaming temperature of AC, which is very important for adjusting the decomposition temperature of the foaming agent. The decomposition temperature of the chemical foaming agent should be higher than the melting temperature of the biodegradable polymer and lower than the degradation temperature of the plant fiber filler. The ratio of AC / ZnO should ensure that AC cannot decompose before the matrix melts, and the decomposition temperature cannot exceed the degradation temperature of the wood powder filler. A suitable AC / ZnO weight ratio can achieve better foaming effect.
[0086] In a second aspect, the present invention further provides a method for preparing a degradable high-resilience foam packaging material, which can be used to prepare the degradable high-resilience foam packaging material described in the first aspect of the present invention.
[0087] The preparation method comprises:
[0088] Step 1: According to a certain ratio, weigh a certain amount of biodegradable polymer and put it into a high-speed mixer to mix evenly;
[0089] Step 2: Spread the plant fiber filler evenly on the tray, dry it, weigh a certain amount of the dried plant fiber filler, add it into the high-speed mixer and continue to mix it evenly;
[0090] Step 3: Weigh a certain amount of chemical foaming agent and catalyst, mix them evenly, then add them into a high-speed mixer and continue to mix evenly;
[0091] Step 4: Weigh a certain amount of physical foaming agent and add it into a high-speed mixer and continue to mix evenly to obtain the final mixed material;
[0092] Step 5: Spread the final mixed material in a mold and put it into an oven for processing; the processing includes two stages, the first stage processing temperature is 140-150° C., the time is 10-20 minutes; the second stage processing temperature is 160-170° C., the time is 10-20 minutes;
[0093] Step 6: Take out the mold and cool it to room temperature. The material is cooled and solidified to obtain a foaming packaging material.
[0094] Furthermore, the method for preparing the degradable high-resilience foam packaging material is:
[0095] The drying temperature in step 2 is 100°C to 105°C, preferably 103°C;
[0096] The first stage processing temperature in step 5 is preferably 145° C. and the time is 15 min; the second stage processing temperature is preferably 165° C. and the time is 15 min.
[0097] In one embodiment, in the method for preparing a degradable high-resilience foam packaging material, the biodegradable polymer and the plant fiber filler are base materials; the composition and mass percentage of the base material are:
[0098] Biodegradable polymer 70%~90%,
[0099] Plant fiber filler 10% to 30%;
[0100] The foaming agent is a mixed foaming agent, including a physical foaming agent and a chemical foaming agent;
[0101] The catalyst includes zinc oxide.
[0102] Further, the biodegradable polymer includes a first biodegradable polymer and a second biodegradable polymer;
[0103] The first biodegradable polymer includes one or a mixture of polybutylene adipate / terephthalate (PBAT), polybutylene succinate (PBS), polylactic acid (PLA), polyhydroxyalkanoate (PHA), polycaprolactone (PCL), thermoplastic starch (TPS), and polycarbonate (PPC);
[0104] The second biodegradable polymer includes one or a mixture of styrene thermoplastic elastomer, polyurethane thermoplastic elastomer (TPU), polyolefin thermoplastic elastomer, polyamide thermoplastic elastomer (TPEA), ester thermoplastic elastomer (TPEE), organic fluorine thermoplastic elastomer (TPF), organic silicon thermoplastic elastomer or ethylene thermoplastic elastomer;
[0105] Preferably, the composition and mass percentage of the first biodegradable polymer and the second biodegradable polymer are:
[0106] The first biodegradable polymer is polybutylene adipate / terephthalate (PBAT) 40% to 80%;
[0107] The second biodegradable polymer is polyurethane thermoplastic elastomer (TPU) 10% to 50%.
[0108] In one embodiment, the plant fiber filler includes one or a mixture of wood powder, bamboo powder, straw or waste plant fibers;
[0109] Furthermore, the plant fiber filler is wood powder; preferably, the mass percentage of the wood powder is 20%; the mesh number of the wood powder is 40-200 meshes, and preferably the mesh number of the wood powder is 100 meshes.
[0110] In one embodiment, the chemical foaming agent includes one or a mixture of azobisisobutyronitrile (AIBN), azodicarbonamide (AC), hydrazine hydrogen sulfate (HSCN), dimethyl sulfate (DMS), isopentyl nitrite (IIPN), sodium bicarbonate, aluminum hydroxide, magnesium hydroxide or melamine. The physical foaming agent includes a microsphere expansion agent and / or a microsphere foaming agent.
[0111] Furthermore, the mixed foaming agent accounts for 2% to 8% of the weight of the base material, preferably 2%; the microsphere expansion agent accounts for 1% to 4% of the total weight of the mixed foaming agent, preferably 2%; the chemical foaming agent accounts for 1% to 3% of the weight of the base material, preferably 2%.
[0112] Furthermore, the catalyst accounts for 1% to 3% by weight of the base material, preferably 2%; and the weight ratio of the chemical foaming agent to the catalyst is 4:1 to 1:1.
[0113] In a specific embodiment, a method for preparing a degradable foam packaging material comprises the following steps:
[0114] Step 1: Weigh a certain amount of PBAT and TPU according to a certain ratio, put them into a high-speed mixer and mix them evenly;
[0115] Step 2: Spread the wood powder filler evenly on the tray, weigh a certain amount of wood powder after drying, add it into the high-speed mixer and continue to mix evenly;
[0116] Step 3: Weigh a certain amount of AC and ZnO, mix them evenly, then add them into a high-speed mixer and continue mixing evenly;
[0117] Step 4: Weigh a certain amount of microsphere expansion agent and add it into a high-speed mixer and continue to mix evenly to obtain the final mixed material;
[0118] Step 5: Spread the final mixed material in a mold and put it into an oven for processing; the processing includes two stages, the first stage processing temperature is 145°C, the time is 15 minutes; the second stage processing temperature is 165°C, the time is 15 minutes, the temperature of the mixed material reaches the decomposition temperature of the AC foaming agent and the expansion temperature of the microsphere expansion agent, and the foaming is completed under the synergistic effect of AC and the microsphere expansion agent;
[0119] Step 6: Take out the mold and cool it to room temperature to cool and solidify the material to obtain a degradable foam packaging material.
[0120] In the above preparation steps, TPU is added to improve the melt strength of the matrix material after melting. PBAT and TPU are first added to the high-speed mixer for mixing, and then the wood powder is poured into the high-speed mixer for further mixing. The wood powder is used as a filler and nucleating agent and is evenly distributed in the matrix material. Finally, the foaming agent is poured into the high-speed mixer for further mixing.
[0121] The preparation method described in the present invention adopts a one-step segmented molding in a hot press. In the first stage, the substrate is heated and melted without the decomposition of the foaming agent, and the melt strength of the substrate is improved. In the second stage, the foaming agent is decomposed in the molten substrate and fully foamed. At the same time, the temperature of each stage is related to the substrate material, the amount of modified TPU added, the degradation temperature and amount of wood powder, the AC / ZnO ratio, etc., and is an unconventional choice. The temperature of the first stage depends on the ratio of the substrate material and the ratio of AC / ZnO, which is higher than the melting temperature of the substrate material and lower than the decomposition temperature of AC; the temperature of the second stage depends on the melting temperature of the substrate material, the degradation temperature of the wood powder, and the AC / zinc oxide ratio, which is higher than the melting temperature of the substrate material and the decomposition temperature of AC, and at the same time lower than the degradation temperature of the wood powder.
[0122] The preparation method of the present application does not require modification of the material before hot pressing, and the preparation process is highly efficient.
[0123] The present invention provides three different specific embodiments. Figure 2-6 As shown, according to GB / T8168-2008, the material is sampled, its density and expansion ratio are calculated, the sample pore morphology is analyzed using a stereo microscope, and a universal testing machine is used to perform a compression test to obtain a ten-cycle compression curve of the material. The specific material performance data is shown in Table 1.
[0124] The following are the component contents of 3 embodiments:
[0125] Example 1
[0126] Wood flour 10%, PBAT 80%, TPU 10%, microsphere expansion agent 1%, AC 1%, ZnO 1%.
[0127] Example 2
[0128] Wood flour 20%, PBAT 60%, TPU 20%, microsphere expansion agent 2%, AC 2%, ZnO 2%.
[0129] Example 3
[0130] Wood flour 30%, PBAT 40%, TPU 30%, microsphere expansion agent 4%, AC 3%, ZnO 3%.
[0131] Table 1 Material performance data table
[0132]
[0133] It can be seen from the material performance data of the above specific embodiments that the amount of mixed foaming agent added has a great influence on the foaming ratio, density and resilience of the material. The material obtained by AC foaming has a higher foaming ratio, a lower density and a much improved resilience. In addition, the addition of wood powder can play a heterogeneous nucleation role, increase the number of crystallization nucleation points, and is more conducive to the formation of bubble nuclei, and the bubbles formed are more and more uniform. The degradable high-resilience foaming packaging material of the present invention can be widely used in the packaging fields of industries such as industry, express delivery, food, and daily chemicals.
[0134] The degradable high-resilience foam packaging material and the preparation method thereof according to the first and second aspects of the present invention have at least one of the following advantages:
[0135] 1. The present invention uses thermoplastic biodegradable plastics and thermoplastic elastomers as matrix materials, especially polybutylene adipate / terephthalate (PBAT) and polyurethane thermoplastic elastomer (TPU) as matrix materials. Compared with traditional plastics, the packaging material of the present invention is biodegradable; when polybutylene adipate / terephthalate (PBAT) and polyurethane thermoplastic elastomer (TPU) are blended, the melt strength of the blend is improved, and it has a strong recoverable elastic deformation, which can bind more foaming gas, reduce the escape of foaming gas, increase the diffusion rate of foaming gas, and increase the biaxial tensile force of the cell wall to withstand the cell growth, so it is beneficial to the formation of bubble nuclei, bubble growth, and stable solidification of bubbles, and greatly improves the expandability of the blend.
[0136] Second, the present invention uses plant fibers from a wide range of sources, especially wood powder, as fillers and nucleating agents, and plastic reduction can reduce costs. Plant fibers as fillers can increase melt strength, but cannot melt in the plastic homogeneous system to play a heterogeneous nucleation role, which is conducive to the formation and diffusion of uniform bubble nuclei, and the material foaming is more uniform.
[0137] 3. The present invention uses physical foaming agents and chemical foaming agents for synergistic foaming, and the prepared material has high resilience.
[0138] Fourth, the preparation method of the present invention adopts a one-step molding method. There is no need to modify the materials before preparation. The raw materials are mixed evenly and then placed in a mold and heated at high temperature. The preparation process is simple and efficient.
[0139] Although some embodiments of the present general inventive concept have been shown and described, it will be appreciated by those skilled in the art that changes may be made to these embodiments without departing from the principles and spirit of the present general inventive concept, the scope of which is defined by the claims and their equivalents.
Claims
1. A degradable high-resilience foam packaging material, characterized in that: It includes a base material, a foaming agent and a catalyst; the composition and mass percentage of the base material are: Biodegradable polymer 70%~90%, Plant fiber filler 10% to 30%; The foaming agent is a mixed foaming agent, including a physical foaming agent and a chemical foaming agent; The catalyst includes zinc oxide.
2. The degradable high-resilience foam packaging material according to claim 1, characterized in that: The biodegradable polymer includes a first biodegradable polymer and a second biodegradable polymer; The first biodegradable polymer includes one or a mixture of polybutylene adipate / terephthalate (PBAT), polybutylene succinate (PBS), polylactic acid (PLA), polyhydroxyalkanoate (PHA), polycaprolactone (PCL), thermoplastic starch (TPS), and polycarbonate (PPC); The second biodegradable polymer includes one or a mixture of styrene-based thermoplastic elastomer, polyurethane-based thermoplastic elastomer (TPU), polyolefin-based thermoplastic elastomer, polyamide-based thermoplastic elastomer (TPEA), ester-based thermoplastic elastomer (TPEE), organic fluorine-based thermoplastic elastomer (TPF), organic silicon-based thermoplastic elastomer or ethylene-based thermoplastic elastomer.
3. The degradable high-resilience foam packaging material according to claim 2, characterized in that: The composition and mass percentage of the first biodegradable polymer and the second biodegradable polymer are: The first biodegradable polymer is 40% to 80% polybutylene adipate / terephthalate; The second biodegradable polymer is polyurethane thermoplastic elastomer (TPU) 10% to 50%.
4. The degradable high-resilience foam packaging material according to claim 1, characterized in that: The plant fiber filler includes one or a mixture of wood powder, bamboo powder, straw or waste plant fibers; Preferably, the mass percentage of the plant fiber filler is 20%; the mesh number of the plant fiber filler is 40-200 meshes, preferably the mesh number of the plant fiber filler is 100 meshes; Preferably, the plant fiber filler is wood powder.
5. The degradable high-resilience foam packaging material according to claim 1, characterized in that: The chemical foaming agent includes one or a mixture of azobisisobutyronitrile (AIBN), azodicarbonamide (AC), hydrazine hydrogen sulfate (HSCN), dimethyl sulfate (DMS), isopentyl nitrite (IIPN), sodium bicarbonate, aluminum hydroxide, magnesium hydroxide or melamine.
6. The degradable high resilience foam packaging material according to claim 1, characterized in that: The mixed foaming agent accounts for 2% to 7% of the weight of the base material, preferably 2%; the physical foaming agent accounts for 1% to 4% of the total weight of the mixed foaming agent, preferably 2%; the chemical foaming agent accounts for 1% to 3% of the weight of the base material, preferably 2%.
7. The degradable high-resilience foam packaging material according to claim 6, characterized in that: The physical foaming agent includes a microsphere expansion agent and / or a microsphere foaming agent.
8. The degradable high-resilience foam packaging material according to claim 1, characterized in that: The catalyst accounts for 1% to 3% of the weight of the base material, preferably 2%; the weight ratio of the chemical foaming agent to the catalyst is 4:1 to 1:
1.
9. A method for preparing a degradable high-resilience foam packaging material according to any one of claims 1 to 8, characterized in that: The preparation method comprises: Step 1: According to a certain ratio, weigh a certain amount of biodegradable polymer and put it into a high-speed mixer to mix evenly; Step 2: Spread the plant fiber filler evenly on the tray, dry it, weigh a certain amount of the dried plant fiber filler, add it into the high-speed mixer and continue to mix it evenly; Step 3: Weigh a certain amount of chemical foaming agent and catalyst, mix them evenly, then add them into a high-speed mixer and continue to mix evenly; Step 4: Weigh a certain amount of physical foaming agent and add it into a high-speed mixer and continue to mix evenly to obtain the final mixed material; Step 5: Spread the final mixed material in a mold and put it into an oven for processing; the processing includes two stages, the first stage processing temperature is 140-150° C., the time is 10-20 minutes; the second stage processing temperature is 160-170° C., the time is 10-20 minutes; Step 6: Take out the mold and cool it to room temperature. The material is cooled and solidified to obtain a foaming packaging material.
10. The method for preparing a degradable high-resilience foam packaging material according to claim 9, characterized in that: The drying temperature in step 2 is 100°C to 110°C, preferably 103°C; The first stage processing temperature in step 5 is preferably 145° C. and the time is 15 minutes; the second stage processing temperature is preferably 165° C. and the time is 15 minutes.
Citation Information
Cited By
Degradable expandable polylactic acid polymer foam material and preparation method thereof
CN119463439A