Cutter coating suitable for titanium alloy machining, preparation method of cutter coating and cutter
Through multi-layer structure coating design and alloying control, the problem of insufficient high temperature resistance and anti-adhesion of tool coatings in titanium alloy processing is solved, the tool life is extended and the wear is reduced, and the overall coating quality is improved. performance.
Patent Information
- Application Number
- CN202411073457.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-08-06
AI Technical Summary
Existing tool coatings have insufficient high temperature resistance, adhesive wear resistance, toughness and adhesion in titanium alloy processing, resulting in shortened tool life.
A multi-layer structural coating design is adopted, including the bottom layer, the sub-bottom layer, the sub-top layer and the top layer. W, Mo, V, Si and B elements are incorporated into the AlTiN and AlCrN coatings through alloying control to form a Magnéli phase and fine-grained structure. , combining the characteristics of AlCrMN, TiSiN and AlTiMeN, using TX material with good anti-adhesion properties as the top layer, and deposited using cathodic arc technology.
It significantly improves the cutting life of the tool, reduces the amount of wear, enhances the wear resistance, toughness and anti-adhesion of the coating, and extends the service life of the tool.
Smart Images

Figure CN118756100A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of surface engineering and numerical control tool cutting, and in particular relates to a tool coating suitable for titanium alloy processing, a preparation method thereof, and a tool. Background Art
[0002] Titanium alloys are widely used in aerospace, defense, petrochemical, biomedicine and other fields due to their light weight and high strength. Although the development of CNC cutting and grinding technology has made titanium alloy processing technology increasingly mature and ensured processing accuracy, the low thermal conductivity, high hardness and high chemical affinity of titanium alloys still lead to tool adhesion and chipping problems during cutting.
[0003] At present, traditional coated tools are not suitable for titanium alloy processing because the high affinity of the Ti element in the coating and titanium alloy (TiN, AlTiN, AlCrN) leads to rapid tool failure. However, with the continuous innovation of coating technology, such as the emergence of new coatings such as soft coatings, superhard coatings, multilayer coatings and nano-composite coatings, the application of coated tools in titanium alloy processing has gradually increased and shown obvious advantages. Summary of the invention
[0004] The present invention overcomes at least one of the limitations of existing tool coatings in terms of high temperature resistance, adhesive wear resistance, toughness and adhesion, and in particular the problem of shortened tool life caused by these limitations. Therefore, the tool coating provided by the present invention is particularly suitable for titanium alloy processing, which not only significantly improves the cutting life of the tool, but also effectively reduces the amount of wear.
[0005] The present invention solves the above technical problems through the following technical solutions.
[0006] The present invention provides a tool coating suitable for titanium alloy processing, wherein the coating structure comprises one of the following (a) or (b);
[0007] (a) bottom layer, second bottom layer, second top layer and top layer;
[0008] (b) bottom layer and top layer;
[0009] Wherein, the bottom layer is (Al a Cr b M 1-a-b )N;
[0010] The sub-bottom layer is (Al c Ti d Me 1-c-d )N / (Al a Cr b M 1-a-b )N / (Ti e Si1-e )N loop layers;
[0011] The second top layer is (Ti e Si 1-e )N / (Al c Ti d Me 1-c-d )N loop layers;
[0012] The top layer is TX;
[0013] M is at least one of W, Mo, V, Si, and B;
[0014] Me is at least one of W, Mo, V, Si and B;
[0015] T is at least one of Zr, Nb and Cr;
[0016] X is at least one of N, C, and CN;
[0017] 0.4≤a≤0.8, 0.2≤b≤0.5, 1-ab≥0;
[0018] 0.4≤c≤0.7, 0.3≤d≤0.6, 1-cd≥0;
[0019] 0.5≤e≤0.9.
[0020] Preferably, 0.6≤a≤0.8, 0.2≤b≤0.4, 1-ab≥0;
[0021] 0.4≤c≤0.6, 0.3≤d≤0.5, 1-cd≥0;
[0022] 0.6≤e≤0.9.
[0023] More preferably, 0.6≤a≤0.7, 0.2≤b≤0.35, 1-ab≥0;
[0024] 0.45≤c≤0.6, 0.3≤d≤0.45, 1-cd≥0;
[0025] 0.8≤e≤0.9.
[0026] a~e, 1-ab, 1-cd, and 1-e are all atomic ratios.
[0027] Among them, (Al a Cr b M 1-a-b )Al in N a Cr b M 1-a-b The molar ratio of Al to N is 1:1; c Ti dMe 1-c-d The molar ratio of Ti to N is 1:1; e Si 1-e The molar ratio of N to N is 1:1.
[0028] The addition of W, Mo, and V elements in the present invention enables the coating to generate Magnéli phases during the tribological process, reduces the friction coefficient, provides a good lubrication effect, and thus improves the wear resistance of the coating. The addition of Si and B elements can generate a nanocrystalline AlTiN or AlCrN coating wrapped by amorphous BN or SiN, thereby achieving a fine grain strengthening effect, improving the hardness and toughness of the coating, and extending the life of the coated tool.
[0029] In the present invention, the substrate selected for the tool coating is a CNC blade made of cemented carbide or ceramic material.
[0030] Furthermore, the hardness of the substrate is 1300-1500 HV 30 .
[0031] In the present invention, the thickness of the coating is 1.5 to 4.0 μm, preferably 2.0 to 4.0 μm.
[0032] In the present invention, the thickness of the bottom layer is 0.2-3.5 μm, preferably 0.2-3.1 μm.
[0033] In the present invention, the thickness of the sub-bottom layer is 0.8-1.5 μm, preferably 0.9-1.5 μm.
[0034] In the present invention, the thickness of the sub-top layer is 0.8-1.5 μm, preferably 0.9-1.5 μm.
[0035] In the present invention, the thickness of the top layer is 0.2-1.5 μm, preferably 0.2-1.0 μm.
[0036] In the present invention, the ratio of the thickness of the sub-bottom layer to the sub-top layer is 0.5-2:1, preferably 0.6-1.5:1.
[0037] In the present invention, the bottom layer is composed of (Al a Cr b M 1-a-b )N deposition formed.
[0038] In the present invention, the sub-bottom layer is composed of (Al c Ti d Me 1-c-d )N、(Al a Cr b M 1-a-b )N and (Ti e Si1-e )N three layers are deposited alternately in sequence.
[0039] In the present invention, the sub-top layer is (Ti e Si 1-e )N and (Al c Ti d Me 1-c-d )N two layers are deposited alternately in sequence.
[0040] In the present invention, the top layer is formed by TX deposition.
[0041] In the present invention, the bottom layer is a single-layer structure.
[0042] In the present invention, the top layer is a single-layer structure.
[0043] In the present invention, the number of cycles of the sub-bottom layer is 0 to 180 layers, wherein (Al c Ti d Me 1-c-d )N / (Al a Cr b M 1-a-b )N / (Ti e Si 1-e )N is a recurrent layer.
[0044] In the present invention, the number of cycles of the sub-top layer is 0 to 200 layers, wherein (Ti e Si 1-e )N / (Al c Ti d Me 1-c-d )N is a recurrent layer.
[0045] In the present invention, the innermost layer of the sub-bottom layer is (Al c Ti d Me 1-c-d )N.
[0046] In the present invention, the outermost layer of the sub-bottom layer is (Ti e Si 1-e )N.
[0047] In the present invention, the innermost layer of the sub-top layer is (Ti e Si 1-e )N.
[0048] In the present invention, the outermost layer of the sub-top layer is (Al c Ti d Me 1-c-d )N.
[0049] In the present invention, the outermost layer of the sub-bottom layer and the innermost layer of the sub-top layer have the same chemical composition.
[0050] In the present invention, the innermost layer of the sub-bottom layer and the outermost layer of the sub-top layer have the same chemical composition.
[0051] The present invention also provides a method for preparing the tool coating suitable for titanium alloy processing, wherein the coating is formed by vapor deposition.
[0052] In the present invention, the vapor deposition adopts cathode arc technology.
[0053] In the present invention, the reaction gas for the vapor deposition is at least one of nitrogen and acetylene.
[0054] In the present invention, the arc current of the arc source of the vapor deposition is 150-200A, preferably 200A.
[0055] In the present invention, the bias voltage for depositing the bottom layer and the top layer in the vapor deposition is -40 to -80V, preferably -40V.
[0056] In the present invention, the bias voltage for depositing the sub-bottom layer and the sub-top layer in the vapor deposition is -30 to -100V, preferably -80V.
[0057] In the present invention, the deposition temperature in the vapor deposition is 400-500°C, preferably 500°C.
[0058] In the present invention, the purity of the target material used in the vapor deposition is ≥99.8%.
[0059] In the present invention, the target material for depositing the bottom layer is Al a Cr b M 1-a-b alloy.
[0060] In the present invention, the target material for depositing the sub-bottom layer is Al c Ti d Me 1-c-d Alloy, Al a Cr b M 1-a-b Alloy and Ti e Si 1-e alloy.
[0061] In the present invention, the target material for depositing the second top layer is Ti e Si 1-e Alloy and Al c Ti d Me 1-c-d alloy.
[0062] In the present invention, the target material for depositing the top layer is metal T.
[0063] A cutting tool comprises the aforementioned cutting tool coating suitable for titanium alloy processing.
[0064] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0065] Compared with the prior art, the present invention has the following beneficial effects:
[0066] 1. The present invention uses cathode arc technology to deposit tool coatings, and successfully incorporates alloying elements Me and M into AlTiN and AlCrN coatings through alloying control means to form AlTiMeN and AlCrMN coatings, respectively. Among them, the addition of W, Mo and V elements can promote the formation of Magnéli phase in the coating, which has excellent lubrication properties and helps to reduce friction and wear. At the same time, the doping of S and B elements can refine the grains, which not only enhances the hardness of the coating, but also improves its toughness.
[0067] 2. The present invention develops a four-layer structure coating, and this design makes full use of the characteristics of three coatings: AlCrMN, TiSiN and AlTiMeN. Although AlCrMN has poor thermal stability, it has excellent high temperature resistance. The Cr2O3 layer formed on the surface after high temperature oxidation is relatively dense and can effectively slow down the oxidation process. The AlTiMeN coating has good thermal stability, but relatively poor high temperature resistance. The TiSiN coating has good high temperature resistance, but the TiO2 layer formed after high temperature oxidation is loose and porous, and cannot effectively prevent oxygen from invading. It needs to rely on the nano-composite structure of the bottom layer to slow down the oxidation process. From the bottom layer to the sub-top layer, the coating structure is macroscopically manifested as a gradual decrease in the AlCrMN component, while the AlTiMeN and TiSiN components gradually increase. Specifically, the bottom layer AlCrMN coating not only provides good adhesion, but also serves as the last barrier to protect the substrate, with low stress and high temperature oxidation resistance. The sub-bottom layer combines the thermal stability of AlTiMeN, the high temperature resistance of AlCrMN and the high hardness of TiSiN, and effectively coordinates these three characteristics through a nano multilayer structure. The design logic of the sub-top layer is similar to that of the sub-bottom layer, which further optimizes the performance of the coating. This structural design enables the coating to maintain good adhesion while integrating the advantages of various materials to improve the overall performance of the coating, especially in applications under high temperature environments.
[0068] 3. In order to further improve the overall performance of the coating, the present invention specifically uses TX with anti-adhesion properties as the top coating. Due to its excellent chemical stability, TX material is not easy to chemically react or melt weld with titanium (Ti) metal during the cutting process, thereby effectively preventing adhesion between materials. This anti-adhesion property is crucial to improving the service life of cutting tools and maintaining cleanliness during the cutting process. By applying TX material to the top layer of the coating structure, not only the durability of the coating is enhanced, but it also helps to maintain the stability and performance of the cutting tool under high temperature and high pressure environments.
[0069] 4. The coating of the present invention not only exhibits excellent chipping resistance, wear resistance and adhesion resistance, but also significantly improves the service life of the tool. The cutting life of the tool containing the coating of the present invention is 188 to 240 minutes; in some preferred embodiments, the cutting life can reach 210 to 240 minutes; in more preferred embodiments, the cutting life can reach 216 to 240 minutes. BRIEF DESCRIPTION OF THE DRAWINGS
[0070] Figure 1 Schematic diagram of tool coating structure.
[0071] Figure 2 This is a scanning electron microscope image of the tool coating of Example 15. DETAILED DESCRIPTION
[0072] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and carefully in combination with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.
[0073] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0074] The "range" disclosed in the present invention is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of a particular range. The range defined in this way can be inclusive or exclusive of end values, and can be combined arbitrarily, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60-120 and 80-110 is listed for a specific parameter, it is understood that the range of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present invention, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" represents that all real numbers between "0-5" have been fully listed herein, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0075] If not otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form a new technical solution.
[0076] Unless otherwise specified, all technical features and optional technical features of the present invention can be combined with each other to form a new technical solution.
[0077] If not otherwise specified, all steps of the present invention may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0078] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0079] If not specifically stated, in the present invention, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0080] Figure 1 Schematic diagram of coating structure, in which: L1 is the bottom layer, L2 is the sub-bottom layer, L3 is the sub-top layer, and L4 is the top layer.
[0081] The base material is selected with a hardness of 1420HV 30 Carbide CNC blades.
[0082] In L2, (Al c Ti d Me 1-c-d )N / (Al a Cr b M 1-a-b )N / (Ti e Si 1-e )The number of cycles of the N cycle layer is m times, m=0~180.
[0083] In L3, (Ti e Si 1-e )N / (Al c Ti d Me 1-c-d )The number of cycles of the N cycle layer is n, n=0~200.
[0084] The deposition conditions of the following examples and comparative examples are as follows:
[0085] 1) Deposition technology: cathode arc technology;
[0086] 2) Deposition pressure: 3.5Pa;
[0087] 3) Reaction gas: nitrogen, acetylene, different reaction gases are selected according to different TX in the top layer of each embodiment and comparative example;
[0088] When X is N, nitrogen is selected; when X is C, acetylene is selected; when X is CN, a mixed gas of acetylene and nitrogen is selected.
[0089] 4) Deposition bias: The bias for depositing the bottom and top layers is -40V, and the bias for depositing the second bottom and second top layers is -80V;
[0090] 5) Target current: The arc current of each arc source is 200A;
[0091] 6) Deposition temperature: 500°C.
[0092] Example 1
[0093] The tool coating suitable for titanium alloy processing in this embodiment consists of a bottom layer and a top layer, and the thickness of the coating is 3.2 μm.
[0094] 1. Structure of each coating:
[0095] The bottom layer is (Al 0.7 Cr 0.3 )N.
[0096] The top layer is ZrN.
[0097] The thickness of the bottom layer was 2.8 μm.
[0098] The thickness of the top layer was 0.4 μm.
[0099] 2. Preparation methods of each coating:
[0100] The target material for depositing the bottom layer is Al 0.7 Cr 0.3 alloy.
[0101] The target material for depositing the top layer is metal Zr.
[0102] Example 2
[0103] The tool coating suitable for titanium alloy processing in this embodiment consists of a bottom layer and a top layer, and the thickness of the coating is 3.0 μm.
[0104] 1. Structure of each coating:
[0105] The bottom layer is (Al 0.7 Cr 0.3 )N.
[0106] The top layer is NbN.
[0107] The thickness of the bottom layer was 2.7 μm.
[0108] The thickness of the top layer was 0.3 μm.
[0109] 2. Preparation methods of each coating:
[0110] The target material for depositing the bottom layer is Al 0.7 Cr 0.3 alloy.
[0111] The target material for depositing the top layer is metallic Nb.
[0112] Example 3
[0113] The tool coating suitable for titanium alloy processing in this embodiment consists of a bottom layer and a top layer, and the thickness of the coating is 3.8 μm.
[0114] 1. Structure of each coating:
[0115] The bottom layer is (Al 0.7 Cr 0.3 )N.
[0116] The top layer is CrN.
[0117] The thickness of the bottom layer was 3.0 μm.
[0118] The thickness of the top layer was 0.8 μm.
[0119] 2. Preparation methods of each coating:
[0120] The target material for depositing the bottom layer is Al 0.7 Cr 0.3 alloy.
[0121] The target material for depositing the top layer is metal Cr.
[0122] Example 4
[0123] The tool coating suitable for titanium alloy processing in this embodiment consists of a bottom layer and a top layer, and the thickness of the coating is 2.8 μm.
[0124] 1. Structure of each coating:
[0125] The bottom layer is (Al 0.7 Cr 0.3 )N.
[0126] The top layer is CrCN.
[0127] The thickness of the bottom layer was 2.1 μm.
[0128] The thickness of the top layer was 0.7 μm.
[0129] 2. Preparation methods of each coating:
[0130] The target material for depositing the bottom layer is Al 0.7 Cr 0.3 alloy.
[0131] The target material for depositing the top layer is metal Cr.
[0132] Example 5
[0133] The tool coating suitable for titanium alloy processing in this embodiment consists of a bottom layer and a top layer, and the thickness of the coating is 2.8 μm.
[0134] 1. Structure of each coating:
[0135] The bottom layer is (Al 0.63 Cr 0.27 V 0.1 )N.
[0136] The top layer is ZrN.
[0137] The thickness of the bottom layer was 2.3 μm.
[0138] The thickness of the top layer was 0.5 μm.
[0139] 2. Preparation methods of each coating:
[0140] The target material for depositing the bottom layer is Al 0.63 Cr 0.27 V 0.1 alloy.
[0141] The target material for depositing the top layer is metal Zr.
[0142] Example 6
[0143] The tool coating suitable for titanium alloy processing in this embodiment consists of a bottom layer and a top layer, and the thickness of the coating is 3.2 μm.
[0144] 1. Structure of each coating:
[0145] The bottom layer is (Al 0.63 Cr 0.27 Si 0.1 )N.
[0146] The top layer is ZrN.
[0147] The thickness of the bottom layer was 2.7 μm.
[0148] The thickness of the top layer was 0.5 μm.
[0149] 2. Preparation methods of each coating:
[0150] The target material for depositing the bottom layer is Al 0.63 Cr 0.27 Si 0.1 alloy.
[0151] The target material for depositing the top layer is metal Zr.
[0152] Example 7
[0153] The tool coating suitable for titanium alloy processing in this embodiment consists of a bottom layer and a top layer, and the thickness of the coating is 3.4 μm.
[0154] 1. Structure of each coating:
[0155] The bottom layer is (Al 0.63 Cr 0.27 B 0.1 )N.
[0156] The top layer is ZrN.
[0157] The thickness of the bottom layer was 3.1 μm.
[0158] The thickness of the top layer was 0.3 μm.
[0159] 2. Preparation methods of each coating:
[0160] The target material for depositing the bottom layer is Al 0.63 Cr 0.27 B 0.1 alloy.
[0161] The target material for depositing the top layer is metal Zr.
[0162] Example 8
[0163] The tool coating suitable for titanium alloy processing in this embodiment consists of a bottom layer and a top layer, and the thickness of the coating is 2.4 μm.
[0164] 1. Structure of each coating:
[0165] The bottom layer is (Al 0.63 Cr 0.27 Si 0.067 W 0.033 )N.
[0166] The top layer is ZrN.
[0167] The thickness of the bottom layer was 2.0 μm.
[0168] The thickness of the top layer was 0.4 μm.
[0169] 2. Preparation methods of each coating:
[0170] The target material for depositing the bottom layer is Al 0.63 Cr 0.27 Si 0.067 W 0.033 alloy.
[0171] The target material for depositing the top layer is metal Zr.
[0172] Example 9
[0173] The tool coating suitable for titanium alloy processing in this embodiment consists of a bottom layer, a sub-bottom layer, a sub-top layer and a top layer, and the thickness of the coating is 3.7 μm.
[0174] 1. Structure of each coating:
[0175] The bottom layer is (Al 0.7 Cr 0.3 )N.
[0176] The sub-bottom layer is (Al 0.6 Ti 0.3 B 0.1 )N / (Al 0.7 Cr 0.3 )N / (Ti 0.85 Si 0.15 )N recurrent layers.
[0177] The second top layer is (Ti 0.85 Si 0.15 )N / (Al 0.6 Ti 0.3 B 0.1 )N loop layers;
[0178] The top layer is ZrN.
[0179] The thickness of the bottom layer was 0.4 μm.
[0180] The thickness of the sub-bottom layer was 1.1 μm.
[0181] The thickness of the sub-top layer was 1.1 μm.
[0182] The thickness of the top layer was 1.1 μm.
[0183] The ratio of the thickness of the sub-bottom layer to the sub-top layer is 1:1.
[0184] The number of circulation layers of the sub-bottom layer is 90 layers.
[0185] The number of circulation layers of the second top layer is 150.
[0186] 2. Preparation methods of each coating:
[0187] The target material for depositing the bottom layer is Al 0.7 Cr 0.3 alloy.
[0188] The target material for depositing the sub-bottom layer is Al 0.6 Ti 0.3 B 0.1 Alloy, Al 0.7 Cr 0.3 Alloy, Ti 0.85 Si 0.15 alloy.
[0189] The target material for depositing the second top layer is Al 0.6 Ti 0.3 B 0.1 Alloy, Ti 0.85 Si0.15 alloy.
[0190] The target material for depositing the top layer is metal Zr.
[0191] Example 10
[0192] The tool coating suitable for titanium alloy processing in this embodiment consists of a bottom layer, a sub-bottom layer, a sub-top layer and a top layer, and the thickness of the coating is 3.6 μm.
[0193] 1. Structure of each coating:
[0194] The bottom layer is (Al 0.7 Cr 0.3 )N.
[0195] The sub-bottom layer is (Al 0.6 Ti 0.3 B 0.1 )N / (Al 0.7 Cr 0.3 )N / (Ti 0.85 Si 0.15 )N recurrent layers.
[0196] The second top layer is (Ti 0.85 Si 0.15 )N / (Al 0.6 Ti 0.3 B 0.1 )N recurrent layers.
[0197] The top layer is ZrN.
[0198] The thickness of the bottom layer was 0.5 μm.
[0199] The thickness of the sub-bottom layer is 1.5 μm.
[0200] The thickness of the sub-top layer was 1.0 μm.
[0201] The thickness of the top layer was 0.6 μm.
[0202] The thickness ratio of the sub-bottom layer to the sub-top layer is 1.5:1.
[0203] The number of circulation layers of the sub-bottom layer is 60 layers.
[0204] The number of circulation layers of the second top layer is 100.
[0205] 2. Preparation methods of each coating:
[0206] The target material for depositing the bottom layer is Al 0.7 Cr 0.3 alloy.
[0207] The target material for depositing the sub-bottom layer is Al0.6 Ti 0.3 B 0.1 Alloy, Al 0.7 Cr 0.3 Alloy, Ti 0.85 Si 0.15 alloy.
[0208] The target material for depositing the second top layer is Al 0.6 Ti 0.3 B 0.1 Alloy, Ti 0.85 Si 0.15 alloy.
[0209] The target material for depositing the top layer is metal Zr.
[0210] Embodiment 11
[0211] The tool coating suitable for titanium alloy processing in this embodiment consists of a bottom layer, a sub-bottom layer, a sub-top layer and a top layer, and the thickness of the coating is 3.8 μm.
[0212] 1. Structure of each coating:
[0213] The bottom layer is (Al 0.7 Cr 0.3 )N.
[0214] The sub-bottom layer is (Al 0.6 Ti 0.3 B 0.1 )N / (Al 0.7 Cr 0.3 )N / (Ti 0.85 Si 0.15 )N recurrent layers.
[0215] The second top layer is (Ti 0.85 Si 0.15 )N / (Al 0.6 Ti 0.3 B 0.1 )N recurrent layers.
[0216] The top layer is ZrN.
[0217] The thickness of the bottom layer was 0.3 μm.
[0218] The thickness of the sub-bottom layer was 1.0 μm.
[0219] The thickness of the sub-top layer was 1.5 μm.
[0220] The thickness of the top layer was 1.0 μm.
[0221] The thickness ratio of the sub-bottom layer to the sub-top layer is 1:1.5.
[0222] The number of circulation layers of the sub-bottom layer is 30.
[0223] The number of circulation layers of the second top layer is 50.
[0224] 2. Preparation methods of each coating:
[0225] The target material for depositing the bottom layer is Al 0.7 Cr 0.3 alloy.
[0226] The target material for depositing the sub-bottom layer is Al 0.6 Ti 0.3 B 0.1 Alloy, Al 0.7 Cr 0.3 Alloy, Ti 0.85 Si 0.15 alloy.
[0227] The target material for depositing the second top layer is Al 0.6 Ti 0.3 B 0.1 Alloy, Ti 0.85 Si 0.15 alloy.
[0228] The target material for depositing the top layer is metal Zr.
[0229] Example 12
[0230] The tool coating suitable for titanium alloy processing in this embodiment consists of a bottom layer, a sub-bottom layer, a sub-top layer and a top layer, and the thickness of the coating is 3.8 μm.
[0231] 1. Structure of each coating:
[0232] The bottom layer is (Al 0.7 Cr 0.3 )N.
[0233] The sub-bottom layer is (Al 0.6 Ti 0.3 W 0.1 )N / (Al 0.7 Cr 0.3 )N / (Ti 0.85 Si 0.15 )N recurrent layers.
[0234] The second top layer is (Ti 0.85 Si 0.15 )N / (Al 0.6 Ti 0.3 W 0.1 )N recurrent layers.
[0235] The top layer is ZrN.
[0236] The thickness of the bottom layer was 0.5 μm.
[0237] The thickness of the sub-bottom layer was 1.1 μm.
[0238] The thickness of the sub-top layer was 1.1 μm.
[0239] The thickness of the top layer was 1.1 μm.
[0240] The ratio of the thickness of the sub-bottom layer to the sub-top layer is 1:1.
[0241] The number of circulation layers of the sub-bottom layer is 90 layers.
[0242] The number of circulation layers of the second top layer is 150.
[0243] 2. Preparation methods of each coating:
[0244] The target material for depositing the bottom layer is Al 0.7 Cr 0.3 alloy.
[0245] The target material for depositing the sub-bottom layer is Al 0.6 Ti 0.3 W 0.1 Alloy, Al 0.7 Cr 0.3 Alloy, Ti 0.85 Si 0.15 alloy.
[0246] The target material for depositing the second top layer is Al 0.6 Ti 0.3 W 0.1 Alloy, Ti 0.85 Si 0.15 alloy.
[0247] The target material for depositing the top layer is metal Zr.
[0248] Example 13
[0249] The tool coating suitable for titanium alloy processing in this embodiment consists of a bottom layer, a sub-bottom layer, a sub-top layer and a top layer, and the thickness of the coating is 3.8 μm.
[0250] 1. Structure of each coating:
[0251] The bottom layer is (Al 0.7 Cr 0.3 )N.
[0252] The sub-bottom layer is (Al 0.6 Ti 0.3 Mo 0.1 )N / (Al 0.7 Cr0.3 )N / (Ti 0.85 Si 0.15 )N recurrent layers.
[0253] The second top layer is (Ti 0.85 Si 0.15 )N / (Al 0.6 Ti 0.3 Mo 0.1 )N recurrent layers.
[0254] The top layer is ZrN.
[0255] The thickness of the bottom layer was 0.5 μm.
[0256] The thickness of the sub-bottom layer was 1.1 μm.
[0257] The thickness of the sub-top layer was 1.1 μm.
[0258] The thickness of the top layer was 1.1 μm.
[0259] The ratio of the thickness of the sub-bottom layer to the sub-top layer is 1:1.
[0260] The number of circulation layers of the sub-bottom layer is 90 layers.
[0261] The number of circulation layers of the second top layer is 150.
[0262] 2. Preparation methods of each coating:
[0263] The target material for depositing the bottom layer is Al 0.7 Cr 0.3 alloy.
[0264] The target material for depositing the sub-bottom layer is Al 0.6 Ti 0.3 Mo 0.1 Alloy, Al 0.7 Cr 0.3 Alloy, Ti 0.85 Si 0.15 alloy.
[0265] The target material for depositing the second top layer is Al 0.6 Ti 0.3 Mo 0.1 Alloy, Ti 0.85 Si 0.15 alloy.
[0266] The target material for depositing the top layer is metal Zr.
[0267] Embodiment 14
[0268] The tool coating suitable for titanium alloy processing in this embodiment is composed of a bottom layer, a sub-bottom layer, a sub-top layer and a top layer.
[0269] The thickness of the coating was 3.0 μm.
[0270] 1. Structure of each coating:
[0271] The bottom layer is (Al 0.7 Cr 0.3 )N.
[0272] The sub-bottom layer is (Al 0.6 Ti 0.32 Mo 0.08 )N / (Al 0.7 Cr 0.3 )N / (Ti 0.85 Si 0.15 )N recurrent layers.
[0273] The second top layer is (Ti 0.85 Si 0.15 )N / (Al 0.6 Ti 0.32 Mo 0.08 )N recurrent layers.
[0274] The top layer is ZrN.
[0275] The thickness of the bottom layer was 0.5 μm.
[0276] The thickness of the sub-bottom layer was 1.0 μm.
[0277] The thickness of the sub-top layer was 1.0 μm.
[0278] The thickness of the top layer was 0.5 μm.
[0279] The ratio of the thickness of the sub-bottom layer to the sub-top layer is 1:1.
[0280] The number of circulation layers of the sub-bottom layer is 90 layers.
[0281] The number of circulation layers of the second top layer is 150.
[0282] 2. Preparation methods of each coating:
[0283] The target material for depositing the bottom layer is Al 0.7 Cr 0.3 alloy.
[0284] The target material for depositing the sub-bottom layer is Al 0.6 Ti 0.32 Mo 0.08 Alloy, Al 0.7 Cr 0.3 Alloy, Ti0.85 Si 0.15 alloy.
[0285] The target material for depositing the second top layer is Al 0.6 Ti 0.32 Mo 0.08 Alloy, Ti 0.85 Si 0.15 alloy.
[0286] The target material for depositing the top layer is metal Zr.
[0287] Embodiment 15
[0288] The tool coating suitable for titanium alloy processing in this embodiment is composed of a bottom layer, a sub-bottom layer, a sub-top layer and a top layer.
[0289] The thickness of the coating was 3.9 μm.
[0290] 1. Structure of each coating:
[0291] The bottom layer is (Al 0.7 Cr 0.3 )N.
[0292] The sub-bottom layer is (Al 0.6 Ti 0.32 Mo 0.08 )N / (Al 0.7 Cr 0.3 )N / (Ti 0.8 Si 0.2 )N recurrent layers.
[0293] The second top layer is (Ti 0.8 Si 0.2 )N / (Al 0.6 Ti 0.32 Mo 0.08 )N recurrent layers.
[0294] The top layer is ZrN.
[0295] The thickness of the bottom layer was 0.6 μm.
[0296] The thickness of the sub-bottom layer was 1.1 μm.
[0297] The thickness of the sub-top layer was 1.1 μm.
[0298] The thickness of the top layer was 1.1 μm.
[0299] The ratio of the thickness of the sub-bottom layer to the sub-top layer is 1:1.
[0300] The number of circulation layers of the sub-bottom layer is 90 layers.
[0301] The number of circulation layers of the second top layer is 150.
[0302] The scanning electron microscope image of the tool coating prepared in this experiment is shown in Figure 2 The partial enlargement on the right side of the figure is for illustration only, and the framed area does not represent the actual partial enlargement range. 2. Preparation methods of each coating:
[0303] The target material for depositing the bottom layer is Al 0.7 Cr 0.3 alloy.
[0304] The target material for depositing the sub-bottom layer is Al 0.6 Ti 0.32 Mo 0.08 Alloy, Al 0.7 Cr 0.3 Alloy, Ti 0.8 Si 0.2 alloy.
[0305] The target material for depositing the second top layer is Al 0.6 Ti 0.32 Mo 0.08 Alloy, Ti 0.8 Si 0.2 alloy.
[0306] The target material for depositing the top layer is metal Zr.
[0307] Example 16
[0308] The tool coating suitable for titanium alloy processing in this embodiment is composed of a bottom layer, a sub-bottom layer, a sub-top layer and a top layer, and the thickness of the coating is 3.0 μm.
[0309] 1. Structure of each coating:
[0310] The bottom layer is (Al 0.62 Cr 0.31 Si 0.07 )N.
[0311] The sub-bottom layer is (Al 0.57 Ti 0.38 B 0.05 )N / (Al 0.62 Cr 0.31 Si 0.07 )N / (Ti 0.85 Si 0.15 )N recurrent layers.
[0312] The second top layer is (Ti 0.85 Si 0.15 )N / (Al 0.57 Ti 0.38 B 0.05)N recurrent layers.
[0313] The top layer is ZrN.
[0314] The thickness of the bottom layer was 0.2 μm.
[0315] The thickness of the sub-bottom layer was 0.9 μm.
[0316] The thickness of the sub-top layer was 0.9 μm.
[0317] The thickness of the top layer was 1.0 μm.
[0318] The ratio of the thickness of the sub-bottom layer to the sub-top layer is 1:1.
[0319] The number of circulation layers of the sub-bottom layer is 90 layers.
[0320] The number of circulation layers of the second top layer is 150.
[0321] 2. Preparation methods of each coating:
[0322] The target material for depositing the bottom layer is Al 0.62 Cr 0.31 Si 0.07 alloy.
[0323] The target material for depositing the sub-bottom layer is Al 0.57 Ti 0.38 B 0.05 Alloy, Al 0.62 Cr 0.31 Si 0.07 Alloy, Ti 0.85 Si 0.15 alloy.
[0324] The target material for depositing the second top layer is Al 0.57 Ti 0.38 B 0.05 Alloy, Ti 0.85 Si 0.15 alloy.
[0325] The target material for depositing the top layer is metal Zr.
[0326] Embodiment 17
[0327] The tool coating suitable for titanium alloy processing in this embodiment consists of a bottom layer, a sub-bottom layer, a sub-top layer and a top layer, and the thickness of the coating is 3.6 μm.
[0328] 1. Structure of each coating:
[0329] The bottom layer is (Al 0.62 Cr 0.3 Si 0.05 W0.03 )N.
[0330] The sub-bottom layer is (Al 0.45 Ti 0.45 B 0.1 )N / (Al 0.62 Cr 0.3 Si 0.05 W 0.03 )N / (Ti 0.85 Si 0.15 )N recurrent layers.
[0331] The second top layer is (Ti 0.85 Si 0.15 )N / (Al 0.45 Ti 0.45 B 0.1 )N recurrent layers.
[0332] The top layer is ZrN.
[0333] The thickness of the bottom layer was 0.7 μm.
[0334] The thickness of the sub-bottom layer was 1.1 μm.
[0335] The thickness of the sub-top layer was 1.0 μm.
[0336] The thickness of the top layer was 0.8 μm.
[0337] The ratio of the thickness of the sub-bottom layer to the sub-top layer is 1.1:1.
[0338] The number of circulation layers of the sub-bottom layer is 90 layers.
[0339] The number of circulation layers of the second top layer is 150.
[0340] 2. Preparation methods of each coating:
[0341] The target material for depositing the bottom layer is Al 0.62 Cr 0.3 Si 0.05 W 0.03 alloy.
[0342] The target material for depositing the sub-bottom layer is Al 0.45 Ti 0.45 B 0.1 Alloy, Al 0.62 Cr 0.3 Si 0.05 W 0.03 Alloy, Ti 0.85 Si 0.15 alloy.
[0343] The target material for depositing the second top layer is Al0.45 Ti 0.45 B 0.1 Alloy, Ti 0.85 Si 0.15 alloy.
[0344] The target material for depositing the top layer is metal Zr.
[0345] Embodiment 18
[0346] The tool coating suitable for titanium alloy processing in this embodiment consists of a bottom layer, a sub-bottom layer, a sub-top layer and a top layer, and the thickness of the coating is 2.6 μm.
[0347] 1. Structure of each coating:
[0348] The bottom layer is (Al 0.6 Cr 0.3 V 0.1 )N.
[0349] The sub-bottom layer is (Al 0.6 Ti 0.3 B 0.1 )N / (Al 0.6 Cr 0.3 V 0.1 )N / (Ti 0.85 Si 0.15 )N recurrent layers.
[0350] The second top layer is (Ti 0.85 Si 0.15 )N / (Al 0.6 Ti 0.3 B 0.1 )N recurrent layers.
[0351] The top layer is ZrN.
[0352] The thickness of the bottom layer was 0.3 μm.
[0353] The thickness of the sub-bottom layer was 1.0 μm.
[0354] The thickness of the sub-top layer was 1.0 μm.
[0355] The thickness of the top layer was 0.3 μm.
[0356] The ratio of the thickness of the sub-bottom layer to the sub-top layer is 1:1.
[0357] The number of circulation layers of the sub-bottom layer is 90 layers.
[0358] The number of circulation layers of the second top layer is 150.
[0359] 2. Preparation methods of each coating:
[0360] The target material for depositing the bottom layer is Al 0.6 Cr 0.3 V 0.1 alloy.
[0361] The target material for depositing the sub-bottom layer is Al 0.6 Ti 0.3 B 0.1 Alloy, Al 0.6 Cr 0.3 V 0.1 Alloy, Ti 0.85 Si 0.15 alloy.
[0362] The target material for depositing the second top layer is Al 0.6 Ti 0.3 B 0.1 Alloy, Ti 0.85 Si 0.15 alloy.
[0363] The target material for depositing the top layer is metal Zr.
[0364] Embodiment 19
[0365] The tool coating suitable for titanium alloy processing in this embodiment is composed of a bottom layer, a bottom layer, a sub-top layer and a top layer, and the thickness of the coating is 3.2 μm.
[0366] 1. Structure of each coating:
[0367] The bottom layer is (Al 0.6 Cr 0.3 B 0.1 )N.
[0368] The sub-bottom layer is (Al 0.6 Ti 0.32 Mo 0.08 )N / (Al 0.6 Cr 0.3 B 0.1 )N / (Ti 0.85 Si 0.15 )N recurrent layers.
[0369] The second top layer is (Ti 0.85 Si 0.15 )N / (Al 0.6 Ti 0.32 Mo 0.08 )N recurrent layers.
[0370] The top layer is ZrN.
[0371] The thickness of the bottom layer was 0.4 μm.
[0372] The thickness of the sub-bottom layer was 1.2 μm.
[0373] The thickness of the sub-top layer was 1.2 μm.
[0374] The thickness of the top layer was 0.4 μm.
[0375] The ratio of the thickness of the sub-bottom layer to the sub-top layer is 1:1.
[0376] The number of circulation layers of the sub-bottom layer is 90 layers.
[0377] The number of circulation layers of the second top layer is 150.
[0378] 2. Preparation methods of each coating:
[0379] The target material for depositing the bottom layer is Al 0.6 Cr 0.3 B 0.1 alloy.
[0380] The target material for depositing the sub-bottom layer is Al 0.6 Ti 0.32 Mo 0.08 Alloy, Al 0.6 Cr 0.3 B 0.1 Alloy, Ti 0.85 Si 0.15 alloy.
[0381] The target material for depositing the second top layer is Al 0.6 Ti 0.32 Mo 0.08 Alloy, Ti 0.85 Si 0.15 alloy.
[0382] The target material for depositing the top layer is metal Zr.
[0383] Embodiment 20
[0384] The tool coating suitable for titanium alloy processing in this embodiment is composed of a bottom layer, a bottom layer, a sub-top layer and a top layer, and the thickness of the coating is 3.2 μm.
[0385] 1. Structure of each coating:
[0386] The bottom layer is (Al 0.6 Cr 0.3 B 0.1 )N.
[0387] The sub-bottom layer is (Al 0.6 Ti 0.32 Mo 0.08 )N / (Al 0.6 Cr 0.3 B0.1 )N / (Ti 0.85 Si 0.15 )N recurrent layers.
[0388] The second top layer is (Ti 0.85 Si 0.15 )N / (Al 0.6 Ti 0.32 Mo 0.08 )N recurrent layers.
[0389] The top layer is ZrC.
[0390] The thickness of the bottom layer was 0.3 μm.
[0391] The thickness of the sub-bottom layer was 1.1 μm.
[0392] The thickness of the sub-top layer was 1.0 μm.
[0393] The thickness of the top layer was 0.8 μm.
[0394] The ratio of the thickness of the sub-bottom layer to the sub-top layer is 1.1:1.
[0395] The number of circulation layers of the sub-bottom layer is 90 layers.
[0396] The number of circulation layers of the second top layer is 150.
[0397] 2. Preparation methods of each coating:
[0398] The target material for depositing the bottom layer is Al 0.6 Cr 0.3 B 0.1 alloy.
[0399] The target material for depositing the sub-bottom layer is Al 0.6 Ti 0.32 Mo 0.08 Alloy, Al 0.6 Cr 0.3 M 0.1 Alloy and Ti 0.85 Si 0.15 alloy.
[0400] The target material for depositing the second top layer is Ti 0.85 Si 0.15 Alloy and Al 0.6 Ti 0.32 Mo 0.08 alloy.
[0401] The target material for depositing the top layer is metal Zr.
[0402] Comparative Example 1
[0403] The tool coating suitable for titanium alloy processing in this comparative example consists of a base layer, and the thickness of the coating is 3.0 μm.
[0404] 1. Structure of each coating:
[0405] The bottom layer is (Al 0.67 Ti 0.33 )N.
[0406] The thickness of the bottom layer was 3.0 μm.
[0407] 2. Preparation methods of each coating:
[0408] The target material for depositing the bottom layer is Al 67 Ti 33 alloy.
[0409] Comparative Example 2
[0410] The tool coating suitable for titanium alloy processing in this comparative example consists of a base layer, and the thickness of the coating is 3.0 μm.
[0411] 1. Structure of each coating:
[0412] The bottom layer is (Al 0.7 Cr 0.3 )N.
[0413] The thickness of the bottom layer was 3.0 μm.
[0414] 2. Preparation methods of each coating:
[0415] The target material for depositing the bottom layer is Al 0.7 Cr 0.3 alloy.
[0416] Effect Example
[0417] The cutting tools containing the coatings of the above embodiments and comparative examples were subjected to cutting tests under the following conditions. The test results are shown in Table 1.
[0418] Flat bottom milling cutter: D6.0R0.5x16xd6x50-4T;
[0419] Processing method: side milling;
[0420] Cutting speed Vc: 170m / min;
[0421] Feed fz: 0.056mm / rev;
[0422] Cutting depth Ap: 8mm;
[0423] Cutting width Ae: 0.4mm;
[0424] Cooling method: water cooling;
[0425] Workpiece material: Ti-6Al-4V (TC4).
[0426] Table 1
[0427]
[0428] From the above examples and comparative examples, it can be seen that in Examples 1 to 4, the coating surface has an anti-adhesive top coating design, so that the coated tool has a good adhesive wear effect during the cutting process, and thus the cutting life of the coated tool is slightly longer.
[0429] In Examples 5, 7, and 8, since the bottom layer of the coating is alloy-doped, the coating has good wear resistance and lubricity, and thus the lifespan is improved. However, in Example 6, since too much Si content is added, the amorphous content in the coating is too high, and the hardness of the coating is reduced, so the effect is slightly worse.
[0430] In Examples 9 to 11, the number of cycles of the sub-bottom layer and the sub-top layer is optimized. The higher the number of cycles, the thinner the thickness of each layer, the better the strengthening effect of the nano multilayer structure, and thus the longer the cutting life of the coated tool.
[0431] Examples 12 to 15 conducted comparative experiments on the Si content in the doped metal Me and TiSiN, and found that the cutting life of the coated tool was basically the same when W and Mo were doped at the same content (Example 12, Example 13); however, when the Mo content was slightly lower, the coating performed slightly better, but overall, the difference was not very large. However, the increase in Si content had a greater impact on the service life of the coating. After the Si content increased to 20at% (Example 15), the cutting life of the coated tool increased. This may be because W and Mo are basically the same in terms of lubricity, but the increase in Si content has a greater impact on the nanocomposite structure of the TiSiN coating.
[0432] In Examples 16 to 20, V, Si, and B were doped into AlCrN, and acetylene as a reaction gas was added into ZrN. The results show that the elements doped into AlCrN have a certain good effect on the cutting life of the coating, and the surface ZrCN has basically the same performance as ZrN in the actual cutting process.
[0433] Compared with the comparative examples, the above embodiments have obvious advantages in cutting effect over the comparative examples in terms of structural optimization and coating composition optimization, especially in the process of titanium alloy processing, the chipping resistance of the coated tool has been significantly enhanced.
[0434] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods. The specific embodiments described above further describe the purpose, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A tool coating suitable for titanium alloy processing, characterized in that: The coating structure includes one of the following (a) or (b); (a) bottom layer, second bottom layer, second top layer and top layer; (b) bottom layer and top layer; Wherein, the bottom layer is (Al a Cr b M 1-a-b )N; The sub-bottom layer is (Al c Ti d Me 1-c-d )N / (Al a Cr b M 1-a-b )N / (Ti e Si 1-e )N loop layers; The second top layer is (Ti e Si 1-e )N / (Al c Ti d Me 1-c-d )N loop layers; The top layer is TX; M is at least one of W, Mo, V, Si, and B; Me is at least one of W, Mo, V, Si and B; T is at least one of Zr, Nb and Cr; X is at least one of N, C, and CN; 0.4≤a≤0.8, 0.2≤b≤0.5, 1-ab≥0; 0.4≤c≤0.7, 0.3≤d≤0.6, 1-cd≥0; 0.5≤e≤0.9。 2. The tool coating suitable for titanium alloy processing according to claim 1, characterized in that: The substrate selected for the tool coating is a CNC blade made of cemented carbide or ceramic material, wherein the hardness of the substrate is 1300-1800 HV 30 .
3. The tool coating suitable for titanium alloy processing according to claim 1, characterized in that: Satisfy at least one of the following conditions (1) to (6): (1) The thickness of the coating is 1.5 to 4.0 μm; (2) The thickness of the bottom layer is 0.2 to 3.5 μm; (3) The thickness of the sub-bottom layer is 0.8 to 1.5 μm; (4) The thickness of the sub-top layer is 0.8 to 1.5 μm; (5) The thickness of the top layer is 0.2 to 1.5 μm; (6) The thickness ratio of the sub-bottom layer to the sub-top layer is 0.5 to 2:
1.
4. The tool coating suitable for titanium alloy processing according to claim 1, characterized in that: Satisfy at least one of the following conditions (1) to (4): (1) The bottom layer is composed of (Al a Cr b M 1-a-b )N deposition formation; (2) The sub-bottom layer is composed of (Al c Ti d Me 1-c-d )N、(Al a Cr b M 1-a-b )N and (Ti e Si 1-e )N three layers are deposited alternately in sequence; (3) The second top layer is (Ti e Si 1-e )N and (Al c Ti d Me 1-c-d )N two layers are deposited alternately in sequence; (4) The top layer is formed by TX deposition.
5. The tool coating suitable for titanium alloy processing according to claim 1, characterized in that: Satisfy at least one of the following conditions (1) to (4): (1) The bottom layer is a single-layer structure; (2) The top layer is a single-layer structure; (3) The number of cycles of the sub-bottom layer is 0 to 180 layers, wherein (Al c Ti d Me 1-c-d )N / (Al a Cr b M 1-a-b )N / (Ti e Si 1-e )N is a loop layer; (4) The number of cycles of the second top layer is 0 to 200, wherein (Ti e Si 1-e )N / (Al c Ti d Me 1-c-d )N is a recurrent layer.
6. The tool coating suitable for titanium alloy processing according to claim 1, characterized in that: Satisfy at least one of the following conditions (1) to (4): (1) The innermost layer of the sub-bottom layer is (Al c Ti d Me 1-c-d )N; (2) The outermost layer of the sub-bottom layer is (Ti e Si 1-e )N; (3) The innermost layer of the second top layer is (Ti e Si 1-e )N; (4) The outermost layer of the sub-top layer is (Al c Ti d Me 1-c-d )N.
7. The tool coating suitable for titanium alloy processing according to claim 1, characterized in that: Satisfy at least one of the following conditions (1) to (2): (1) The outermost layer of the second bottom layer has the same chemical composition as the innermost layer of the second top layer; (2) The innermost layer of the sub-bottom layer and the outermost layer of the sub-top layer have the same chemical composition.
8. The method for preparing a tool coating suitable for titanium alloy processing according to any one of claims 1 to 7, characterized in that: The coatings are all formed by vapor deposition; Wherein, the vapor deposition satisfies at least one of the following conditions (1) to (7): (1) The vapor deposition adopts cathode arc technology; (2) The reaction gas for the vapor deposition is nitrogen or acetylene; (3) The arc current of the arc source of the vapor deposition is 100-200A; (4) The vacuum degree of the vapor deposition is 1.0 to 6.0 Pa; (5) The bias voltage for depositing the bottom layer and the top layer during the vapor deposition is -30 to -100 V; (6) The bias voltage for depositing the sub-bottom layer and the sub-top layer during the vapor deposition is -30 to -200 V; (7) The deposition temperature in the vapor deposition is 400-600°C.
9. The method for preparing a tool coating suitable for titanium alloy processing according to claim 8, characterized in that: Satisfy at least one of the following conditions (1) to (5): (1) The purity of the target material used in the vapor deposition is ≥99.8%; (2) The target material for depositing the bottom layer is Al a Cr b M 1-a-b alloy; (3) The target material for depositing the sub-bottom layer is Al c Ti d Me 1-c-d Alloy, Al a Cr b M 1-a-b Alloy and Ti e Si 1-e alloy; (4) The target material for depositing the second top layer is Ti e Si 1-e Alloy and Al c Ti d Me 1-c-d alloy; (5) The target material for depositing the top layer is metal T.
10. A tool comprising the tool coating suitable for titanium alloy processing as claimed in claims 1 to 7.
Citation Information
Patent Citations
Composite coating for cutter as well as preparation method and application of composite coating
CN116024526A
Cutting tool containing nano-composite multilayer coating and preparation method thereof
CN116083846A
Isometric crystal and columnar crystal combined ZrN-CrAlN composite coating as well as preparation method and application thereof