Method for preparing formic acid / formate through electrocatalytic reduction of carbon dioxide based on metal cation reinforced solid electrolyte
By introducing metal cations into the solid electrolyte and adjusting the anolyte components, the problems of high solid electrolyte resistivity and low catalytic efficiency are solved, efficient electrocatalytic reduction of carbon dioxide is achieved, product separation costs are reduced, and the electrolytic cell efficiency is improved. Stable and suitable for large-scale industrial applications.
Patent Information
- Application Number
- CN202410774187.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-11
AI Technical Summary
In the existing carbon dioxide electrocatalytic reduction technology, the high resistivity of the solid electrolyte leads to low current density, corrosion of the catholyte and high product separation costs, and the lack of metal cation catalysis leads to low catalytic efficiency and serious hydrogen evolution side reactions.
Introduce metal cations (such as sodium ions) into the solid electrolyte, adjust the anolyte composition, improve the conductivity, and achieve controllable generation of formic acid/formate solution by adjusting the anolyte composition.
It improves the efficiency of electrocatalytic reduction of carbon dioxide, reduces product separation costs, and enhances the stability of gas diffusion electrodes. The Faradaic efficiency reaches more than 80%, making it suitable for large-scale industrial applications.
Smart Images

Figure CN118756170A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrocatalysis, and in particular to a method for preparing formic acid / formates by electrocatalytic reduction of carbon dioxide based on metal cation-enhanced solid electrolyte. Background Art
[0002] The rapid development of society has led to the extensive use of fossil fuel energy, the energy crisis caused by the continuous emission of carbon dioxide, and climate change have caused great threats to the global ecosystem. As the cost of renewable electricity continues to decline, the competitiveness of producing chemical raw materials through electrocatalytic reduction of carbon dioxide has greatly improved, and it has great development potential.
[0003] The cathode electrolyte used in the current conventional carbon dioxide electrocatalytic reduction technology is easy to corrode the gas diffusion electrode during the electrocatalytic process, causing flooding and salting out, reducing the utilization efficiency of carbon dioxide and making it difficult to ensure stability. At the same time, the liquid product is a mixed solution of high-concentration electrolyte and target product, and the separation cost is extremely high, making it difficult to achieve large-scale industrial application.
[0004] Xia et al. developed a new membrane electrode solid electrolyte electrolytic cell reactor. By introducing a solid electrolyte to replace the ion transport function of the cathode electrolyte, the problem of decreased stability of the electrolytic cell and high product separation cost caused by the use of the cathode electrolyte can be avoided, and finally the production of formic acid with a concentration of 0.1 mol / L was achieved (Nat Energy, 2019, 4, 776). Fan et al. continued to use this type of reactor, combined with the anodic hydrogen oxidation reaction, and concentrated pure formic acid from the steam (Nat Commun, 2020, 11, 3633).
[0005] However, due to the high resistivity of the solid electrolyte itself, the current density when it is used for electrocatalytic carbon dioxide reduction is lower than that of the flow electrolyzer. In addition, studies have shown that metal cations such as potassium and sodium play a vital role in the electrocatalytic carbon dioxide reduction reaction. The carbon dioxide reduction without metal cation catalysis faces the problems of low catalytic efficiency, low current density, and serious hydrogen evolution side reaction (Nat Catal, 2022, 5, 268–276). Although the electrocatalytic carbon dioxide reduction technology combined with the anodic hydrogen oxidation reaction reduces the overpotential for the formation of formic acid, it is actually a reaction that converts high-value hydrogen into low-value formic acid, and the economic benefits of the product are greatly reduced. Even so, Fan et al.'s membrane electrode solid electrolyte electrolyzer combined with the anodic hydrogen oxidation reaction can only operate for a long time at 30mA / cm 2 Under current density (Nat Commun, 2020, 11, 3633). Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a method for preparing formic acid / formates by electrocatalytic reduction of carbon dioxide based on metal cation-enhanced solid electrolytes. The present invention introduces metal cations (such as sodium ions) into the solid electrolyte, and adjusts the cationic components in the anolyte, which not only improves the conductivity of the solid electrolyte, but also effectively promotes the electrocatalytic reduction of carbon dioxide. In addition, the controllable generation of formic acid / formates solution can be achieved by adjusting the components of the anolyte, and the product can be used as a chemical raw material, an energy carrier, a supplementary carbon source in sewage treatment, etc. This technology is an excellent choice for large-scale industrial applications.
[0007] The first object of the present invention is to provide a method for preparing formic acid / formates by electrocatalytic reduction of carbon dioxide based on metal cation-enhanced solid electrolyte, comprising the following steps:
[0008] (1) Provide a solid electrolytic cell reaction device, comprising a cathode flow channel plate, a gas diffusion cathode, an anion exchange membrane, a solid electrolyte layer, a cation exchange membrane, an anode catalyst, and an anode flow channel plate arranged in sequence; the gas diffusion cathode comprises a gas diffusion layer, a microporous layer, and a cathode catalyst layer in sequence; the solid electrolyte layer is obtained by ion exchange of a solid electrolyte in an alkali metal salt solution;
[0009] (2) Pass carbon dioxide gas into the cathode flow channel plate, pump cathode electrolyte and anode electrolyte into the solid electrolyte layer and anode flow channel plate respectively, apply voltage to the solid electrolytic cell reaction device, and wait for the current to gradually increase to greater than 10 mA / cm 2 Afterwards, the electrocatalytic carbon dioxide reduction reaction occurs;
[0010] (3) Collecting the liquid flowing out of the solid electrolyte layer to obtain a formic acid / formate solution free of electrolyte.
[0011] In some embodiments of the present invention, in step (1), the solid electrolyte is a cationic solid electrolyte; further, the solid electrolyte is a hydrogen-type ion exchange resin composed of styrene-divinylbenzene copolymer. Preferably, the ion exchange resin model is 50W X8, particle size is 200-400 mesh.
[0012] And / or, the concentration of the sodium salt solution or potassium salt solution is 0.1-2 mol / L;
[0013] And / or, the ion exchange time is more than 24 hours;
[0014] And / or, the alkali metal in the alkali metal salt solution is selected from one or more of lithium, sodium, potassium, and cesium, and the salt in the alkali metal salt solution is sulfate or carbonate, such as sodium sulfate, potassium sulfate, cesium sulfate, sodium carbonate, potassium carbonate, etc.
[0015] In some embodiments of the present invention, in step (1), the cathode catalyst layer is formed by uniformly mixing a cathode catalyst, an alcohol solution, a perfluorosulfonic acid ion polymer solution, and a hydrophobic agent dispersion, and ultrasonically dispersing the mixture to obtain a catalyst dispersion, which is then sprayed on the surface of the microporous layer and dried.
[0016] In some embodiments of the present invention, the cathode catalyst is selected from one or more of a metal element, a metal oxide or a metal sulfide; further, the metal element is selected from any one of bismuth, tin and indium, and the metal in the metal oxide or metal sulfide is selected from any one of bismuth, tin and indium. And / or, the metal element, metal oxide or metal sulfide is a micron or nanometer powder.
[0017] Preferably, the cathode catalyst includes bismuth trioxide, tin oxide, bismuth powder, indium trioxide, etc. Commercial catalysts can be used selectively, and conventional methods such as precipitation, hydrothermal, calcination, and chemical reduction can also be used to prepare the cathode catalyst.
[0018] Furthermore, the cathode catalyst is preferably one or more of bismuth trioxide nanopowder, bismuth nanopowder, and oxygen vacancy bismuth catalyst.
[0019] Furthermore, the oxygen vacancy bismuth catalyst can be prepared by chemical reduction method, as follows:
[0020] The oxygen vacancy bismuth catalyst is obtained by reacting bismuth trioxide nanopowder with a reducing agent in water, performing solid-liquid separation on the reaction liquid, and freeze-drying the obtained solid.
[0021] Preferably, the mass ratio of the bismuth trioxide nanopowder to the reducing agent is 2 to 8:1;
[0022] Preferably, the reducing agent is selected from potassium borohydride.
[0023] Preferably, the mass volume ratio of the bismuth trioxide nanopowder to deionized water is (5-20) g:1 L;
[0024] Preferably, the reaction time is 10 to 60 minutes.
[0025] Preferably, the freeze-drying temperature is -40 to -60°C, and the drying time is 10 to 24 hours.
[0026] And / or, the alcohol in the alcohol solution includes ethanol and / or isopropanol;
[0027] and / or, the hydrophobic agent is selected from polytetrafluoroethylene (PTFE) and / or polyvinylidene fluoride (PVDF);
[0028] And / or, the perfluorosulfonic acid ion polymer solution is D520 solution;
[0029] and / or, the mass volume ratio of the cathode catalyst to the alcohol solution is (5-20): 1 mg / mL;
[0030] and / or, the amount of the perfluorosulfonic acid ion polymer solution added is 20 to 50 μL / mL;
[0031] and / or, the concentration of the hydrophobic agent dispersion is 5 to 20%;
[0032] And / or, the addition amount of the hydrophobic agent dispersion is 5 to 25 μL / mL.
[0033] Preferably, the ultrasonic dispersion time of the catalyst dispersion is 20 to 60 minutes;
[0034] Preferably, the spraying amount of the catalyst dispersion is 0.2 to 10 mg / cm 2 ;
[0035] Preferably, the spraying further includes drying, and the drying is performed under heating by an infrared heating lamp, the drying temperature is preferably 35 to 50° C., and the drying time is preferably 0.5 to 2 hours.
[0036] In the present invention, in step (1), the cathode flow channel plate and the anode flow channel plate are both composed of a titanium plate with gas and liquid microchannels engraved on one side, and have gas / liquid flow channels and inlet / outlet ends. The cathode flow channel plate is a carbon dioxide gas flow channel, and the anode flow channel plate is an anode electrolyte flow channel. The solid electrolyte is a solid electrolyte that can transmit cations such as hydrogen ions, sodium ions, and potassium ions. The cation exchange membrane is a membrane that allows cations such as hydrogen ions, sodium ions, and potassium ions to pass through, but does not allow inorganic anions such as hydroxide, bicarbonate, carbonate, and sulfate or anions of cathode products such as formate and acetate, as well as gas molecules to pass through.
[0037] In some embodiments of the present invention, in step (1), the anode catalyst is a catalyst capable of oxidizing water to generate oxygen in sulfuric acid and / or sodium sulfate solution, including but not limited to one or more of titanium mesh loaded with iridium oxide, titanium foam, iridium oxide, nickel foam, and iron nickel foam, and is prepared into a mesh / felt shape to fully contact with the anode electrolyte.
[0038] Preferably, the anolyte is titanium felt loaded with iridium oxide.
[0039] Preferably, the porosity of the titanium felt loaded with iridium oxide is 60-70%;
[0040] Preferably, the iridium oxide loading rate is 1 to 2 mg / cm 2 (measured in metallic iridium).
[0041] In some embodiments of the present invention, in step (1), the solid electrolyte layer is a cathode electrolyte flow channel.
[0042] In some embodiments of the present invention, in step (1), the gas diffusion layer is supported by carbon fiber paper, and the microporous layer is a microporous carbon-based layer.
[0043] In some embodiments of the present invention, in step (1), the anion exchange membrane is a membrane that allows inorganic anions including hydroxide, bicarbonate, carbonate, sulfate, or cathode product anions such as formate and acetate to pass through, but does not allow cations such as hydrogen ions, sodium ions, potassium ions, and gas molecules to pass through, and is generally composed of a high molecular polymer skeleton and anion conductive groups.
[0044] In some embodiments of the present invention, in step (2), the flow rate of the carbon dioxide gas is 0.1 to 100 mL·min -1 cm -2 .
[0045] In some embodiments of the present invention, in step (2), the cathode electrolyte is deionized water;
[0046] And / or, the anolyte is selected from one or more of sulfuric acid solution, sulfuric acid-sodium sulfate solution, sulfuric acid-potassium sulfate solution, sodium hydroxide solution, potassium hydroxide solution, sodium bicarbonate solution, and potassium bicarbonate solution.
[0047] In some embodiments of the present invention, in step (2), the voltage is -1 to -5 V, and the current is -10 to -1000 mA / cm 2 ;
[0048] And / or, the reaction temperature of the electrocatalytic carbon dioxide reduction reaction is 0°C to 60°C.
[0049] In the present invention, the method for preparing formic acid / sodium formate by electrocatalytic reduction of carbon dioxide based on metal cation-enhanced solid electrolyte is as follows:
[0050] The electrolytic cell is assembled in the order of cathode flow channel plate, fluororubber gasket 1, gas diffusion cathode, anion exchange membrane, fluororubber gasket 2, solid electrolyte layer, fluororubber gasket 3, cation exchange membrane, anode catalyst, fluororubber gasket 4, and anode flow channel plate; wherein the fluororubber gasket serves the functions of sealing, separation and protection, and therefore is not reflected in the schematic diagram of the electrolytic cell device.
[0051] Preferably, the thickness of the fluororubber gasket 1 is 0.2 mm, and the opening is a 1.5×1.5 cm rectangle; the thickness of the fluororubber gaskets 2 and 3 is 0.2 mm, and the opening is a 1×1 cm rectangle; the thickness of the fluororubber gasket 4 is 0.2-1 mm, and the opening is a 1.5×1.5 cm rectangle;
[0052] The electrolyte is pumped into the electrolytic cell device at a certain flow rate, and the cathode and anode electrolytes flow through the solid electrolyte layer and the anode flow channel plate respectively;
[0053] Passing high-purity carbon dioxide gas into the cathode flow channel plate at a certain flow rate, and diffusing the carbon dioxide into the cathode catalyst layer;
[0054] A certain voltage is applied to the electrolytic cell device, and carbon dioxide is catalytically reduced to formate ions. The formate ions pass through the anion exchange membrane and are enriched on the surface of the solid electrolyte. They are flushed and collected by the flowing cathode electrolyte. At the same time, water oxidation reaction occurs at the anode to produce oxygen.
[0055] The cathode electrolyte is deionized water, and the liquid product of the electrocatalytic reduction of carbon dioxide is enriched on the surface of the solid electrolyte through the anion exchange membrane and is washed and collected by the flowing cathode electrolyte.
[0056] Preferably, the volume of the cathode electrolyte is 10 to 1000 mL;
[0057] Preferably, the cathode electrolyte flow rate is 5 to 50 mL / L.
[0058] Preferably, the anolyte includes but is not limited to sulfuric acid, sulfuric acid-sodium sulfate, sulfuric acid-potassium sulfate, sodium hydroxide, potassium hydroxide, sodium bicarbonate, potassium bicarbonate solution. The anolyte flows through the anode channel plate and flows through the anode catalyst to produce water oxidation reaction to generate oxygen.
[0059] Preferably, the anolyte is sulfuric acid with a pH of 0 to 1 or sulfuric acid-0.1 to 1 mol / L sodium sulfate solution with a pH of 0 to 1.
[0060] Preferably, the volume of the anolyte is 10 to 1000 mL;
[0061] Preferably, the cathode electrolyte flow rate is 50 to 500 mL / L;
[0062] The voltage applied to the electrolytic cell is E0 to E0-5 V, where E0 is the theoretical standard electrode potential of the cathode and anode reactions;
[0063] Preferably, the electrolysis current is controlled to be -1 to -1000 mA / cm 2 ;
[0064] Preferably, the cathode gas diffusion electrode area is 1 to 4 cm2 ;
[0065] Preferably, the flow rate of the high-purity carbon dioxide gas is 0.1 to 100 mL min-1 relative to the area of the cathode gas diffusion electrode. -1 cm -2 ;
[0066] The method is carried out at a temperature ranging from 0°C to 60°C, preferably from 15°C to 25°C.
[0067] The above technical solution of the present invention has the following advantages compared with the prior art:
[0068] The present invention can produce a formic acid / sodium formate solution without electrolyte, effectively reducing the downstream separation cost of the product, while increasing the single-pass conversion rate of carbon dioxide and improving the stability of the gas diffusion electrode electrolytic cell.
[0069] The method for electrocatalytic reduction of carbon dioxide according to the present invention can catalytically reduce carbon dioxide with high efficiency, and the Faraday efficiency is generally higher than 80% and can reach 100% at most. BRIEF DESCRIPTION OF THE DRAWINGS
[0070] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:
[0071] Figure 1 The present invention is a schematic diagram of an electrolytic cell device for electrocatalytic reduction of carbon dioxide. The following are the descriptions of the accompanying drawings: 1, cathode flow channel plate, 2, gas diffusion cathode, 3, anion exchange membrane, 4, solid electrolyte layer, 5, cation exchange membrane, 6, anode catalyst, 7, anode flow channel plate; 21, gas diffusion layer, 22, microporous layer, 23, cathode catalyst layer.
[0072] Figure 2 is an X-ray diffraction image of the cathode catalyst in the example.
[0073] Figure 3 This is a diagram showing the effects of potassium and sodium ions on the performance of electrocatalytic reduction of carbon dioxide.
[0074] Figure 4 This is a stability test performance diagram of the electrocatalytic reduction of carbon dioxide technology provided according to the present invention. DETAILED DESCRIPTION
[0075] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0076] Embodiment 1:
[0077] This embodiment provides a method for preparing formic acid solution by electrocatalytic reduction of carbon dioxide:
[0078] 1. The device uses a commercially available flow electrolytic cell. The cathode and anode flow channel slots are standard serpentine flow channels, with a 3mm thick polyetheretherketone plate in the middle for placing solid electrolytes. The flow electrolytic cell, gas diffusion electrode, anion and cation exchange membranes, and anode catalysts are all commercially available products.
[0079] The gas diffusion electrode is a hydrophobic carbon paper with a macroporous support material and a microporous carbon powder layer, and a certain amount of polytetrafluoroethylene is added to perform hydrophobic treatment. The model is SGL 28BC, the thickness is 235 μm, and the water surface contact angle is greater than 130°; the anion exchange membrane is composed of a polystyrene random copolymer electrolyte, the model is X37-50 grade FA, thickness is 50μm; the cation exchange membrane is composed of perfluorosulfonic acid / polytetrafluoroethylene copolymer, model is N115, thickness 127μm; the anode catalyst is a titanium mesh loaded with iridium oxide, with an area of 1.5×1.5cm and a thickness of 0.4mm, wherein the iridium oxide loading rate is 1mg / cm 2 (in terms of metallic iridium); the solid electrolyte is a hydrogen-type ion exchange resin composed of a styrene-divinylbenzene copolymer, the model of which is 50WX8, particle size is 400 mesh. The solid electrolyte was ion exchanged in 0.5 mol / L sodium sulfate solution for 24 h, and the excess sodium sulfate on the surface was washed off with deionized water before use.
[0080] 2. The gas diffusion cathode is prepared by the following method:
[0081] The cathode catalyst, isopropanol, perfluorosulfonic acid ion polymer solution and polytetrafluoroethylene dispersion are mixed and ultrasonically dispersed to obtain a catalyst dispersion as a catalyst layer slurry. The catalyst dispersion is evenly sprayed on a gas diffusion electrode by a spray gun, and a gas diffusion cathode is obtained after drying.
[0082] The cathode catalyst is an oxygen vacancy bismuth catalyst prepared by chemical reduction method. The specific method is as follows: 2g of bismuth trioxide nanopowder and 0.25g of potassium borohydride are reacted in 100mL of deionized water for 30min, and the solid-liquid separation is performed by suction filtration through a 0.45μm water system microporous filter membrane. The obtained solid is freeze-dried at -50°C for 12h to obtain an oxygen vacancy bismuth catalyst. The structural characterization is shown in Figure 2 .
[0083] The purity of the isopropanol is 99.9%, and the amount added is 1 mL;
[0084] The perfluorosulfonic acid ion polymer solution model is D520, added volume 50 μL;
[0085] The polytetrafluoroethylene dispersion has a concentration of 5wt% and an addition amount of 20 μL;
[0086] The ultrasonic dispersion time of the catalyst dispersion is 30 minutes;
[0087] The spraying amount of the catalyst dispersion is 0.3 mL;
[0088] The drying is carried out under heating by an infrared heating lamp, the drying temperature is 40° C., and the drying time is 1 hour.
[0089] 3. The electrocatalytic reduction of carbon dioxide test was carried out using the above electrolytic cell and the gas diffusion cathode, comprising the following steps:
[0090] The electrolytic cell was assembled in the order of cathode flow channel plate, fluororubber gasket 1 (thickness 0.2mm, opening 1.5×1.5cm rectangle), gas diffusion cathode, anion exchange membrane, fluororubber gasket 2 (thickness 0.2mm, opening 1×1cm rectangle), solid electrolyte layer, fluororubber gasket 3 (thickness 0.2mm, opening 1×1cm rectangle), cation exchange membrane, anode catalyst, fluororubber gasket 4 (thickness 0.4mm, opening 1.5×1.5cm rectangle), and anode flow channel plate; 50mL of deionized water was circulated into the solid electrolyte layer at a flow rate of 10mL / h; 50mL of 0.5mol / L sulfuric acid was circulated into the anode flow channel plate at a flow rate of 50mL / h; high-purity carbon dioxide gas (99.99%) was pumped at 10mL·min -1 cm -2 The flow rate of carbon dioxide is passed into the cathode flow channel plate, and carbon dioxide diffuses to the cathode catalyst layer; a voltage of -4V is applied to the electrolytic cell device, and timing is started after the current increases to a steady state, carbon dioxide is catalytically reduced to formate ions, and the formate ions are enriched on the surface of the solid electrolyte through the anion exchange membrane, and are washed and collected by the flowing cathode electrolyte, while water oxidation reaction occurs at the anode to produce oxygen. The method is carried out at a temperature of 20°C.
[0091] Figure 2 The X-ray diffraction images of bismuth powder, bismuth trioxide powder and oxygen vacancy bismuth catalyst. Figure 2 It can be seen that the oxygen vacancy bismuth catalyst has a composite structure of zero-valent bismuth and bismuth trioxide, indicating that the strong reducing agent causes the oxygen atoms in bismuth trioxide to be partially stripped off when preparing the oxygen vacancy bismuth catalyst. The material with this structure has abundant oxygen vacancies and grain boundaries, which is helpful for the electrocatalytic reduction of carbon dioxide.
[0092] After 3 hours of electrocatalytic reaction, the current density was measured to be -117.8 mA / cm2 The concentration of the formic acid solution produced was measured by hydrogen nuclear magnetic resonance spectroscopy to be 0.118 mol / L, and the Faraday efficiency was 89.6%.
[0093] Embodiment 2:
[0094] The difference from Example 1 is:
[0095] The cathode catalyst is commercially available bismuth trioxide nanopowder with a purity of 99.9%, an average particle size of 100 nm, and an addition amount of 10 mg. The rest of the implementation method is the same as in Example 1.
[0096] After 10 hours of electrocatalytic reaction, the current density was measured to be -71.6 mA / cm 2 The concentration of the formic acid solution produced was measured by hydrogen nuclear magnetic resonance spectroscopy to be 0.183 mol / L, and the Faraday efficiency was 73.2%.
[0097] The reason for the difference in effect from Example 1 is that when the oxygen vacancy bismuth catalyst is prepared in Example 1, the strong reducing agent causes the oxygen atoms in bismuth trioxide to be partially stripped off, resulting in the material having rich oxygen vacancies and grain boundaries, which is helpful for the electrocatalytic reduction of carbon dioxide.
[0098] Embodiment 3:
[0099] This embodiment provides a method for preparing sodium formate solution by electrocatalytic reduction of carbon dioxide:
[0100] 1. The device uses a commercially available flow electrolytic cell. The cathode and anode flow channel slots are standard serpentine flow channels, with a 3mm thick polyetheretherketone plate in the middle for placing solid electrolytes. The flow electrolytic cell, gas diffusion electrode, anion and cation exchange membranes, and anode catalysts are all commercially available products.
[0101] The gas diffusion electrode is a hydrophobic carbon paper with a macroporous support material and a microporous carbon powder layer, and a certain amount of polytetrafluoroethylene is added to perform hydrophobic treatment. The model is SGL 28BC, the thickness is 235 μm, and the water surface contact angle is greater than 130°; the anion exchange membrane is composed of a polystyrene random copolymer electrolyte, the model is FAA-pk-130, thickness is 130 μm; the cation exchange membrane is composed of perfluorosulfonic acid / polytetrafluoroethylene copolymer, model is N115, thickness 127μm; the anode catalyst is a titanium mesh loaded with iridium oxide, with an area of 1.5×1.5cm and a thickness of 0.4mm, wherein the iridium oxide loading rate is 2mg / cm 2 (in terms of metallic iridium); the solid electrolyte is a hydrogen-type ion exchange resin composed of a styrene-divinylbenzene copolymer, the model of which is 50W X8, particle size is 100 mesh. Solid-state electrolysis is carried out in 0.5 mol / L sodium sulfate solution for 24 hours, and the excess sodium sulfate on the surface is washed off with deionized water before use.
[0102] 2. The gas diffusion cathode is prepared by the following method:
[0103] The cathode catalyst, isopropanol, perfluorosulfonic acid ion polymer solution and polytetrafluoroethylene dispersion are mixed and ultrasonically dispersed to obtain a catalyst dispersion as a catalyst layer raw material. A certain amount of the catalyst dispersion is evenly sprayed on the gas diffusion electrode by a spray gun, and a gas diffusion cathode is obtained after drying;
[0104] The cathode catalyst is an oxygen vacancy bismuth catalyst prepared by chemical reduction. 2 g of bismuth trioxide nanopowder and 0.25 g of potassium borohydride are reacted in 100 mL of deionized water for 30 min, and the solid-liquid separation is performed by suction filtration through a 0.45 μm water system microporous filter membrane, and the obtained solid is freeze-dried at -50°C for 12 h to obtain an oxygen vacancy bismuth catalyst.
[0105] The cathode catalyst addition amount is 10 mg;
[0106] The purity of the isopropanol is 99.9%, and the amount added is 1 mL;
[0107] The perfluorosulfonic acid ion polymer solution model is D520, added volume was 40 μL;
[0108] The concentration of the polytetrafluoroethylene dispersion is 10%, and the amount added is 20 μL;
[0109] The ultrasonic dispersion time of the catalyst dispersion is 30 minutes;
[0110] The spraying amount of the catalyst dispersion is 0.25 mL;
[0111] The drying is carried out under an infrared heating lamp, the drying temperature is 40° C., and the drying time is 1 hour.
[0112] 3. The electrocatalytic reduction of carbon dioxide test was carried out using the above electrolytic cell and the gas diffusion cathode, comprising the following steps:
[0113] The electrolytic cell was assembled in the order of cathode flow channel plate, fluororubber gasket 1 (thickness 0.2mm, opening 1.5×1.5cm rectangle), gas diffusion cathode, anion exchange membrane, fluororubber gasket 2 (thickness 0.2mm, opening 1×1cm rectangle), solid electrolyte layer, fluororubber gasket 3 (thickness 0.2mm, opening 1×1cm rectangle), cation exchange membrane, anode catalyst, fluororubber gasket 4 (thickness 0.4mm, opening 1.5×1.5cm rectangle), and anode flow channel plate; 50mL of deionized water was circulated into the solid electrolyte layer at a flow rate of 20mL / h; 100mL of 0.5mol / L sulfuric acid-sodium sulfate with pH=1 was circulated into the anode flow channel plate at a flow rate of 50mL / h; high-purity carbon dioxide gas (99.99vt%) was pumped at 20mL·min -1 cm -2 The flow rate of carbon dioxide is passed into the cathode flow channel plate, and carbon dioxide diffuses to the cathode catalyst layer; a voltage of -3.5V is applied to the electrolytic cell device, and timing is started after the current increases to a steady state, carbon dioxide is catalytically reduced to formate ions, and the formate ions are enriched on the surface of the solid electrolyte through the anion exchange membrane, and are washed and collected by the flowing cathode electrolyte, while water oxidation reaction occurs at the anode to produce oxygen. The method is carried out at a temperature of 25°C.
[0114] After 4 hours of electrocatalytic reaction, the current density was measured to be -173.6 mA / cm 2 The concentration of the sodium formate solution produced was measured by hydrogen nuclear magnetic resonance spectroscopy to be 0.248 mol / L, and the Faraday efficiency was 96.4%.
[0115] Comparative Example 1:
[0116] The difference with embodiment 3 is:
[0117] The anolyte is 100 mL of 0.5 mol / L neutral sodium sulfate solution without sulfuric acid. The other conditions are the same as those in Example 2.
[0118] After 2 hours of electrocatalytic reaction, the current density was measured to be -124.2 mA / cm 2 The concentration of the sodium formate solution produced was measured by hydrogen nuclear magnetic resonance spectroscopy to be 7.88 mmol / L, and the Faraday efficiency was 85.1%.
[0119] Example 4: This example provides a method for preparing formic acid solution by electrocatalytic reduction of carbon dioxide:
[0120] 1. The device uses a commercially available flow electrolytic cell. The cathode and anode flow channel slots are standard serpentine flow channels, with a 3mm thick polyetheretherketone plate in the middle for placing solid electrolytes. The flow electrolytic cell, gas diffusion electrode, anion and cation exchange membranes, and anode catalysts are all commercially available products.
[0121] The gas diffusion electrode is a hydrophobic carbon paper with a macroporous support material and a microporous carbon powder layer, and a certain amount of polytetrafluoroethylene is added to perform hydrophobic treatment. The model is SGL 28BC, the thickness is 235 μm, and the water surface contact angle is greater than 130°; the anion exchange membrane is composed of a polystyrene random copolymer electrolyte, the model is X37-50 grade FA, thickness is 50μm; the cation exchange membrane is composed of perfluorosulfonic acid / polytetrafluoroethylene copolymer, model is N115, thickness 127μm; the anode catalyst is titanium felt loaded with iridium oxide, area 1.5×1.5cm, thickness 0.4mm, where the iridium oxide loading rate is 2mg / cm 2 (in terms of metallic iridium); the solid electrolyte is a hydrogen-type ion exchange resin composed of a styrene-divinylbenzene copolymer, the model of which is 50WX8, particle size is 400 mesh. The solid electrolyte was ion exchanged in 0.5 mol / L sodium sulfate solution for 24 h, and the excess sodium sulfate on the surface was washed off with deionized water before use.
[0122] 2. The gas diffusion cathode is prepared by the following method:
[0123] The catalyst, isopropanol, perfluorosulfonic acid ion polymer solution and polytetrafluoroethylene dispersion are mixed and ultrasonically dispersed to obtain a catalyst dispersion as a catalyst layer raw material. A certain amount of the catalyst dispersion is evenly sprayed on the gas diffusion electrode by a spray gun, and a gas diffusion cathode is obtained after drying;
[0124] The cathode catalyst is an oxygen vacancy bismuth catalyst prepared by chemical reduction. 2 g of bismuth trioxide nanopowder and 0.125 g of potassium borohydride are reacted in 100 mL of deionized water for 25 min, and the solid-liquid separation is performed by suction filtration through a 0.45 μm water system microporous filter membrane, and the obtained solid is freeze-dried at -60°C for 24 h to obtain an oxygen vacancy bismuth catalyst.
[0125] The amount of cathode catalyst added was 10 mg;
[0126] The purity of the isopropanol is 99.9%, and the amount added is 1 mL;
[0127] The perfluorosulfonic acid ion polymer solution model is D520, added volume 50 μL;
[0128] The concentration of the polytetrafluoroethylene dispersion is 5%, and the added amount is 40 μL;
[0129] The ultrasonic dispersion time of the catalyst dispersion is 30 minutes;
[0130] The spraying amount of the catalyst dispersion is 0.5 mL;
[0131] The drying is carried out under heating by an infrared heating lamp, the drying temperature is 45° C., and the drying time is 1 hour.
[0132] 3. The electrocatalytic reduction of carbon dioxide test was carried out using the above electrolytic cell and the gas diffusion cathode, comprising the following steps:
[0133] The electrolytic cell was assembled in the order of cathode flow channel plate, fluororubber gasket 1 (0.2 mm thick, with a 1.5×1.5 cm rectangular hole), gas diffusion cathode, anion exchange membrane, fluororubber gasket 2 (0.2 mm thick, with a 1×1 cm rectangular hole), solid electrolyte layer, fluororubber gasket 3 (0.2 mm thick, with a 1×1 cm rectangular hole), cation exchange membrane, anode catalyst, fluororubber gasket 4 (0.4 mm thick, with a 1.5×1.5 cm rectangular hole), and anode flow channel plate; 50 mL of deionized water was circulated into the solid electrolyte layer at a flow rate of 10 mL / h; 100 mL of 0.5 mol / L sulfuric acid was circulated into the anode flow channel plate at a flow rate of 30 mL / h; high-purity carbon dioxide gas (99.99 vt%) was pumped into the anode flow channel plate at a flow rate of 20 mL·min -1 cm -2 The flow rate of carbon dioxide is passed into the cathode flow channel plate, and carbon dioxide diffuses to the cathode catalyst layer; a voltage of -4V is applied to the electrolytic cell device, and timing is started after the current increases to a steady state, carbon dioxide is catalytically reduced to formate ions, and the formate ions are enriched on the surface of the solid electrolyte through the anion exchange membrane, and are washed and collected by the flowing cathode electrolyte, while water oxidation reaction occurs at the anode to produce oxygen. The method is carried out at a temperature of 20°C.
[0134] After 5 hours of electrocatalytic reaction, the current density was measured to be -121.8 mA / cm 2 The formic acid yield was measured by hydrogen nuclear magnetic resonance spectroscopy to be 10.50 mmol, the concentration of the produced formic acid solution was 0.210 mol / L, and the Faraday efficiency was 92.2%.
[0135] Comparative Example 2:
[0136] The difference with embodiment 4 is:
[0137] No solid electrolyte was placed in the polyetheretherketone plate, deionized water was directly used as the electrolyte at the cathode, and 50 mL of deionized water was circulated and pumped into the polyetheretherketone plate at a flow rate of 10 mL / L. The other conditions were the same as those in Example 3.
[0138] After 10 h of electrocatalytic reaction, there was no significant increase in the current density, and the measured current density was -14.2 mA / cm 2The yield of sodium formate was measured by hydrogen nuclear magnetic resonance spectroscopy to be 0.426 mmol, the concentration of the produced sodium formate solution was 0.852 mmol / L, and the Faraday efficiency was only 16.1%.
[0139] Experiments on the effects of metal cations on electrocatalytic carbon dioxide reduction were conducted in a flow electrolytic cell, such as Figure 3 As shown, according to the results of linear sweep voltammetry, it can be seen that the current density of electrocatalytic carbon dioxide reduction involving sodium and potassium ions is significantly higher than the current density when hydrogen ions are used as cations. This is due to the local electric field induced by metal cations. The results show that metal cations play a key role in the electrocatalytic carbon dioxide reduction, proving the necessity of introducing metal cations such as sodium ions in solid electrolytes.
[0140] Figure 4 The figure shows the stability test performance of the electrocatalytic reduction of carbon dioxide technology provided by the present invention. The test conditions are the same as those in Example 4. The first 4 hours are the start-up time of the battery. Within 50 hours after startup, the current density increases to a certain extent, reaching 150 mA / cm 2 The above results show that the Faraday efficiency is maintained above 85%, which proves that the electrocatalytic reduction of carbon dioxide technology provided by the present invention can effectively inhibit the hydrogen evolution side reaction, improve the stability of the electrolytic cell, and prepare a formic acid / sodium formate solution without electrolyte. The product can be used as a chemical raw material, energy carrier, and supplementary carbon source in sewage treatment. This technology is an excellent choice for large-scale industrial applications.
[0141] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. A method for preparing formic acid / formates by electrocatalytic reduction of carbon dioxide based on metal cation-enhanced solid electrolytes, It is characterized in that The following steps are involved: (1) Provide a solid electrolytic cell reaction device, comprising a cathode flow channel plate, a gas diffusion cathode, an anion exchange membrane, a solid electrolyte layer, a cation exchange membrane, an anode catalyst, and an anode flow channel plate arranged in sequence; the gas diffusion cathode comprises a gas diffusion layer, a microporous layer, and a cathode catalyst layer in sequence; the solid electrolyte layer is obtained by ion exchange of a solid electrolyte in an alkali metal salt solution; (2) Pass carbon dioxide gas into the cathode flow channel plate, pump cathode electrolyte and anode electrolyte into the solid electrolyte layer and anode flow channel plate respectively, apply voltage to the solid electrolytic cell reaction device, and wait for the current to gradually increase to greater than 10 mA / cm 2 Afterwards, the electrocatalytic carbon dioxide reduction reaction occurs; (3) Collecting the liquid flowing out of the solid electrolyte layer to obtain a formic acid / formate solution free of electrolyte.
2. The method according to claim 1, It is characterized in that In step (1), the solid electrolyte is a cationic solid electrolyte; And / or, the concentration of the sodium salt solution or potassium salt solution is 0.1-2 mol / L; And / or, the ion exchange time is more than 24 hours; And / or, the alkali metal in the alkali metal salt solution is selected from one or more of lithium, sodium, potassium and cesium.
3. The method according to claim 1, It is characterized in that In step (1), the cathode catalyst layer is formed by uniformly mixing cathode catalyst, alcohol solution, perfluorosulfonic acid ion polymer solution and hydrophobic agent dispersion, spraying the mixture on the surface of the microporous layer and drying the mixture.
4. The method according to claim 3, It is characterized in that The mass volume ratio of cathode catalyst to alcohol solution is (5-20): 1 mg / mL; and / or, the amount of the perfluorosulfonic acid ion polymer solution added is 20 to 50 μL / mL; and / or, the concentration of the hydrophobic agent dispersion is 5 to 20%; And / or, the addition amount of the hydrophobic agent dispersion is 5 to 25 μL / mL.
5. The method according to claim 3, It is characterized in that The cathode catalyst is selected from one or more of a metal element, a metal oxide or a metal sulfide; And / or, the alcohol in the alcohol solution includes ethanol and / or isopropanol; and / or, the hydrophobic agent is selected from polytetrafluoroethylene and / or polyvinylidene fluoride; And / or, the perfluorosulfonic acid ion polymer solution is a Nafion solution.
6. The method according to claim 5, It is characterized in that The metal element is selected from any one of bismuth, tin and indium, and the metal in the metal oxide or metal sulfide is selected from any one of bismuth, tin and indium; And / or, the metal element, metal oxide or metal sulfide is micron or nanometer powder.
7. The method according to claim 1, It is characterized in that In step (1), the anode catalyst is one or more of titanium felt loaded with iridium oxide, iridium oxide, titanium mesh, nickel foam, and nickel-iron foam; And / or, the solid electrolyte layer is a cathode electrolyte flow channel.
8. The method according to claim 1, It is characterized in that In step (2), the flow rate of the carbon dioxide gas is 0.1 to 100 mL min -1 cm -2 .
9. The method according to claim 1, It is characterized in that In step (2), the cathode electrolyte is deionized water; And / or, the anolyte is selected from one or more of sulfuric acid solution, sulfuric acid-sodium sulfate solution, sulfuric acid-potassium sulfate solution, sodium hydroxide solution, potassium hydroxide solution, sodium bicarbonate solution, and potassium bicarbonate solution.
10. The method according to claim 1, It is characterized in that In step (2), the voltage is -1 to -5 V, and the current is -10 to -1000 mA / cm 2 ; And / or, the reaction temperature of the electrocatalytic carbon dioxide reduction reaction is 0°C to 60°C.
Citation Information
Cited By
Method for electrochemical separation of organic acids and bases
CN119607886A
Method for electrochemically separating organic acids and bases
CN119607886B
Rapid evaluation method for performance of solid electrolyte reactor
CN119881022A
Method for producing high-concentration formic acid based on circulating electrolysis of tin-doped bismuth nanosheets
CN122214886A
A method for cyclic electrolysis production of high-concentration formic acid based on tin-doped bismuth nanosheets
CN122214886B