Method for cyclically preparing oxygen evolution electrode material through aqueous zinc ion battery

Manganese dioxide cathode materials are prepared through aqueous zinc ion battery cycles, and through zinc ion intercalation/extraction and pickling treatments, the electrochemical activity specific surface area is increased, solving the problems of high overpotential and high manufacturing cost of traditional precious metal catalysts, and achieving high-efficiency analysis. Oxygen electrocatalytic performance, suitable for applications in the field of water electrolysis.

CN118756196APending Publication Date: 2024-10-11CHINA UNIV OF GEOSCIENCES (WUHAN)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410758603.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Traditional precious metal catalysts have high overpotential and high manufacturing cost in the oxygen evolution reaction (OER) process of water electrolysis reaction, which limits the improvement of electrolysis reaction efficiency. The electrocatalytic performance of low-cost manganese dioxide materials needs to be further improved to replace precious metal catalysts. .

Method used

Manganese dioxide cathode materials are prepared through aqueous zinc ion battery cycles. The intercalation/extraction of zinc ions leads to an increase in material defects and an increase in the electrochemical activity specific surface area. Combined with pickling and drying processes, a high-efficiency oxygen evolution electrode material is prepared.

Benefits of technology

Significantly reduces the overpotential of the catalytic reaction, making the material's electrocatalytic activity close to that of the precious metal RuO2, reducing manufacturing costs and making it suitable for large-scale applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756196A_ABST
    Figure CN118756196A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of nano materials and electrochemistry, in particular to a method for cyclically preparing an oxygen evolution electrode material through an aqueous zinc ion battery. The invention relates to a method for cyclically preparing an oxygen evolution electrode material through an aqueous zinc ion battery, which comprises the following steps: pretreating foamed nickel, putting the pretreated foamed nickel into a KMnO4 solution, and reacting for a certain time under a certain temperature condition to obtain a manganese dioxide positive electrode material; selecting a manganese dioxide positive electrode material as a positive electrode, a zinc sheet as a negative electrode and zinc sulfate as an electrolyte to assemble the aqueous zinc ion battery; after the water-based zinc ion battery is subjected to charge-discharge cycle treatment, the manganese dioxide positive electrode material is taken out to be subjected to acid pickling, washing and drying, and the oxygen evolution electrode material can be obtained. The oxygen evolution electrode material is prepared from the charge-discharge cycle of the aqueous zinc ion battery to the failure of the battery, and the electrochemical activity specific surface area of the electrode is improved after long-time electrochemical cycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nanomaterials and electrochemical technology, and in particular to a method for preparing an oxygen evolution electrode material through circulation of an aqueous zinc ion battery. Background Art

[0002] Large-scale hydrogen production by water electrolysis is expected to alleviate the energy crisis and solve environmental pollution problems. However, the oxygen evolution reaction (OER) process in the water electrolysis reaction has a slow kinetic process and a high overpotential, which limits the improvement of the water electrolysis reaction efficiency. 2 、RuO 2 Precious metal electrocatalysts such as MgO2 can effectively reduce the overpotential of OER reaction and have excellent catalytic performance, but they are expensive and not conducive to large-scale application. 2 ) materials have the characteristics of abundant reserves and easy structural adjustment, and are widely used in batteries and electrocatalytic systems. They are considered to be one of the ideal alternative materials for precious metal catalysts. 2 The electrocatalytic performance of MnO is expected to be further improved compared with that of precious metal catalysts. Common methods include element doping and nanostructure design to adjust the 2 The electronic structure and electrochemically active specific surface area of ​​the Mn sites in the catalyst can improve the electrocatalytic performance, but many synthesis strategies often involve relatively expensive raw materials or relatively complex synthesis process systems, resulting in high manufacturing costs, which limits the large-scale commercial production and application of the materials. Summary of the invention

[0003] The present invention provides a process flow and a synthesis method for preparing a high-efficiency oxygen evolution electrode material by circulating an aqueous zinc ion battery. The operation process is simple, and the obtained manganese dioxide positive electrode material has relatively excellent electrocatalytic performance and can replace the expensive RuO 2 catalyst.

[0004] A method for preparing an oxygen evolution electrode material by circulating an aqueous zinc ion battery comprises the following steps:

[0005] After pretreatment, nickel foam was placed in KMnO 4 In the solution, after reacting for a certain period of time under certain temperature conditions, a manganese dioxide positive electrode material is obtained;

[0006] A manganese dioxide positive electrode material is selected as the positive electrode, a zinc sheet is selected as the negative electrode, and zinc sulfate is selected as the electrolyte to assemble an aqueous zinc ion battery; after the aqueous zinc ion battery is subjected to charge and discharge cycle treatment, the manganese dioxide positive electrode material is taken out for acid washing, and then washed and dried to obtain an oxygen evolution electrode material.

[0007] Furthermore, the pretreatment operation of the nickel foam is: cutting the nickel foam into a certain size, ultrasonically washing the nickel foam using hydrochloric acid and anhydrous ethanol respectively, and vacuum drying the nickel foam.

[0008] Furthermore, KMnO 4 The concentration of the solution is 1-10 mM, the concentration of hydrochloric acid is 1-6 M, and the size of the nickel foam is 4 cm*6 cm.

[0009] Further, the concentration of zinc sulfate is 0.1-3.3M.

[0010] Furthermore, the specific conditions for the charge and discharge cycle treatment of the aqueous zinc ion battery are: the aqueous zinc ion battery is charged and discharged at a rate of 0.1 to 10C until the discharge capacity of the manganese dioxide positive electrode material is reduced to less than 30% of the initial discharge capacity of the manganese dioxide positive electrode material.

[0011] Furthermore, the acid solution used for pickling is one or more of hydrochloric acid, nitric acid, sulfuric acid and acetic acid, the concentration range of the acid solution is 0.01-1 mol / L, and the pickling times are three times.

[0012] Furthermore, the drying temperature is 60 to 90° C., the drying environment is a vacuum environment, and the drying time is 6 to 24 hours.

[0013] Furthermore, the washing process is an alternating washing process using water and ethanol.

[0014] The oxygen evolution electrode material is prepared by the method for preparing the oxygen evolution electrode material through the circulation of aqueous zinc ion batteries.

[0015] Application of the above oxygen evolution electrode materials in the field of water electrolysis.

[0016] The beneficial effects of the present invention are as follows: the present invention prepares an oxygen evolution electrode material from the charge and discharge cycle of an aqueous zinc ion battery until the battery fails. After a long period of electrochemical cycle, the active material maintains the original electrode structure, and the electrochemical active specific surface area of ​​the electrode is improved. When applied to the field of oxygen evolution electrocatalysis, the overpotential of the catalytic reaction can be significantly reduced, reaching the same level as the noble metal RuO 2 Similar catalytic activity of electrocatalytic materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 is a SEM image of the oxygen evolution electrode material of Comparative Example 1 of the present invention;

[0018] Figure 2 is an LSV curve diagram of the oxygen evolution electrode material of Comparative Example 1 of the present invention;

[0019] Figure 3 is an LSV curve diagram of the oxygen evolution electrode material of Comparative Example 2 of the present invention;

[0020] Figure 4 is an LSV curve diagram of the oxygen evolution electrode material of Comparative Example 3 of the present invention;

[0021] Figure 5 is a SEM image of the oxygen evolution electrode material of Example 1 of the present invention;

[0022] Figure 6 1 is the LSV curve of the oxygen evolution electrode material of Example 1 of the present invention. DETAILED DESCRIPTION

[0023] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.

[0024] During the battery charge and discharge process, zinc ions are constantly embedded in / out of the crystal structure of the manganese dioxide material, causing the manganese dioxide lattice to be strained and produce defects. After a long battery cycle, a large number of defects are produced in the manganese dioxide electrode material, and its zinc ion storage capacity drops sharply, causing positive electrode failure. However, the large number of defects produced will cause the electrochemical specific surface area of ​​the manganese dioxide material to increase, so that the manganese metal sites with electrocatalytic activity are fully exposed, thereby improving the electrolytic water oxygen evolution performance of the material. Therefore, the present invention is through the water system zinc manganese dioxide battery cycle, in order to prepare an efficient manganese dioxide-based oxygen evolution electrode material.

[0025] A method for preparing a high-efficiency oxygen evolution electrode material by circulating an aqueous zinc ion battery of the present invention comprises the following steps:

[0026] S1. Cut a 4cm*6cm nickel foam, then use a certain concentration of hydrochloric acid and anhydrous ethanol for ultrasonic washing, and use a vacuum oven to dry the nickel foam. Then weigh a certain amount of potassium permanganate (KMnO 4 ), and dissolved it in a certain volume of deionized water, the washed nickel foam was mixed with the KMnO 4 The solutions were transferred to a 100 mL reactor and reacted at a certain temperature for a certain period of time to obtain a manganese dioxide positive electrode material;

[0027] S2, selecting the manganese dioxide positive electrode material prepared in S1 as the positive electrode, the zinc sheet as the negative electrode, and 2M zinc sulfate as the electrolyte, assembling an aqueous zinc ion battery, and disassembling the aqueous zinc ion battery in which the discharge capacity of the manganese dioxide positive electrode material is reduced to 30% of its initial discharge capacity after a long-term charge and discharge cycle at 0.1 to 10C, and taking out the manganese dioxide positive electrode material;

[0028] S3, washing the manganese dioxide positive electrode material in S2 with one or more of 0.01-1 mol / L dilute hydrochloric acid, nitric acid, sulfuric acid and acetic acid for 3 times;

[0029] S4. Wash the manganese dioxide positive electrode material in S3 with water and ethanol for several times, and then vacuum dry it at 60-90°C for 6-24h to obtain the oxygen evolution electrode material.

[0030] It should be noted that although the failed manganese dioxide positive electrode material in this step can no longer provide a high zinc ion storage capacity, after long-term electrochemical cycles, the electrode is activated and its electrochemical specific surface area is improved. There are some passivation layers such as zinc oxide and zinc hydroxide on the surface of the failed manganese dioxide positive electrode, which can be completely removed after a simple dilute acid wash, and then washed clean with water and ethanol and dried for standby use, which is conducive to subsequent electrocatalytic performance testing.

[0031] <Comparative Example 1>

[0032] A method for preparing an oxygen evolution electrode material comprises the following steps:

[0033] S1, cut 4cm*6cm nickel foam, then use 6mol·L -1 The cut nickel foam was ultrasonically washed with hydrochloric acid and anhydrous ethanol for 15 min, and then dried; 10 mmol of potassium permanganate (KMnO 4 ) and dissolved it in 80 mL of water. The washed nickel foam was mixed with the KMnO 4 The solution was transferred to a 100 mL reactor and reacted at 160° C. for 10 h to obtain a manganese dioxide positive electrode material;

[0034] S2, washing the manganese dioxide positive electrode material in S1 with 0.1 mol / L dilute hydrochloric acid for 3 times;

[0035] S3. The manganese dioxide positive electrode material in S2 was washed with water and ethanol for several times, and then vacuum dried at 60°C for 12 h to obtain an oxygen evolution electrode material.

[0036] The scanning electron microscope image of the oxygen evolution electrode material prepared in this comparative example is as follows Figure 1 As shown in the figure, the original manganese dioxide active material is a two-dimensional nanosheet structure with a layer thickness of about 23.1nm. After electrochemical evaluation, it was found that its active specific surface area is 95.3cm -2 The electrode was used for water electrolysis test and found that Figure 2 The LSV curves show that the original manganese dioxide has a -2 The overpotential at a current density of 388 mV.

[0037] <Comparative Example 2>

[0038] A method for preparing an oxygen evolution electrode material comprises the following steps:

[0039] S1, cut 4cm*6cm nickel foam, then use 6mol·L -1 The cut nickel foam was ultrasonically washed with hydrochloric acid and anhydrous ethanol for 15 min, and then dried; 10 mmol of potassium permanganate (KMnO 4 ) and dissolved it in 80 mL of water. The washed nickel foam was mixed with the KMnO 4 The solution was transferred to a 100 mL reactor and reacted at 160° C. for 10 h to obtain a manganese dioxide positive electrode material;

[0040] S2, selecting the manganese dioxide positive electrode material prepared in S1 as the positive electrode, the zinc sheet as the negative electrode, and 2M zinc sulfate as the electrolyte, assembling an aqueous zinc ion battery, disassembling the aqueous zinc ion battery after 10 cycles of charge and discharge under 5C conditions, and taking out the manganese dioxide positive electrode material;

[0041] S3, washing the manganese dioxide positive electrode material in S2 with 0.1 mol / L dilute hydrochloric acid three times;

[0042] S4. Wash the manganese dioxide positive electrode material in S3 with water and ethanol three times, and vacuum dry it at 60°C for 12 hours to obtain the oxygen evolution electrode material.

[0043] The oxygen evolution electrode material prepared in this comparative example has a discharge capacity of 90% of the initial discharge capacity after 10 charge and discharge cycles. Electrochemical evaluation found that its active specific surface area is 99.4 cm -2 The electrode was used for water electrolysis test and found that Figure 3 The LSV curves show that the unfailed manganese dioxide electrode has a -2 The overpotential at the current density is 379 mV, which indicates that the electrochemical active area of ​​the non-failed manganese dioxide electrode is limited, resulting in almost unchanged oxygen evolution electrocatalytic activity of the electrode material.

[0044] <Comparative Example 3>

[0045] A non-acid-washed spent manganese dioxide positive electrode material, comprising the following steps:

[0046] S1, cut 4cm*6cm nickel foam, then use 6mol·L -1 The cut nickel foam was ultrasonically washed with hydrochloric acid and anhydrous ethanol for 15 min and then dried. 10 mmol of potassium permanganate (KMnO 4 ) and dissolved it in 80 mL of water. The washed nickel foam was mixed with the KMnO 4 The solution was transferred to a 100 mL reactor and reacted at 160° C. for 10 h to obtain a manganese dioxide positive electrode material;

[0047] S2, selecting the manganese dioxide positive electrode material prepared in S1 as the positive electrode, the zinc sheet as the negative electrode, and 2M zinc sulfate as the electrolyte, assembling an aqueous zinc ion battery, disassembling the aqueous zinc ion battery after 200 cycles of charge and discharge under 5C conditions, and taking out the manganese dioxide positive electrode material;

[0048] S3. Wash the manganese dioxide positive electrode material in S2 with water and ethanol three times, and then vacuum dry it at 60°C for 12 hours to obtain the oxygen evolution electrode material.

[0049] The oxygen evolution electrode material prepared in this comparative example has a discharge capacity of 26% of the initial discharge capacity after 200 charge and discharge cycles. The electrochemical evaluation found that its active specific surface area is 126.3 cm -2 The electrode was used for water electrolysis test and found that Figure 4 The LSV curves show that the unfailed manganese dioxide electrode has a -2 The overpotential at a current density of 336 mV is 336 mV, which proves that there is a passivation layer of zinc oxide or zinc hydroxide on the electrode surface, which is not conducive to improving the electrochemical active specific surface area and oxygen evolution electrocatalytic activity of the electrode.

[0050] <Example 1>

[0051] A method for preparing an oxygen evolution electrode material by circulating an aqueous zinc ion battery comprises the following steps:

[0052] S1, cut 4cm*6cm nickel foam, then use 6mol·L -1 The cut nickel foam was ultrasonically washed with hydrochloric acid and anhydrous ethanol for 15 min, and then dried; 10 mmol of potassium permanganate (KMnO 4 ) and dissolved it in 80 mL of water. The washed nickel foam was mixed with the KMnO 4 The solution was transferred to a 100 mL reactor and reacted at 160° C. for 10 h to obtain a manganese dioxide positive electrode material;

[0053] S2, selecting the manganese dioxide positive electrode material prepared in S1 as the positive electrode, the zinc sheet as the negative electrode, and 2M zinc sulfate as the electrolyte, assembling an aqueous zinc ion battery, disassembling the aqueous zinc ion battery after 200 cycles of charge and discharge under 5C conditions, and taking out the manganese dioxide positive electrode material;

[0054] S3, washing the manganese dioxide positive electrode material in S2 with 0.1 mol / L dilute hydrochloric acid three times;

[0055] S4. Wash the manganese dioxide positive electrode material in S3 with water and ethanol for several times, and then vacuum dry it at 60°C for 12 hours to obtain the oxygen evolution electrode material.

[0056] The oxygen evolution electrode material prepared in Example 1 was characterized by scanning electron microscopy, and the results are as follows: Figure 5 As shown in the figure, the microstructure of the recovered manganese dioxide is still a nanosheet structure. Figure 1 By comparison, the thickness of the nanosheets of the material has not changed significantly and is still about 24.1nm. Through the electrochemical active surface area test, it was found that after the battery charge and discharge cycle and the dilute hydrochloric acid washing, the electrochemical active surface area of ​​the oxygen evolution electrode material was effectively increased to 160.5cm -2 .like Figure 6 As shown, it was found that the material -2 At a current density of 1.3 Å, the overpotential of the electrode is only 308 mV, which is comparable to the commercial RuO 2 The electrocatalyst is prepared, and the overpotential is reduced by 80 mV compared with the non-failed manganese dioxide electrode material prepared in Comparative Example 1. The above results show that the oxygen evolution electrode material of this embodiment has excellent electrocatalytic performance, and the manganese dioxide prepared by the present invention has great application prospects in the field of water electrolysis, which is conducive to the realization of industrial development and application.

[0057] <Example 2>

[0058] A method for preparing an oxygen evolution electrode material by circulating an aqueous zinc ion battery comprises the following steps:

[0059] S1, cut 4cm*6cm nickel foam, then use 6mol·L -1 The cut nickel foam was ultrasonically washed with hydrochloric acid and anhydrous ethanol for 15 min and then dried. 10 mmol of potassium permanganate (KMnO 4 ) and dissolved it in 80 mL of water. The washed nickel foam was mixed with the KMnO 4 The solution was transferred to a 100 mL reactor and reacted at 160° C. for 10 h to obtain a manganese dioxide positive electrode material;

[0060] S2, selecting the manganese dioxide positive electrode material prepared in S1 as the positive electrode, the zinc sheet as the negative electrode, and 2M zinc sulfate as the electrolyte, assembling an aqueous zinc ion battery, disassembling the aqueous zinc ion battery after 200 cycles of charge and discharge under 2C conditions, and taking out the manganese dioxide positive electrode material;

[0061] S3, washing the manganese dioxide positive electrode material in S2 with 0.1 mol / L dilute hydrochloric acid three times;

[0062] S4. Wash the manganese dioxide positive electrode material in S3 with water and ethanol for several times, and then vacuum dry it at 60°C for 12 hours to obtain the oxygen evolution electrode material.

[0063] This embodiment changes the cycle rate conditions of the aqueous zinc battery. After 200 charge and discharge cycles, the discharge capacity is 11% of the initial discharge capacity. The electrocatalytic performance test of the obtained oxygen evolution electrode material shows that the material has a high conductivity at 10 mA cm -2 At a current density of , the oxygen evolution overpotential of the electrode is 310 mV. Compared with Example 1, its electrocatalytic performance is almost unchanged.

[0064] <Example 3>

[0065] A method for preparing an oxygen evolution electrode material by circulating an aqueous zinc ion battery comprises the following steps:

[0066] S1, cut 4cm*6cm nickel foam, then use 6mol·L -1 The cut nickel foam was ultrasonically washed with hydrochloric acid and anhydrous ethanol for 15 min and then dried. 10 mmol of potassium permanganate (KMnO 4 ) and dissolved it in 80 mL of water. The washed nickel foam was mixed with the KMnO 4 The solution was transferred to a 100 mL reactor and reacted at 160° C. for 10 h to obtain a manganese dioxide positive electrode material;

[0067] S2, selecting the manganese dioxide positive electrode material prepared in S1 as the positive electrode, the zinc sheet as the negative electrode, and 2M zinc sulfate as the electrolyte, assembling an aqueous zinc ion battery, disassembling the aqueous zinc ion battery after 200 cycles of charge and discharge under 0.1C conditions, and taking out the manganese dioxide positive electrode material;

[0068] S3, washing the manganese dioxide positive electrode material in S2 with 1 mol / L dilute sulfuric acid three times;

[0069] S4. Wash the manganese dioxide positive electrode material in S3 with water and ethanol for several times, and then vacuum dry it at 60°C for 12 hours to obtain the oxygen evolution electrode material.

[0070] In this example, the concentration of dilute hydrochloric acid was changed, and the electrocatalytic performance of the recovered manganese dioxide electrode material was tested. It was found that the material -2 At a current density of , the oxygen evolution overpotential of the electrode is 306 mV. Compared with Example 1, its electrocatalytic performance is almost unchanged.

[0071] <Example 4>

[0072] A method for preparing an oxygen evolution electrode material by circulating an aqueous zinc ion battery comprises the following steps:

[0073] S1, cut 4cm*6cm nickel foam, then use 6mol·L -1The cut nickel foam was ultrasonically washed with hydrochloric acid and anhydrous ethanol for 15 min and then dried. 10 mmol of potassium permanganate (KMnO 4 ) and dissolved it in 80 mL of water. The washed nickel foam was mixed with the KMnO 4 The solution was transferred to a 100 mL reactor and reacted at 160° C. for 10 h to obtain a manganese dioxide positive electrode material;

[0074] S2, selecting the manganese dioxide positive electrode material prepared in S1 as the positive electrode, the zinc sheet as the negative electrode, and 2M zinc sulfate as the electrolyte, assembling an aqueous zinc ion battery, disassembling the aqueous zinc ion battery after 200 cycles of charge and discharge under 5C conditions, and taking out the manganese dioxide positive electrode material;

[0075] S3, washing the manganese dioxide positive electrode material in S2 with 0.5 mol / L dilute nitric acid three times;

[0076] S4. Wash the manganese dioxide positive electrode material in S3 with water and ethanol for several times, and then vacuum dry it at 90°C for 6 hours to obtain the oxygen evolution electrode material.

[0077] This example changes the temperature and time of vacuum drying, and tests the electrocatalytic performance of the oxygen evolution electrode material prepared in this example. It is found that the material has a high conductivity at 10 mA cm -2 At a current density of , the oxygen evolution overpotential of the electrode is 315 mV. Compared with Example 1, its electrocatalytic performance is almost unchanged.

[0078] <Example 5>

[0079] A method for preparing an oxygen evolution electrode material by circulating an aqueous zinc ion battery comprises the following steps:

[0080] S1, cut 4cm*6cm nickel foam, then use 6mol·L -1 The cut nickel foam was ultrasonically washed with hydrochloric acid and anhydrous ethanol for 15 min and then dried. 10 mmol of potassium permanganate (KMnO 4 ) and dissolved it in 80 mL of water. The washed nickel foam was mixed with the KMnO 4 The solution was transferred to a 100 mL reactor and reacted at 160° C. for 10 h to obtain a manganese dioxide positive electrode material;

[0081] S2, selecting the manganese dioxide positive electrode material prepared in S1 as the positive electrode, the zinc sheet as the negative electrode, and 0.1M zinc sulfate as the electrolyte, assembling an aqueous zinc ion battery, disassembling the aqueous zinc ion battery after 200 cycles of charge and discharge under 0.1C conditions, and taking out the manganese dioxide positive electrode material;

[0082] S3, washing the manganese dioxide positive electrode material in S2 with a mixed acid solution of 0.5 mol / L dilute hydrochloric acid and 0.5 mL dilute acetic acid for 3 times;

[0083] S4. Wash the manganese dioxide positive electrode material in S3 with water and ethanol for several times, and then dry it in vacuum at 90°C for 24 hours to obtain the oxygen evolution electrode material.

[0084] <Example 6>

[0085] A method for preparing an oxygen evolution electrode material by circulating an aqueous zinc ion battery comprises the following steps:

[0086] S1, cut 4cm*6cm nickel foam, and then use 1mol·L -1 The cut nickel foam was ultrasonically washed with hydrochloric acid and anhydrous ethanol for 15 min and then dried. 10 mmol of potassium permanganate (KMnO 4 ) and dissolved it in 80 mL of water. The washed nickel foam was mixed with the KMnO 4 The solution was transferred to a 100 mL reactor and reacted at 160° C. for 10 h to obtain a manganese dioxide positive electrode material;

[0087] S2, selecting the manganese dioxide positive electrode material prepared in S1 as the positive electrode, the zinc sheet as the negative electrode, and 0.1M zinc sulfate as the electrolyte, assembling an aqueous zinc ion battery, disassembling the aqueous zinc ion battery after 200 cycles of charge and discharge under 3C conditions, and taking out the manganese dioxide positive electrode material;

[0088] S3, washing the manganese dioxide positive electrode material in S2 with 0.5 mol / L dilute hydrochloric acid three times;

[0089] S4. Wash the manganese dioxide positive electrode material in S3 with water and ethanol for several times, and then vacuum dry it at 90°C for 6 hours to obtain the oxygen evolution electrode material.

[0090] In the absence of conflict, the above embodiments and features in the embodiments may be combined with each other.

[0091] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an oxygen evolution electrode material by circulating an aqueous zinc ion battery, characterized in that: The following steps are involved: After pretreatment, the nickel foam is placed in a KMnO4 solution and reacted for a certain time at a certain temperature to obtain a manganese dioxide positive electrode material; A manganese dioxide positive electrode material is selected as the positive electrode, a zinc sheet is selected as the negative electrode, and zinc sulfate is selected as the electrolyte to assemble an aqueous zinc ion battery; after the aqueous zinc ion battery is subjected to charge and discharge cycle treatment, the manganese dioxide positive electrode material is taken out and sequentially subjected to acid washing, washing and drying treatment to obtain an oxygen evolution electrode material.

2. A method for preparing an oxygen evolution electrode material by circulating an aqueous zinc ion battery according to claim 1, characterized in that: The pretreatment operation of the nickel foam is: cutting the nickel foam into a certain size, washing the nickel foam with hydrochloric acid and anhydrous ethanol by ultrasonic, and then drying the nickel foam in vacuum.

3. A method for preparing an oxygen evolution electrode material by circulating an aqueous zinc ion battery according to claim 2, characterized in that: The concentration of KMnO4 solution is 1-10mM, the concentration of hydrochloric acid is 1-6M, and the size of nickel foam is 4cm*6cm.

4. The method for preparing oxygen evolution electrode materials by circulating aqueous zinc ion batteries according to claim 1, characterized in that: The concentration of zinc sulfate is 0.1-3.3M.

5. The method for preparing oxygen evolution electrode materials by circulating aqueous zinc ion batteries according to claim 1, characterized in that: The specific conditions for the charge and discharge cycle treatment of the aqueous zinc ion battery are: the aqueous zinc ion battery is charged and discharged at a rate of 0.1 to 5C until the discharge capacity of the manganese dioxide positive electrode material is reduced to less than 30% of the initial discharge capacity of the manganese dioxide positive electrode material.

6. The method for preparing oxygen evolution electrode materials by circulating aqueous zinc ion batteries according to claim 1, characterized in that: The acid solution used for pickling is one or more of hydrochloric acid, nitric acid, sulfuric acid and acetic acid, the concentration range of the acid solution is 0.1-1 mol / L, and the pickling times are three times.

7. The method for preparing oxygen evolution electrode materials by circulating aqueous zinc ion batteries according to claim 1, characterized in that: The drying temperature is 60-90°C, the drying environment is a vacuum environment, and the drying time is 6-24 hours.

8. The method for preparing oxygen evolution electrode materials by circulating aqueous zinc ion batteries according to claim 1, characterized in that: The washing process is to use water and ethanol alternately.

9. The oxygen evolution electrode material prepared by the method for preparing oxygen evolution electrode material by circulating an aqueous zinc ion battery according to claims 1-8.

10. Use of the oxygen evolution electrode material according to claim 9 in the field of water electrolysis.