Method for producing high-purity gold based on diaphragm electrolytic refining

The processing process of separating gold and base metals through diaphragm electrolysis, combined with the automated operation of PLC control panel, solves the problems of gold backlog and long production cycle in traditional gold purification methods, achieves stable and automated production of high-purity gold, and reduces environmental protection and labor costs.

CN118756249APending Publication Date: 2024-10-11YUNNAN DIANJIN INVESTMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410831884.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing gold purification methods, such as traditional electrolytic refining, solvent extraction and chemical reduction, have a large backlog of gold, long production cycles, poor adaptability of raw materials, high pressure on safety and environmental protection, high labor intensity, high cost and poor stability when preparing high-purity gold. problem.

Method used

The diaphragm electrolysis method is used to separate the gold dissolution tank and the base metal reduction tank through the diaphragm. The PLC control panel is used to perform the electrochemical dissolution and electrowinning precipitation process to avoid gold backlog, improve the stability of high-purity gold, and realize automated production.

Benefits of technology

It reduces the gold backlog, improves the stability and automation of high-purity gold, reduces production costs and environmental risks, simplifies processes, and improves raw material adaptability and labor efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756249A_ABST
    Figure CN118756249A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of gold purification, and discloses a method for producing high-purity gold based on diaphragm electrolytic refining, which comprises the following operation steps: S1, before operation, a gold dissolving tank A, a base metal reduction tank B, a gold dissolving tank C, a gold reduction tank D, a current balance tank E and a gold reduction tank F are filled and separated by diaphragms; according to the method, the diaphragm is ingeniously adopted to separate the tank body, the gold dissolution process and the gold precipitation process are separated, a pregnant solution does not need to be prepared, gold accumulation is greatly reduced, meanwhile, base metal ions enter the base metal reduction tank through the diaphragm, the stability of high-purity gold is further improved, and toxic and harmful gases such as hydrogen sulfide, nitric oxide and sulfur dioxide are not generated in the whole process; meanwhile, no waste water or waste residues are generated, safety and environmental protection risks caused by three wastes are reduced, automatic production can be achieved by adopting PLC control in the gold dissolution and electrodeposition precipitation process and setting corresponding parameters, manual intervention is not needed, the automation degree is high, and the labor intensity is small.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gold purification, and in particular to a method for producing high-purity gold based on diaphragm electrolytic refining. Background Art

[0002] At present, the gold purification methods commonly used by gold production enterprises mainly include solvent extraction, traditional electrolytic refining, chlorination refining and chemical reduction. Various purification processes have their specific application scope and advantages and disadvantages. When preparing high-purity gold, most refineries use traditional electrolytic refining, solvent extraction and chemical reduction.

[0003] Traditional electrolytic refining method: The traditional electrolytic refining method has the following disadvantages when preparing high-purity gold: 1. It needs to make liquid, that is, gold mother liquor, which will cause a large backlog of gold. 2. The traditional electrolytic refining method requires two electrolysis processes to prepare high-purity gold. The first electrolysis produces 99.997% of 1# gold, and the second anode plate is cast, and then the second electrolysis produces 99.999% high-purity gold, resulting in a long production cycle. 3. In the traditional electrolytic refining method, the gold anode plate dissolution and gold electrolytic deposition are both in the same tank. When the impurity content of the anode plate is high, first, the impurities are enriched in the mother liquor and affect the electrolysis efficiency. Second, the impurities will be precipitated on the cathode plate with the gold and affect the stability of the high-purity gold. That is, this method of preparing high-purity gold has poor adaptability to raw materials.

[0004] Solvent extraction method: The solvent extraction method has the following disadvantages when preparing high-purity gold: 1. The extraction process uses a large amount of organic solvents, which are toxic, flammable and explosive, and have high requirements for equipment and safety. The amount of three wastes produced is large, the working environment is poor, the degree of automation is low, and there is organic pollution. 2. The extraction process is an endothermic reaction and needs to be carried out under high temperature conditions, which further aggravates the volatilization of organic solvents; the extraction process is slow and the gold recovery rate is low. 3. In the extraction method, the oil phase and gold will combine and are not easy to separate, which affects the subsequent cleaning and drying of the gold powder.

[0005] Chemical reduction method: The chemical reduction method has the following disadvantages when preparing high-purity gold: 1. The equipment is large, the degree of automation is low, the labor intensity is high, there are many processes, and the production cycle is long. 2. This method produces a large amount of toxic and harmful gases such as hydrogen sulfide, nitrogen oxides, and sulfur dioxide during the production process, which puts great pressure on the environmental protection. 3. During the aqua regia gold dissolution process, silver chloride wraps the crude gold, reducing the dissolution rate of the crude gold, so the amount of acid is increased on the basis of the theoretical amount of acid, further increasing the cost and environmental pressure. 4. The method adds reagents based on experience in the removal of nitrate and reduction stages, which will directly affect the purity of the gold powder, so the stability of high-purity gold is poor.

[0006] In order to solve the problems in the preparation process of high-purity gold, the traditional electrolytic refining method contains a large backlog of gold, a long production cycle, and poor raw material adaptability; the solvent extraction method contains a large amount of organic solvent usage, high safety requirements, a large amount of three wastes generated, a low gold recovery rate, and difficulty in separating gold powder; the chemical reduction method contains the disadvantages of high labor intensity, long cycle, high cost, high environmental pressure, poor stability, etc. Therefore, the present invention proposes a method for producing high-purity gold based on diaphragm electrolytic refining. Summary of the invention

[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions: A method for producing high-purity gold based on diaphragm electrolytic refining, comprising the following specific operating steps:

[0008] S1. Before operation, separate the gold dissolution tank A, base metal reduction tank B, gold dissolution tank C, gold reduction tank D, current balance tank E, and gold reduction tank F with diaphragms, inject clean water into the gold dissolution tank A, base metal reduction tank B, gold dissolution tank C, gold reduction tank D, current balance tank E, and gold reduction tank F to ensure that there is no leakage between the tanks, and drain the clean water;

[0009] S2, inject E1 type electrolyte into gold dissolution tank A, gold dissolution tank C, gold reduction tank D, and gold reduction tank F at the same time, inject E2 type electrolyte into base metal reduction tank B and current balance tank E at the same time, and set transfer tank G on one side of gold dissolution tank A, and set transfer tank H on one side of gold reduction tank F, wherein gold dissolution tank A, gold reduction tank D, and transfer tank G are a group, and gold dissolution tank C, gold reduction tank F, and transfer tank H are a group;

[0010] S3, hang the gold anode plate into the gold dissolving tank A and the gold dissolving tank C, set the corresponding parameters through the PLC control panel, and perform electrochemical dissolution into gold dissolving precious liquid, silver generates silver chloride and precipitates at the bottom of the gold dissolving tank A and the gold dissolving tank C, and the base metal selectively enters the base metal reduction tank B and the current balance tank E through the diaphragm for reduction;

[0011] S4, hang the cathode plate into the gold reduction tank D and the gold reduction tank F. After the gold anode plate is dissolved, pump the E1 electrolyte in the gold reduction tank D and the gold reduction tank F into the corresponding transfer tank G and the transfer tank H. The gold dissolving precious liquid in the gold dissolving tank A and the gold dissolving tank C is pumped into the corresponding gold reduction tank D and the gold reduction tank F through the pump. Set the corresponding parameters through the PLC control panel to perform gold electrolytic deposition and attach it to the cathode plate. At the same time, pump the E1 electrolyte in the transfer tank G and the transfer tank H into the gold dissolving tank A and the gold dissolving tank C. Repeat S3;

[0012] S5. After the gold electrolytic deposition is completed, the cathode plate is taken out, rinsed with pure water and the gold sheet is peeled off. Meanwhile, the gold dissolving in the gold dissolving tank A and the gold dissolving tank C is completed, and the electrolytic lean liquid formed in the gold reduction tank D and the gold reduction tank F is transferred to the corresponding transfer tank G and the transfer tank H, and the gold dissolved precious liquid in the gold dissolving tank A and the gold dissolving tank C is pumped into the corresponding gold reduction tank D and the gold reduction tank F again through a pump, and the gold reduction tank D and the gold reduction tank F start the second round of electrolytic deposition, and the electrolytic lean liquid in the transfer tank G and the transfer tank H is transferred to the gold dissolving tank A and the gold dissolving tank C to continue the gold anode plate dissolving;

[0013] S6. Repeat steps S3-S5 to complete the whole process of high-purity gold diaphragm electrolytic refining.

[0014] Preferably, in said S1, the components of the E1 type electrolyte are specifically as follows according to the mass ratio:

[0015] Hydrochloric acid (HCL, concentration) 1-5%, sodium sulfate 8-10%, sodium bisulfate 6-7%, pure water 80% (balance), used for dissolving gold and sinking silver.

[0016] Preferably, in said S1, the composition of the E2 type electrolyte is specifically:

[0017] Sulfuric acid (concentration) 5-10%, sodium sulfate 8-12%, sodium bisulfate 7-8%, pure water 75% (balance) are used for electrolytic deposition of gold.

[0018] Preferably, the cathode plates in the gold reduction tank D and the gold reduction tank F in S1 are made of pure titanium material.

[0019] Preferably, the method uses electrolytic gold mud, alloy gold, and wet gold mud as raw materials.

[0020] Preferably, the Au color purity of the gold anode plate is greater than 95%, and the dissolution and electrodeposition temperature in S2-S4 is 50-60°C.

[0021] Preferably, two cathode plates are hung in each of the gold reduction tanks D and F, and four anode plates are hung in each of the A and C tanks.

[0022] Preferably, when the gold anode plate is dissolved, its parameter voltage is set to 6V, 5V, 4V, 3V in a step-like manner, with a total time of 12 hours, showing a 4-3-3-2 distribution.

[0023] Preferably, during electroplating, the parameter current should be 260A, 220A, 180A, 150A in a step-like manner, with a total time of 12 hours, showing a 4-4-2-2 distribution.

[0024] Preferably, Au in the gold anode plate is greater than 95%, and the total color of the gold sheet is 99.999%.

[0025] The present invention provides a method for producing high-purity gold based on diaphragm electrolytic refining. It has the following beneficial effects:

[0026] 1. The method of the present invention cleverly uses a diaphragm to separate the tank body, separate the gold dissolution and gold precipitation processes, and does not require the preparation of precious liquid, which greatly reduces the gold backlog. At the same time, the base metal ions enter the base metal reduction tank through the diaphragm, further improving the stability of high-purity gold.

[0027] 2. The method of the present invention does not produce toxic and harmful gases such as hydrogen sulfide, nitrogen oxides, sulfur dioxide, etc. during the entire process, and no waste water or waste residue is generated, thereby reducing the safety and environmental risks brought by the three wastes.

[0028] 3. The gold dissolution and electrolytic deposition process of the method of the present invention is controlled by PLC, and the corresponding parameters can be set to realize automatic production without manual intervention, with a high degree of automation and low labor intensity.

[0029] 4. The method of the present invention has strong adaptability to raw materials, can produce high-purity gold by electrolysis in one time, and has extremely low concentration of barren liquid, thereby reducing the overall production cost and achieving good economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 : Schematic diagram of the main body of the electrolytic device of a method for producing high-purity gold based on diaphragm electrolytic refining of the present invention.

[0031] Figure 2 : A process flow chart of a method for producing high-purity gold based on diaphragm electrolytic refining of the present invention. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] Example:

[0034] A method for producing high-purity gold based on diaphragm electrolytic refining includes the following specific operating steps:

[0035] S1. Before operation, separate the gold dissolution tank A, base metal reduction tank B, gold dissolution tank C, gold reduction tank D, current balance tank E, and gold reduction tank F with diaphragms, inject clean water into the gold dissolution tank A, base metal reduction tank B, gold dissolution tank C, gold reduction tank D, current balance tank E, and gold reduction tank F to ensure that there is no leakage between the tanks, and drain the clean water;

[0036] S2, inject E1 type electrolyte into gold dissolution tank A, gold dissolution tank C, gold reduction tank D, and gold reduction tank F at the same time, inject E2 type electrolyte into base metal reduction tank B and current balance tank E at the same time, and set transfer tank G on one side of gold dissolution tank A, and set transfer tank H on one side of gold reduction tank F, wherein gold dissolution tank A, gold reduction tank D, and transfer tank G are a group, and gold dissolution tank C, gold reduction tank F, and transfer tank H are a group;

[0037] S3, hang the gold anode plate into the gold dissolving tank A and the gold dissolving tank C, set the corresponding parameters through the PLC control panel, and perform electrochemical dissolution into gold dissolving precious liquid, silver generates silver chloride and precipitates at the bottom of the gold dissolving tank A and the gold dissolving tank C, and the base metal selectively enters the base metal reduction tank B and the current balance tank E through the diaphragm for reduction;

[0038] S4, hang the cathode plate into the gold reduction tank D and the gold reduction tank F. After the gold anode plate is dissolved, pump the E1 electrolyte in the gold reduction tank D and the gold reduction tank F into the corresponding transfer tank G and the transfer tank H. The gold dissolving precious liquid in the gold dissolving tank A and the gold dissolving tank C is pumped into the corresponding gold reduction tank D and the gold reduction tank F through the pump. Set the corresponding parameters through the PLC control panel to perform gold electrolytic deposition and attach it to the cathode plate. At the same time, pump the E1 electrolyte in the transfer tank G and the transfer tank H into the gold dissolving tank A and the gold dissolving tank C. Repeat S3;

[0039] S5. After the gold electrolytic deposition is completed, the cathode plate is taken out, rinsed with pure water and the gold sheet is peeled off. Meanwhile, the gold dissolving in the gold dissolving tank A and the gold dissolving tank C is completed, and the electrolytic lean liquid formed in the gold reduction tank D and the gold reduction tank F is transferred to the corresponding transfer tank G and the transfer tank H, and the gold dissolving precious liquid in the gold dissolving tank A and the gold dissolving tank C is pumped into the corresponding gold reduction tank D and the gold reduction tank F again through a pump, and the gold reduction tank D and the gold reduction tank F start the second round of electrolytic deposition, and the electrolytic lean liquid in the transfer tank G and the transfer tank H is transferred to the gold dissolving tank A and the gold dissolving tank C to continue the gold anode plate dissolving;

[0040] S6. Repeat steps S3-S5 to complete the whole process of high-purity gold diaphragm electrolytic refining.

[0041] Among them, the components of E1 type electrolyte are as follows by mass: 1-5% hydrochloric acid (measured by HCL mass), 8-10% sodium sulfate, 7% sodium bisulfate, and 80% pure water, which are used for dissolving gold and sinking silver; the components of E2 type electrolyte are as follows by mass: 5-10% sulfuric acid (measured by H2SO4 mass), 10% sodium sulfate, 7% sodium bisulfate, and 75% pure water, which are used for electrolytic deposition of gold.

[0042] The method of producing high-purity gold by diaphragm electrolytic refining uses electrolytic gold mud, gold alloy and wet gold mud as raw materials, controls the Au color of the anode plate to be greater than 95%, and the dissolution and electrolytic deposition temperature is 55°C. The weight of the anode plate is 2.5kg / piece, the size is 140*5*180mm, each group of electrolytic cells hangs 4 anode plates, the total weight of the gold anode plates is 20kg, and the reduction cell hangs 2 titanium cathode plates, the size is 260*1*330mm, and the anode plate dissolution rate is above 99%.

[0043] The present invention invents a new type of diaphragm electrolytic refining method based on the traditional electrolytic refining method. The diaphragm is used to separate the cell body. The base metal ions enter the non-gold-containing liquid cell body through the diaphragm for reduction, thereby avoiding product contamination. At the same time, the adaptability of the raw materials is improved, and high-purity gold can be produced at one time. The gold dissolution and electrolytic deposition processes are controlled by PLC, and automatic production can be realized by setting corresponding parameters. This method has a good promoting effect on the preparation of high-purity gold in precious metal refineries in terms of automation level, product stability, gold backlog, environmental protection pressure, production cycle, etc., and has a good promotion value.

[0044] Experimental example:

[0045] 1. Determination of anode plate gold dissolution time, voltage and dissolution rate

[0046]

[0047]

[0048] Table 1 Statistics of dissolution process parameters

[0049] It can be seen from Table 1 that: (1) Production 1 and Production 2 have different voltages but the same time, and the dissolution rates are both greater than 99%, which meets the technical indicators. This shows that the voltage can be appropriately reduced as the anode plate residue decreases; (2) Production 2 and Production 3 have different voltages but the same time, and the dissolution rate of Production 2 is greater than 99%, which meets the technical indicators. The dissolution rate of Production 3 is less than 99%, which does not meet the technical indicators, which shows that the dissolution voltage cannot be reduced too much; (3) Production 2 and Production 4 have the same voltage but different time, and the dissolution rates are both greater than 99%, which meets the technical indicators. This shows that the time can continue to be reduced under this voltage parameter; (4) Production 4 has the same voltage as Productions 5 and 6 but different time, and the dissolution rate gradually decreases as time decreases.

[0050] To sum up: when the anode plate is dissolved, in order to ensure the gold dissolution efficiency and reduce energy consumption, its parameters should set the voltage to 6V, 5V, 4V, 3V in a step-like shape, with a total time of 12h, and a distribution of about 4-3-3-2, which is the production 4 parameters.

[0051] 2. Determination of parameters for electrolytic deposition of gold sheets

[0052]

[0053] Table 2 Statistics of electrolytic deposition process parameters

[0054] It can be seen from Table 2 that: (1) The current of production 1 is different from that of production 2, but the time is the same. The concentration of the lean solution is less than 10 mg / L, which meets the technical indicators. This shows that the current can be appropriately reduced as the concentration of the lean solution decreases; (2) The current of production 2 is different from that of production 3, but the time is the same. The concentration of the lean solution in production 3 is 13.59 mg / L, which does not meet the technical indicators. This shows that the current cannot be reduced too much; (3) The current of production 2 is the same as that of production 4, but the time is different. The concentration of the lean solution meets the technical indicators, which shows that the time can continue to be reduced under this current parameter; (4) The current of production 4 is the same as that of productions 5 and 6, but the time is different, and the concentration of the lean solution gradually increases as time decreases.

[0055] In summary: During electrolysis, considering energy consumption and electrolysis efficiency comprehensively, the reasonable parameter current should be set to 260A, 220A, 180A, 150A in a step-like shape, with a total time of 12h, and a distribution of 4-4-2-2, which is the production 4 parameters.

[0056] 3. Determination of the color of gold anode plate

[0057]

[0058] Table 3 Gold flake color analysis statistics

[0059] Taking into account the actual production and raw material conditions, raw materials with Au>90% were selected for production. It was found from Table 3 that: (1) In production 1, the color purity of the anode plate was 90%, and the color purity of the gold sheet was 99.998%, which did not meet the technical requirements; (2) In productions 2 and 3, the color purity of the anode plate was 93% and 94.2%, and the total color purity of the gold sheet was 99.999%, but the individual impurities Ag and Cu did not meet the requirements; (3) In productions 4, 5, and 6, the Au content of the anode plate was>95%, and the gold sheet was qualified.

[0060] In summary: when Au of the anode plate is greater than 95%, high-purity gold products that meet the requirements can be produced.

[0061] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for producing high-purity gold based on diaphragm electrolytic refining, characterized in that: The specific steps are as follows: S1. Before operation, separate the gold dissolution tank A, base metal reduction tank B, gold dissolution tank C, gold reduction tank D, current balance tank E, and gold reduction tank F with diaphragms, inject clean water into the gold dissolution tank A, base metal reduction tank B, gold dissolution tank C, gold reduction tank D, current balance tank E, and gold reduction tank F to ensure that there is no leakage between the tanks, and drain the clean water; S2, inject E1 type electrolyte into gold dissolution tank A, gold dissolution tank C, gold reduction tank D, and gold reduction tank F at the same time, inject E2 type electrolyte into base metal reduction tank B and current balance tank E at the same time, and set transfer tank G on one side of gold dissolution tank A, and set transfer tank H on one side of gold reduction tank F, wherein gold dissolution tank A, gold reduction tank D, and transfer tank G are a group, and gold dissolution tank C, gold reduction tank F, and transfer tank H are a group; S3, hanging the gold anode plate into the gold dissolving tank A and the gold dissolving tank C, electrochemically dissolving the gold into precious liquid, silver generates silver chloride and precipitates at the bottom of the gold dissolving tank A and the gold dissolving tank C, and the base metal selectively enters the base metal reduction tank B and the current balance tank E through the diaphragm for reduction; S4, hang the cathode plate into the gold reduction tank D and the gold reduction tank F. After the gold anode plate is dissolved, pump the E1 electrolyte in the gold reduction tank D and the gold reduction tank F into the corresponding transfer tank G and the transfer tank H. The gold dissolving precious liquid in the gold dissolving tank A and the gold dissolving tank C is pumped into the corresponding gold reduction tank D and the gold reduction tank F through a pump to perform gold electrolytic deposition and attach to the cathode plate. At the same time, the E1 electrolyte in the transfer tank G and the transfer tank H is pumped into the gold dissolving tank A and the gold dissolving tank C. Repeat S3; S5. After the gold electrolytic deposition is completed, the cathode plate is taken out, rinsed with pure water and the gold sheet is peeled off. Meanwhile, the gold dissolving in the gold dissolving tank A and the gold dissolving tank C is completed, and the electrolytic lean liquid formed in the gold reduction tank D and the gold reduction tank F is transferred to the corresponding transfer tank G and the transfer tank H, and the gold dissolved precious liquid in the gold dissolving tank A and the gold dissolving tank C is pumped into the corresponding gold reduction tank D and the gold reduction tank F again through a pump, and the gold reduction tank D and the gold reduction tank F start the second round of electrolytic deposition, and the electrolytic lean liquid in the transfer tank G and the transfer tank H is transferred to the gold dissolving tank A and the gold dissolving tank C to continue the gold anode plate dissolving; S6. Repeat steps S3-S5 to complete the whole process of high-purity gold diaphragm electrolytic refining.

2. The method for producing high-purity gold based on diaphragm electrolytic refining according to claim 1, characterized in that: In the S1, the components of the E1 type electrolyte are specifically as follows according to the mass ratio: 1-5% hydrochloric acid, 8-10% sodium sulfate, 6-7% sodium bisulfate, and 80% pure water are used for dissolving gold and sinking silver.

3. The method for producing high-purity gold based on diaphragm electrolytic refining according to claim 1, characterized in that: In S1, the components of the E2 type electrolyte are specifically as follows according to the mass ratio: 5-10% sulfuric acid, 8-12% sodium sulfate, 7-8% sodium bisulfate, and 75% pure water are used for electrolytic gold deposition.

4. The method for producing high-purity gold based on diaphragm electrolytic refining according to claim 1, characterized in that: The cathode plates in the gold reduction tank D and the gold reduction tank F in S1 are made of pure titanium material.

5. The method for producing high-purity gold based on diaphragm electrolytic refining according to claim 1, characterized in that: This method uses electrolytic gold mud, alloy gold and wet gold mud as raw materials.

6. The method for producing high-purity gold based on diaphragm electrolytic refining according to claim 1, characterized in that: The Au color purity of the gold anode plate is greater than 95%, and the dissolution and electrolytic deposition temperature in S2-S4 is 50-60°C.

7. The method for producing high-purity gold based on diaphragm electrolytic refining according to claim 1, characterized in that: Two cathode plates are hung in each of the gold reduction tanks D and F, and four anode plates are hung in each of the A and C tanks.

8. The method for producing high-purity gold based on diaphragm electrolytic refining according to claim 1, characterized in that: When the gold anode plate was dissolved, its parameter voltage was set to 6V, 5V, 4V, and 3V in a step-like manner, with a total time of 12h, showing a 4-3-3-2 distribution.

9. The method for producing high-purity gold based on diaphragm electrolytic refining according to claim 1, characterized in that: During electrolysis, the parameter current should be 260A, 220A, 180A, 150A in a stepped manner, with a total time of 12 hours, showing a 4-4-2-2 distribution.

10. The method for producing high-purity gold based on diaphragm electrolytic refining according to claim 1, characterized in that: The Au content in the gold anode plate is greater than 95%, and the total color of the gold sheet is 99.999%.