Method for reducing severity of lithium battery foil seersucker manufacturing process
By imitating the anode holder structure of tooling and slotting processing, the serious problem of seersucker in copper foil production is solved, uniform precipitation and consistent discharge of copper foil are achieved, and the battery process performance is improved.
Patent Information
- Application Number
- CN202410742542.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-11
AI Technical Summary
During the copper foil production process, seersucker will seriously affect the coating quality, causing the copper foil to be discounted between the roller systems, affecting the battery process performance.
By designing tooling that imitates the structure of the anode holder, pressure is applied to form a depression similar to that in actual production, and groove processing is performed to ensure that the anode plate surface is horizontally consistent and reduce the seersucker phenomenon.
It achieves uniform precipitation and consistent discharge of copper foil, reduces the severity of seersucker, and improves coating quality.
Smart Images

Figure CN118756263A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal electrolytic foil production, and in particular relates to a method for reducing the severity of a lithium battery foil seersucker process. Background Art
[0002] With the rapid development of the electronic information industry and the power battery industry in recent years, the demand for copper foil has increased step by step. In the electronics industry, copper foil is the main material for copper clad laminates (CCL) and printed circuit boards (PCB). In the field of energy storage, the excellent conductivity of copper foil makes it one of the important raw materials for lithium battery current collectors. Among the methods of producing copper foil, the electrodeposition copper method has become the mainstream process for copper foil production at home and abroad due to its cost and process advantages.
[0003] In order to speed up the performance of the battery process, each process must be optimized. The coating process in the battery cell production process is a very important link. If the copper foil is seriously seersucker during the production process, it will be folded between the rollers, affecting the quality of the coating. Summary of the invention
[0004] The purpose of the present invention is to provide a method for reducing the severity of the lithium battery foil seersucker process, by eliminating the lateral depression at the middle bolt on the surface of the anode plate when it is locked on the anode seat, so that the lateral thickness of the anode plate surface is consistent, the discharge is consistent, and the copper foil is deposited evenly, so as to solve the problems in the prior art raised in the above background technology.
[0005] To achieve the above object, the present invention adopts the following technical solution: a method for reducing the severity of lithium battery foil seersucker process, comprising the following steps:
[0006] (a) Lithium battery copper foil with a thickness of 6 μm was selected as the research object to enhance the observability of the seersucker phenomenon and the effectiveness of the test method;
[0007] (b) designing and processing a tooling that simulates the structure of the anode seat, wherein the tooling includes a positioning hole that matches the curvature of the anode tank surface, and is used to simulate the sinking phenomenon during the fixing process of the anode plate;
[0008] (c) Apply pressure to the anode plate and fix it to the fixture through the nut using an electric wrench to form a depression with a depth similar to that in actual production;
[0009] (d) The surface of the anode plate is grooved, and the size of the groove is 1391 mm in length, 26 mm in width, and 0.35 mm in depth, ensuring that it is consistent with the lowest point of the depression, thereby eliminating the lateral unevenness of the surface;
[0010] (e) After coating, the anode plate is reinstalled on the anode base of the electrolysis machine to achieve uniform precipitation of copper foil and reduce seersucker.
[0011] Preferably, in (c), the depth of the depression on the surface of the anode plate is 0.35 mm to 0.5 mm.
[0012] Preferably, in (b), the surface curvature of the tooling matches the curvature of the anode tank.
[0013] Preferably, in (d), the grooving is performed from the middle of the anode plate to both sides.
[0014] Preferably, in (e), the coating is a dielectric layer for electrochemical reaction between the copper foil and the anode plate.
[0015] Preferably, in (c), when the anode plate is fixed, the width of the recess produced at each bolt is 59 mm-61 mm, corresponding to the number of studs on the anode plate.
[0016] Preferably, in (c), the curvature of the back side of the anode plate ranges from 1020 mm to 1024 mm.
[0017] Preferably, in (b), the number of the positioning holes is 13.
[0018] Preferably, in (b), the pressure applied on the anode plate is in the range of 145N-155N.
[0019] Technical effects and advantages of the present invention: Compared with the prior art, the method for reducing the severity of lithium battery foil seersucker process proposed by the present invention has the following advantages:
[0020] The present invention selects lithium battery copper foil with a thickness of 6 μm as a research object to enhance the observability of the seersucker phenomenon and the effectiveness of the test method; designs and processes a tooling that imitates the structure of an anode seat, wherein the tooling includes a positioning hole that matches the curvature of the surface of the anode slot and is used to simulate the depression phenomenon in the process of fixing the anode plate; applies pressure to the anode plate, and uses an electric wrench to fix it on the tooling through a nut to form a depression with a depth similar to that in actual production; grooves the surface of the anode plate, and after coating, reinstalls the anode plate to the anode base of the electrolysis machine to achieve uniform precipitation of the copper foil and reduce seersucker, and eliminates the lateral depression at the middle bolt on the surface of the anode plate when the anode plate is locked on the anode seat, so that the lateral thickness of the anode plate surface is consistent, the discharge is consistent, and the copper foil precipitation is uniform, thereby reducing the severity of the seersucker and other problems. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A flow chart of a method for reducing the severity of lithium battery foil seersucker process of the present invention;
[0022] Figure 2 It is a three-dimensional structural schematic diagram of the tooling of the present invention;
[0023] Figure 3 It is a schematic diagram of the exploded structure of the tooling of the present invention;
[0024] In the figure: 1. anode plate; 2. anode base; 3. sealing pressure cap; 4. nut; 5. gasket; 6. rubber cap; 7. anode slot; 8. positioning hole. DETAILED DESCRIPTION
[0025] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0026] The present invention provides Figure 1 A method for reducing the severity of a lithium battery foil seersucker process is shown, comprising the following steps:
[0027] (a) Lithium battery copper foil with a thickness of 6 μm was selected as the research object to enhance the observability of the seersucker phenomenon and the effectiveness of the test method;
[0028] (b) designing and processing a tooling that simulates the structure of the anode seat, the tooling includes a positioning hole 8 that matches the curvature of the surface of the anode tank 7, which is used to simulate the sinking phenomenon during the fixing process of the anode plate; the curvature of the surface of the tooling matches the curvature of the anode tank; preferably, the number of the positioning holes is 13, such as Figure 2 and Figure 3 shown.
[0029] Furthermore, the tooling is used to lock the anode plate. The tooling processes 13 holes. The curvature of the main tooling surface should be close to the curvature of the anode tank surface. In this way, when the anode plate is locked, a depression will occur at the bolt, which is the same as the actual machine. It is used to simulate the process of locking the anode plate to the surface of the anode seat. In the process of installing the anode plate on the anode base of the electrolysis machine, it is fixed to the anode base by screws and nuts. The locked anode plate is fixed to the machine together with the tooling, and a groove is made in the middle. The depth of the groove is consistent with the lowest surface of the depression. In this way, the entire horizontal surface of the anode plate is the same, which can ensure the uniformity of lateral discharge.
[0030] (c) Apply pressure on the anode plate 1, the pressure range is 145N-155N, preferably 150N, and use an electric wrench to fix it to the tooling through a nut to form a depression of similar depth to that in actual production; preferably, the depth of the depression on the surface of the anode plate is 0.35mm-0.5mm, and the curvature of the back of the anode plate ranges from 1020mm-1024mm, preferably 1022mm. Furthermore, when the anode plate is fixed, the width of the depression generated at each bolt is 59mm-61mm, corresponding to the number of studs on the anode plate. There are as many strips of seersucker as there are studs on the anode plate, and the width is about 60mm, and the seersucker basically covers the entire surface.
[0031] (d) The surface of the anode plate 1 is grooved, and the grooves are made from the middle of the anode plate to both sides. The grooves are 1391 mm in length, 26 mm in width, and 0.35 mm in depth, ensuring that they are consistent with the lowest point of the depression, thereby eliminating the lateral unevenness of the surface; the depth is obtained based on the actual measurement of the foil production machine. The processed set of anode plates is removed and then coated.
[0032] (e) After the coating treatment, the coating is the dielectric layer for the electrochemical reaction between the copper foil and the anode plate, and the anode plate is reinstalled on the anode base 2 of the electrolysis machine to achieve uniform precipitation of the copper foil and reduce seersucker. During the assembly process, the rubber cap 6, the sealing pressure cap 3, the gasket 5, and the nut 4 are sequentially mounted on the bolt.
[0033] Specifically, when the anode plate is locked onto the anode tank, a pit will be formed on the surface of the anode plate due to the force of the screw. The depth of the pit is about 0.35mm-0.5mm, and the degree of depression at each bolt is inconsistent. The larger the depression at the bolt, the larger the pole distance at the bolt. Under the same current density, the thickness of the copper foil precipitated on the cathode roller is inconsistent. The position where the seersucker is produced is between two studs, with a width of about 60mm. There are n studs on the anode plate, and n-1 seersuckers. The corresponding copper foil surface density is low, and the surface density of the non-stud area is high; select 12 anode plates that have been used and withdrawn from the foil machine, clean the surface, and lock it on a tooling similar to the anode plate with a force of 150N. At this time, the anode plate will have inconsistent pits, and the anode plate is grooved horizontally with a width of 26mm, a length of 1391mm, and a depth of 0.35mm. After the grooves are opened, the coating is applied; select electrolytic ultra-thin lithium battery copper foil (thickness of 4.5μm-10μm) as the object.
[0034] The invention eliminates the lateral depression at the middle bolt on the surface of the anode plate when the anode plate is locked on the anode seat, so that the lateral thickness of the anode plate surface is uniform, the discharge is uniform, and the copper foil is uniformly precipitated, thereby reducing the severity of the seersucker and other problems.
[0035] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for reducing the severity of lithium battery foil seersucker process, It is characterized in that The following steps are involved: (a) Lithium battery copper foil with a thickness of 6 μm was selected as the research object to enhance the observability of the seersucker phenomenon and the effectiveness of the test method; (b) designing and processing a tooling that simulates the structure of the anode seat, wherein the tooling includes a positioning hole that matches the curvature of the anode tank surface, and is used to simulate the sinking phenomenon during the fixing process of the anode plate; (c) Apply pressure to the anode plate and fix it to the fixture through the nut using an electric wrench to form a depression with a depth similar to that in actual production; (d) The surface of the anode plate is grooved, and the size of the groove is 1391 mm in length, 26 mm in width, and 0.35 mm in depth, ensuring that it is consistent with the lowest point of the depression, thereby eliminating the lateral unevenness of the surface; (e) After coating, the anode plate is reinstalled on the anode base of the electrolysis machine to achieve uniform precipitation of copper foil and reduce seersucker.
2. A method for reducing the severity of lithium battery foil seersucker process according to claim 1, Features: In (c), the depth of the depression on the surface of the anode plate is 0.35 mm to 0.5 mm.
3. A method for reducing the severity of lithium battery foil seersucker process according to claim 1, Features: In (b), the surface curvature of the tooling matches the curvature of the anode tank.
4. A method for reducing the severity of lithium battery foil seersucker process according to claim 1, Features: In (d), the grooving is done from the middle of the anode plate to both sides.
5. A method for reducing the severity of lithium battery foil seersucker process according to claim 1, Features: In (e), the coating is a dielectric layer for electrochemical reaction between the copper foil and the anode plate.
6. A method for reducing the severity of lithium battery foil seersucker process according to claim 1, Features: In (c), when the anode plate is fixed, the width of the depression produced at each bolt is 59mm-61mm, corresponding to the number of studs on the anode plate.
7. A method for reducing the severity of lithium battery foil seersucker process according to claim 1, Features: In (c), the curvature of the back side of the anode plate ranges from 1020 mm to 1024 mm.
8. A method for reducing the severity of lithium battery foil seersucker process according to claim 1, Features: In (b), the number of positioning holes is 13.
9. A method for reducing the severity of lithium battery foil seersucker process according to claim 1, Features: In (b), the pressure applied on the anode plate ranges from 145N to 155N.