Electrolyte for nickel-based superalloy EBSD sample preparation and sample preparation method
By using an electrolytic solution composed of hydrofluoric acid, organic acid, ethylene glycol butyl ether and ethanol for electrolytic polishing, the problems of low sample preparation efficiency and oxide film interference of nickel-based superalloy EBSD were solved, and efficient sample preparation and The high resolution significantly improves the ability to observe and analyze the crystal structure of nickel-based superalloys.
Patent Information
- Application Number
- CN202410879658.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-11
AI Technical Summary
Nickel-based superalloys have low efficiency in the EBSD sample preparation process. The existing corrosive solution causes the formation of oxide films, interferes with electron beam reflection and scattering, reduces imaging quality and resolution, and affects the true observation and analysis of crystal structures.
An electrolytic solution composed of hydrofluoric acid, organic acid, ethylene glycol butyl ether and ethanol is used for electrolytic polishing to eliminate the oxide film, release surface residual stress, and improve polishing uniformity and resolution. The electrolyte composition ratio is hydrofluoric acid. 5% ~ 16%, organic acid 15% ~ 25%, ethylene glycol butyl ether 10% ~ 30%, ethanol 40% ~ 60%.
The EBSD sample preparation time of nickel-based superalloy is significantly shortened and the sample preparation efficiency is improved. The resolution rate reaches 99%, making it easy to observe and analyze the crystal orientation and microstructure. The sample preparation time does not exceed 0.5 hours.
Smart Images

Figure CN118758983A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-temperature alloy structure and performance analysis and detection, and particularly relates to an electrolyte and a sample preparation method for EBSD sample preparation of nickel-based high-temperature alloys. Background Art
[0002] Nickel-based superalloy is an alloy material with high strength, corrosion resistance and high temperature resistance. It also has excellent thermal fatigue resistance and oxidation resistance. It is widely used in key structural parts under high temperature and high pressure conditions such as aircraft engines, gas turbines, and automobile engines. It has broad application prospects in the fields of aerospace, energy, and automobiles. However, due to its high strength, corrosion resistance, and high temperature resistance, it is difficult to process, has poor machinability, and it is difficult to ensure the integrity of the machined surface. The formation of tensile residual stress, surface / subsurface defects, and microstructural transformation of the surface layer during processing will seriously affect the fatigue life and creep strength of key structural parts during service. Therefore, the characterization of the microstructure of nickel-based superalloy is of great significance for adjusting its processing technology and improving its application performance.
[0003] At present, nickel-based high-temperature alloys are mainly prepared by EBSD using the following methods: the nickel-based high-temperature alloy samples are pre-treated by wire cutting, pre-grinding, etc., and then mechanically polished for EBSD preparation. Mechanical polishing uses diamond grinding paste metallographic polishing from coarse to fine. The polishing is carried out with the center of the sample as the core, and the force should be light, uniform and stable during the operation. At the same time, the polishing surface should be kept moist at all times during the mechanical polishing process. The polishing cloth needs to be cleaned and replaced in each process. Finally, fine polishing is performed with long-pile soft fabric and wet alumina powder. The concentration of alumina powder should be appropriate and not too concentrated, otherwise it is easy to form an oxide film on the surface of the sample. The entire polishing process has high operating requirements and many processes. If you are not careful, it is very easy to cause sample preparation failure. The entire mechanical polishing lasts for 1 to 2 hours, and the overall sample preparation time exceeds 2 hours or even longer, resulting in low EBSD sample preparation efficiency for nickel-based high-temperature alloys.
[0004] In response to the above problems, the prior art, such as application number CN2023109576260, whose invention name is a corrosive liquid for nickel-based high-temperature alloys and a corrosion method thereof, discloses a corrosive liquid composed of hydrochloric acid, nitric acid and an organic corrosion inhibitor, which is mainly used for chemically corroding the surface layer of mechanically polished nickel-based high-temperature alloys, forming a film on the metal surface to protect the metal, thereby reducing the strong oxidizing effect of the mixed solution of pure hydrochloric acid and pure nitric acid on the metal surface, reducing the dissolution of the base metal, preventing the base metal from hydrogen embrittlement, significantly reducing corrosion pits, and obtaining an efficient corrosion morphology.
[0005] However, in the process of EBSD sample preparation of nickel-based high-temperature alloy using the etching solution, an oxide film will be formed on the surface of the nickel-based high-temperature alloy treated with the etching solution. Due to the presence of the oxide film, the reflection and scattering of the electron beam on the metal surface are interfered with, the signal-to-noise ratio of the EBSD image is reduced, the imaging quality is reduced, and the resolution rate of the sample is not high. In addition, due to the presence of the oxide film, the crystal structure and orientation of the metal surface are changed, thereby interfering with the EBSD system's collection and analysis of crystal information, resulting in misjudgment of crystal orientation, which is not conducive to the observation and analysis of the real microscopic morphology such as the sample grain structure. Summary of the invention
[0006] In view of the problems that the existing nickel-based high-temperature alloy has low efficiency in the EBSD sample preparation process and the existing etching solution is not conducive to the observation of the true microscopic morphology of the nickel-based high-temperature alloy, the present invention aims to provide an electrolyte and a sample preparation method for EBSD sample preparation of a nickel-based high-temperature alloy. The pretreated nickel-based high-temperature alloy is electropolished by using the electrolyte, which greatly shortens the EBSD sample preparation time of the nickel-based high-temperature alloy and improves the sample preparation efficiency. The resolution rate of the EBSD sample prepared by the electrolyte combined with the electrolytic polishing method of the present invention can reach 99%, which is convenient for observing and analyzing the crystal orientation and microstructure of the nickel-based high-temperature alloy.
[0007] Based on the above purpose, the technical solution adopted by the present invention is as follows: The invention provides an electrolyte for EBSD sample preparation of nickel-based high-temperature alloys. The electrolyte consists of the following components in volume percentage: 5% to 16% of hydrofluoric acid, 15% to 25% of organic acid, 10% to 30% of ethylene glycol butyl ether, and 40% to 60% of ethanol.
[0008] The present invention uses hydrofluoric acid and organic acid as core components, which is conducive to eliminating a layer of oxide film formed on the surface of the nickel-based high-temperature alloy after mechanical pre-polishing treatment, and at the same time fully releases the residual stress caused by mechanical polishing, so as to achieve the effect of electrolytic polishing of the nickel-based high-temperature alloy. Ethylene glycol butyl ether and ethanol are used as solvent components of the electrolyte, the purpose is to reduce the surface tension and surface friction during the polishing process, reduce the temperature rise of the polishing surface, and avoid the generation of oxide film. At the same time, the use of ethylene glycol butyl ether can increase the viscosity of the electrolyte, improve the quality stability of the electrolyte, help to improve the polishing uniformity, and further improve the polishing effect. The resolution rate of the EBSD sample obtained by electrolytic polishing the pre-treated nickel-based high-temperature alloy with the electrolyte of the present invention is not less than 90%, the crystal structure of the sample is clear, and the grain orientation and lattice parameter information can be accurately identified and obtained.
[0009] Preferably, the volume ratio of hydrofluoric acid to organic acid is 1:(1.5-2.5); the sum of the volume percentages of hydrofluoric acid and organic acid in the electrolyte is between 25% and 40%.
[0010] Hydrofluoric acid is corrosive to nickel-based high-temperature alloys. When used alone, it will react with the metal elements on the surface of the alloy to form metal fluorides or hydrides, causing damage and corrosion to the alloy surface. It may even penetrate into the interior of the alloy, further accelerating the corrosion process and causing excessive corrosion on the sample surface, leading to sample preparation failure. Experiments have found that when hydrofluoric acid and organic acid are used in the above-mentioned proportions, they can lightly etch the alloy surface, thereby releasing surface stress and eliminating surface oxide film.
[0011] Further experiments found that the volume percentage of hydrofluoric acid and organic acid in the electrolyte should not be too high or too low. If the content of both is too high, the etching speed will be too fast and difficult to control. If the content of both is too low, the electrolytic polishing effect cannot be achieved in a short time. Extending the polishing time may cause different dissolution rates in different areas of the metal surface due to uneven current density, which in turn causes uneven polishing effect and obvious pits and protrusions on the alloy surface.
[0012] Preferably, the organic acid comprises at least one of trifluoroacetic acid, trichloroacetic acid, methanesulfonic acid and benzenesulfonic acid.
[0013] The experiment found that the above organic acids can be used for electrolytic polishing of nickel-based high-temperature alloys after being mixed with hydrofluoric acid. Compared with other organic acids, the combination of trichloroacetic acid and hydrofluoric acid has a better effect.
[0014] Preferably, the volume ratio of ethylene glycol butyl ether to ethanol in the electrolyte is 1:(2-4).
[0015] The main function of ethylene glycol butyl ether in the electrolyte is to enhance the viscosity of the system and enhance the stability of the electrolyte. Its proper addition helps to improve the uniformity of electrolytic polishing of the surface of nickel-based high-temperature alloys. However, ethylene glycol butyl ether has low solubility in hydrofluoric acid and organic acids. When the content of ethylene glycol butyl ether in the electrolyte is too high, the electrolyte will become turbid and unusable.
[0016] Preferably, the nickel-based high temperature alloy includes Inconel 738, IN738LC and Hastelloy X.
[0017] It has been found through experiments that the electrolyte of the present invention exhibits a relatively better electrolytic polishing effect on nickel-based high-temperature alloys whose main components are nickel, chromium and tungsten.
[0018] In a second aspect, the present invention provides an electrolytic polishing method for EBSD sample preparation of nickel-based high-temperature alloys, comprising the following steps: using the pretreated nickel-based high-temperature alloy as an anode and a stainless steel plate as a cathode, and performing electrolytic polishing in the above-mentioned electrolyte, and the parameters of the electrolytic polishing are as follows: voltage of 10 to 25 V, current of 0.5 to 0.8 A, electrolysis time of 10 to 20 s, and electrolysis temperature of -10°C to 5°C.
[0019] In the electrolyte of the present invention, the voltage and current of electrolytic polishing can be controlled to realize electrolytic polishing of the nickel-based high-temperature alloy after pre-polishing under low temperature conditions, with a short polishing time and a good polishing effect.
[0020] In a third aspect, the present invention provides an EBSD sample preparation method for a nickel-based high-temperature alloy, comprising the following steps: (1) Pre-grinding: Use 800 mesh, 1500 mesh, and 2500 mesh silicon carbide sandpaper to perform coarse grinding, fine grinding, and fine grinding on the nickel-based high-temperature alloy in sequence; (2) Pre-polishing: Pre-polish the finely ground nickel-based high-temperature alloy using diamond paste of model W1 for 5 to 15 minutes; (3) Electrolytic polishing: electrolytic polishing the nickel-based high-temperature alloy sample after pre-grinding and pre-polishing in steps (1) and (2) using the electrolytic polishing method described in claim 5; (4) Cleaning: The electropolished sample is ultrasonically cleaned in ethanol and dried to obtain a nickel-based high-temperature alloy EBSD sample.
[0021] The pre-grinding and pre-polishing of nickel-based high-temperature alloy samples can also adopt other existing pretreatment processes. The pre-grinding and pre-polishing processes described in the present invention combined with the electrolytic polishing process of the present invention have a relatively good EBSD sample preparation effect on nickel-based high-temperature alloys, and the total sample preparation time does not exceed 30 minutes, and the sample preparation efficiency is high.
[0022] Compared with the prior art, the present invention has the following beneficial effects: The present invention compounds hydrofluoric acid and organic acid in a specific ratio, and controls the usage of total acid, and performs electrolytic polishing on the sample after pretreatment of the nickel-based high-temperature alloy, which can lightly etch the surface of the alloy, achieve the effects of surface stress release and elimination of surface oxide film, and at the same time, adding ethylene glycol butyl ether into the electrolyte helps to improve the uniformity of electrolytic polishing of the nickel-based high-temperature alloy surface, so that the EBSD sample resolution rate after electrolytic polishing treated by the electrolyte of the present invention is as high as 99%, the grain structure information is clearly visible, the sample preparation effect is better, and the overall sample preparation time does not exceed 0.5h, which significantly improves the sample preparation efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the grain morphology of the EBSD sample of the nickel-based high-temperature alloy Inconel 738 in Example 1; Figure 2 This is the grain morphology image of the EBSD sample of the nickel-based high-temperature alloy IN738LC in Example 2. DETAILED DESCRIPTION
[0024] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be understood by those skilled in the art that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. The test methods used in the examples are conventional methods unless otherwise specified; the materials, reagents, etc. used can be obtained from commercial sources unless otherwise specified. Example 1
[0025] This embodiment takes the nickel-based high-temperature alloy Inconel 738 as an example, and provides a method for preparing a sample by EBSD on the nickel-based high-temperature alloy based on electrolytic polishing, comprising the following steps: (1) Pre-grinding: After the nickel-based high-temperature alloy sample with a size of 8 mm × 8 mm × 3 mm was ultrasonically cleaned with ethanol, it was coarsely ground, finely ground and finely ground using 800 mesh, 1500 mesh and 2500 mesh silicon carbide sandpaper on a metallographic pre-grinding machine. At the same time, in order to avoid overheating of the sample surface during the pre-grinding process, water was added to cool it down during the pre-grinding process, and the finely ground sample was cleaned with ethanol.
[0026] (2) Pre-polishing: Pre-polish the sample after fine grinding and cleaning on a polishing machine using diamond paste model W1. Control the speed of the polishing machine to 300 rpm and polish for about 10 minutes until the surface reaches a mirror effect. Use ethanol to clean and remove the diamond paste.
[0027] (3) Electrolytic polishing: The pre-polished sample is placed in an electrolytic cell, with the nickel-based high-temperature alloy sample as the anode and the stainless steel plate as the cathode, and electrolytic polishing is performed in the electrolyte; The parameters of electrolytic polishing were as follows: voltage 10 V, current 0.8 A, electrolysis time 20 s, and electrolysis temperature 5 °C; The electrolyte is composed of the following components in volume percentage: 10% hydrofluoric acid, 15% organic acid trichloroacetic acid, 20% ethylene glycol butyl ether, and 55% ethanol; that is, the volume percentage of total acid in the electrolyte is 25%, the volume percentage of organic solvent is 75%, the volume ratio of hydrofluoric acid to trichloroacetic acid in the total acid is 1:1.5; the volume ratio of ethylene glycol butyl ether to ethanol in the organic solvent is 1:2.75.
[0028] The mixing order and method of the components in the electrolyte are as follows: add ethylene glycol butyl ether to ethanol, mix evenly, then add hydrofluoric acid dropwise to the mixture of ethylene glycol butyl ether and ethanol, after the hydrofluoric acid is completely dissolved and mixed evenly, finally add the organic acid trichloroacetic acid and stir evenly.
[0029] (4) The electropolished sample was immersed in ethanol for ultrasonic cleaning and dried to obtain a nickel-based high-temperature alloy EBSD sample.
[0030] The grain morphology of the nickel-based superalloy EBSD sample prepared by the above method is as follows: Figure 1 As shown, the grain orientation distribution and lattice information inside the sample can be clearly seen, with a resolution of 99%. Example 2
[0031] This embodiment takes the nickel-based high-temperature alloy IN738LC as an example, and provides a method for preparing a sample by EBSD on the nickel-based high-temperature alloy based on electrolytic polishing, comprising the following steps: (1) Pre-grinding: After the nickel-based high-temperature alloy sample with a size of 8 mm × 8 mm × 3 mm was ultrasonically cleaned with ethanol, it was coarsely ground, finely ground and finely ground using 800 mesh, 1500 mesh and 2500 mesh silicon carbide sandpaper on a metallographic pre-grinding machine. At the same time, in order to avoid overheating of the sample surface during the pre-grinding process, water was added to cool it down during the pre-grinding process, and the finely ground sample was cleaned with ethanol.
[0032] (2) Pre-polishing: Pre-polish the sample after fine grinding and cleaning on a polishing machine using diamond paste model W1. Control the speed of the polishing machine to 320 rpm and polish for about 15 minutes until the surface reaches a mirror effect. Use ethanol to clean and remove the diamond paste.
[0033] (3) Electrolytic polishing: The pre-polished sample is placed in an electrolytic cell, with the nickel-based high-temperature alloy sample as the anode and the stainless steel plate as the cathode, and electrolytic polishing is performed in the electrolyte; The parameters of electrolytic polishing were as follows: voltage 25 V, current 0.5 A, electrolysis time 10 s, and electrolysis temperature -10 °C; The electrolyte is composed of the following components in volume percentage: 12% hydrofluoric acid, 24% trifluoroacetic acid, 13% ethylene glycol butyl ether, and 51% ethanol. That is, the volume percentage of the total acid in the electrolyte is 36%, the volume percentage of the organic solvent is 64%, the volume ratio of hydrofluoric acid to trifluoroacetic acid in the total acid is 1:2; the volume ratio of ethylene glycol butyl ether to ethanol in the organic solvent is 1:3.9.
[0034] (4) The electropolished sample was immersed in ethanol for ultrasonic cleaning and dried to obtain a nickel-based high-temperature alloy EBSD sample.
[0035] The grain morphology of the nickel-based superalloy EBSD sample prepared by the above method is as follows: Figure 2 As shown, the crystal structure is clear and the resolution rate is 99%. Example 3
[0036] The total acid volume fraction in the electrolyte of this embodiment is consistent with that in Example 1, which is 25%, and the other components are 20% ethylene glycol butyl ether and 55% ethanol; only the volume ratio of hydrofluoric acid and trichloroacetic acid in the total acid is adjusted as shown in Table 1, and the other parameters are the same as in Example 1. The resolution of EBSD sample preparation of nickel-based high-temperature alloy is analyzed by using hydrofluoric acid and trichloroacetic acid with different volume ratios as the core components in the electrolyte. The results are shown in Table 1, which shows the volume fractions of hydrofluoric acid and trichloroacetic acid in the electrolyte and the volume ratio of the two, as well as the resolution of the sample prepared by the corresponding electrolyte according to the EBSD sample preparation method in Example 1.
[0037] Table 1 Hydrofluoric acid(%) Trichloroacetic acid(%) Hydrofluoric acid:trichloroacetic acid (v:v) Resolution rate(%) 12 13 1:1.08 88 10 15 1:1.5 99 9 16 1:1.78 95 7 18 1:2.57 90 5 20 1:4 75 It can be seen from the results shown in Table 1 that, when the total acid content of hydrofluoric acid and organic acid remains unchanged, reducing or increasing the amount of hydrofluoric acid relative to the organic acid is not conducive to the electrolytic polishing treatment of the nickel-based high-temperature alloy surface.
[0038] Example 4
[0039] The volume ratio of hydrofluoric acid to trichloroacetic acid in the electrolyte of this embodiment is maintained at 1:1.5, which is consistent with that in Example 1. At the same time, the volume ratio of ethylene glycol butyl ether to ethanol in the organic solvent is maintained at about 1:2.75. Only the total acid content in the electrolyte is adjusted as shown in Table 2. The rest of the contents not described are the same as in Example 1. The resolution of EBSD samples prepared by nickel-based high-temperature alloys using electrolytes with different acid contents is analyzed, and the results are shown in Table 2.
[0040] Table 2 Hydrofluoric acid Trichloroacetic acid Total acid content Ethylene glycol butyl ether Ethanol Total amount of organic solvent Resolution 8% 12% 20% 21% 59% 80% 78% 10% 15% 25% 20% 55% 75% 99% 12% 18% 30% 19% 51% 70% 95% 16% 24% 40% 16% 44% 60% 90% 20% 30% 50% 13% 37% 50% 60% It can be seen from the results shown in Table 2 that, when the total acid and the compounding ratio of each component in the organic solvent are kept relatively unchanged, as the total acid content in the electrolyte increases, the resolution rate of the sample prepared by the corresponding electrolyte according to the EBSD sample preparation method described in Example 1 shows a trend of first increasing and then decreasing, especially when the total acid content exceeds 40%, the corrosion to the surface of the nickel-based high-temperature alloy is aggravated, which significantly deteriorates the EBSD sample preparation effect, indicating that the appropriate acid content in the electrolyte is helpful to improve the EBSD sample preparation effect of the nickel-based high-temperature alloy.
[0041] Example 5 The volume fractions of hydrofluoric acid and trichloroacetic acid and the total volume fraction of the organic solvent in the electrolyte of this embodiment are consistent with those in Example 1, that is, the volume fractions of hydrofluoric acid and trichloroacetic acid in the electrolyte are 10% and 15%, respectively, and the volume fraction of the organic solvent is 75%. Relative to Example 1, only the volume ratio of ethylene glycol butyl ether and ethanol in the organic solvent is adjusted as shown in Table 3, and the rest of the unmentioned parts are the same as those in Example 1. The resolution of the EBSD sample of the nickel-based high-temperature alloy was analyzed by the electrolyte described in this embodiment, and the results are shown in Table 3.
[0042] Table 3 Ethylene glycol butyl ether(%) Ethanol(%) Ethylene glycol butyl ether:ethanol (v:v) Resolution rate(%) 30 45 1:1.5 / 25 50 1:2 90 20 55 1:2.75 99 15 60 1:4 95 10 65 1:6.5 85 The “ / ” in Table 3 indicates that the transparency of the electrolyte decreases and the electrolyte is unusable. From the results shown in Table 3, it can be seen that adding an appropriate amount of ethylene glycol butyl ether to the organic solvent helps to improve the EBSD sample preparation effect of the nickel-based high-temperature alloy, but if the amount added is too high, the transparency of the electrolyte will decrease, and some acids will not be dissolved, making the electrolyte unusable.
[0043] Example 6 The difference between this embodiment and embodiment 1 is that the samples of the processed nickel-based high-temperature alloy are different. As shown in Table 4, the different types of nickel-based high-temperature alloys in Table 4 are sampled according to the EBSD sample preparation method described in embodiment 1 and their resolution is analyzed. The results are shown in Table 4.
[0044] Table 4 Nickel-based superalloy Inconel 738 IN738LC INCONEL 625 Hastelloy X GH4169 Inconel 693 Resolution rate(%) 99 99 88 90 85 87 From the results shown in Table 4, it can be seen that the electrolyte of the present invention shows a relatively better electrolytic polishing effect on nickel-based high-temperature alloys whose main components are nickel, chromium, and tungsten, and the electrolytic polishing effect on nickel-based high-temperature alloys whose main components are other main components such as nickel, chromium, and iron is relatively weak, and it may be necessary to adjust the composition or content of the acid in the electrolyte to make it more suitable for the electrolytic polishing of nickel-based high-temperature alloys with other main components.
[0045] Example 7
[0046] The difference between this embodiment and embodiment 1 is that the parameters of electrolytic polishing such as electrolytic voltage and electrolytic temperature are different, and the other parts not described are the same as those in embodiment 1. The influence of different electrolytic voltages and electrolytic temperatures on the resolution of EBSD sample preparation of nickel-based high-temperature alloy is shown in Table 5.
[0047] Table 5 Electrolysis voltage (V) Electrolysis temperature (℃) Resolution rate(%) 5 5 70 10 5 99 25 5 90 30 5 80 10 10 85 10 20 70 From the results shown in Table 5, it can be seen that when the electrolysis voltage is lower than 10 V or higher than 25 V or the electrolysis temperature is higher than 5°C, it is not conducive to the EBSD sample preparation of the nickel-based high-temperature alloy. This shows that in the electrolyte of the present invention, controlling the voltage and current of the electrolytic polishing can realize the electrolytic polishing of the nickel-based high-temperature alloy after the pre-polishing treatment under low temperature conditions, the polishing time is short, and the polishing effect is good.
Claims
1. An electrolyte for EBSD sample preparation of nickel-based high-temperature alloys, characterized in that: The electrolyte is composed of the following components in volume percentage: 5% to 16% hydrofluoric acid, 15% to 25% organic acid, 10% to 30% ethylene glycol butyl ether, and 40% to 60% ethanol.
2. The electrolyte for EBSD sample preparation of nickel-based high-temperature alloy according to claim 1, characterized in that: The volume ratio of the hydrofluoric acid to the organic acid is 1:(1.5-2.5); the sum of the volume percentages of the hydrofluoric acid and the organic acid in the electrolyte is between 25% and 40%.
3. The electrolyte for EBSD sample preparation of nickel-based high-temperature alloy according to claim 1, characterized in that: The organic acid includes at least one of trifluoroacetic acid, trichloroacetic acid, methanesulfonic acid and benzenesulfonic acid.
4. The electrolyte for EBSD sample preparation of nickel-based high-temperature alloy according to claim 1, characterized in that: The volume ratio of ethylene glycol butyl ether to ethanol in the electrolyte is 1:(2-4).
5. The electrolyte for EBSD sample preparation of nickel-based high-temperature alloy according to claim 1, characterized in that: The nickel-based high-temperature alloys include Inconel 738, IN738LC and Hastelloy X.
6. An electrolytic polishing method for EBSD sample preparation of nickel-based high-temperature alloys, characterized in that: The method comprises the following steps: using the pretreated nickel-based high-temperature alloy as an anode and a stainless steel plate as a cathode, and performing electrolytic polishing in the electrolyte described in any one of claims 1 to 4, wherein the parameters of the electrolytic polishing are as follows: a voltage of 10 to 25 V, a current of 0.5 to 0.8 A, an electrolysis time of 10 to 20 s, and an electrolysis temperature of -10°C to 5°C.
7. A method for preparing EBSD samples for nickel-based high-temperature alloys, characterized in that: The steps include: (1) Pre-grinding: Use 800 mesh, 1500 mesh, and 2500 mesh silicon carbide sandpaper to perform coarse grinding, fine grinding, and fine grinding on the nickel-based high-temperature alloy in sequence; (2) Pre-polishing: Pre-polish the finely ground nickel-based high-temperature alloy using diamond paste of model W1 for 5 to 15 minutes; (3) Electrolytic polishing: electrolytic polishing the nickel-based high-temperature alloy sample after pre-grinding and pre-polishing in steps (1) and (2) using the electrolytic polishing method described in claim 5; (4) Cleaning: The electropolished sample is ultrasonically cleaned in ethanol and dried to obtain a nickel-based high-temperature alloy EBSD sample.
Citation Information
Cited By
EBSD electrolytic polishing sample preparation method for medium / high-entropy alloy spherical powder
CN119290935A