Film coating process and preparation process of solar cell and solar cell

Through the auxiliary heating process, the coating temperature uniformity is improved in the solar cell coating process, which solves the problem of silicon wafer surface color difference and dust color difference, and improves the electroluminescence yield and production efficiency.

CN118763142APending Publication Date: 2024-10-11HENGDIAN GRP DMEGC MAGNETICS CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410784487.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing solar cell coating process has shortcomings in rapid response to temperature rise, resulting in color difference and dust color difference between the upper and lower surfaces of the silicon wafer, affecting electroluminescence yield and output.

Method used

The auxiliary heating process is adopted to gradually reduce the power output rate through primary, secondary and tertiary auxiliary heating to improve the uniformity of coating temperature and avoid color difference on the silicon wafer surface. Auxiliary heating equipment is used in the constant temperature step to ensure coating Equipment temperature uniformity and efficiency.

Benefits of technology

It effectively improves film color uniformity and electroluminescence yield, reduces rework rate and production costs, and avoids dust deposition problems caused by excessive coating temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763142A_ABST
    Figure CN118763142A_ABST
Patent Text Reader

Abstract

The invention relates to a solar cell coating process, a solar cell preparation process and a solar cell, the constant temperature step of the coating process adopts auxiliary heating equipment for auxiliary heating, the auxiliary heating comprises first-stage auxiliary heating, second-stage auxiliary heating and third-stage auxiliary heating, and the third-stage auxiliary heating comprises first-stage auxiliary heating, second-stage auxiliary heating and third-stage auxiliary heating. The power output rates of the first-stage auxiliary heating, the second-stage auxiliary heating and the third-stage auxiliary heating are independently selected from 40%-70% of the maximum power of the auxiliary heating equipment, and the power output rates are reduced step by step. An auxiliary heating process is adopted in the constant temperature step of the coating process, color difference between the upper surface and the lower surface of the silicon wafer is avoided through the specific power output rate, meanwhile, dust color difference is avoided, the film color uniformity is effectively improved, and the EL yield of the solar cell is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cell preparation, and in particular to a solar cell coating process, a preparation process and a solar cell. Background Art

[0002] Solar cells are usually passivated by coating aluminum oxide, silicon nitride and other passivation films on the front and back. With the continuous development of solar cell technology, the demand for single-batch production capacity of coating equipment is increasing, and the size of graphite boats and heating furnaces is also increasing. The original single furnace heating method can no longer meet the requirements of rapid response to temperature rise.

[0003] The existing technology effectively shortens the coating process time and improves production efficiency by introducing auxiliary heating equipment into the coating equipment. The operation steps, output power and operation time of the auxiliary heating equipment are of great significance to the uniformity of silicon wafer film color, electroluminescence (EL) yield and output. Therefore, it is necessary to explore the optimal coating process to improve the coating efficiency and the quality of silicon wafers. Summary of the invention

[0004] Based on this, it is necessary to provide a solar cell coating process, a preparation process and a solar cell to address the above problems. The constant temperature step of the coating process adopts an auxiliary heating process to avoid color difference between the upper and lower surfaces of the silicon wafer through a specific power output rate, while avoiding dust color difference, effectively improving the film color uniformity and improving the EL yield of the solar cell.

[0005] A solar cell coating process, wherein the constant temperature step of the coating process adopts auxiliary heating equipment for auxiliary heating, and the auxiliary heating includes primary auxiliary heating, secondary auxiliary heating and tertiary auxiliary heating, wherein the power output rates of the primary auxiliary heating, the secondary auxiliary heating and the tertiary auxiliary heating are each independently selected from 40% to 70% of the maximum power of the auxiliary heating equipment, and the power output rate decreases step by step.

[0006] In one embodiment, the temperature reached when the first-level auxiliary heating ends is 85% to 90% of the target temperature of the constant temperature step; the temperature reached when the second-level auxiliary heating ends is 90% to 95% of the target temperature of the constant temperature step.

[0007] In one of the embodiments, the power output rate difference between the first-stage auxiliary heating and the second-stage auxiliary heating is less than or equal to the power output rate difference between the second-stage auxiliary heating and the third-stage auxiliary heating.

[0008] In one embodiment, the power output rate difference between the primary auxiliary heating and the secondary auxiliary heating is 5% to 10%;

[0009] And / or, the power output rate difference between the second-stage auxiliary heating and the third-stage auxiliary heating is 5% to 15%.

[0010] In one of the embodiments, the power output rate of the primary auxiliary heating is 50% to 70%.

[0011] In one embodiment, the power output rate of the first-level auxiliary heating is greater than or equal to 60% and less than or equal to 70%, the power output rate difference between the first-level auxiliary heating and the second-level auxiliary heating is 5% to 8%, and the power output rate difference between the second-level auxiliary heating and the third-level auxiliary heating is 5% to 12%;

[0012] Alternatively, the power output rate of the first-level auxiliary heating is greater than or equal to 50% and less than 60%, the difference in power output rate between the first-level auxiliary heating and the second-level auxiliary heating is 5% to 7%, and the difference in power output rate between the second-level auxiliary heating and the third-level auxiliary heating is 5% to 10%.

[0013] In one of the embodiments, when the deposition steps of the coating process include more than two deposition steps, a vacuuming step is further included between each deposition step.

[0014] In one embodiment, the coating process includes at least one of a silicon oxide coating process, a silicon nitride coating process, a silicon oxynitride coating process or an aluminum oxide coating process.

[0015] A process for preparing a solar cell includes the above-mentioned film coating process for the solar cell.

[0016] A solar cell manufactured by the above-mentioned solar cell manufacturing process.

[0017] The coating process of the above-mentioned solar cell adopts an auxiliary heating process in the constant temperature step of the coating process. Through a specific power output rate, and the power output rates of the first-level auxiliary heating, the second-level auxiliary heating and the third-level auxiliary heating are gradually reduced, the uniformity of the coating temperature is effectively improved, and the color difference between the upper and lower surfaces of the silicon wafer is avoided, thereby improving the film color uniformity, while improving the electroluminescence (EL) yield of the solar cell, improving the quality of the solar cell, and reducing the rework rate; in addition, it is beneficial to shorten the coating time and improve production efficiency while avoiding the problem of dust deposition in the coating equipment due to excessively high coating temperature, thereby avoiding dust color difference in the silicon wafer. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 This is a flow chart of the coating process of Example 1 of the present invention. DETAILED DESCRIPTION

[0020] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific implementation methods or embodiments, and are not intended to limit the present invention. The optional scope of the term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the combinations include any two related listed items, any more related listed items, or all related listed items.

[0022] The solar cell coating process provided by the present invention has a constant temperature step in which auxiliary heating is performed using an auxiliary heating device, and the auxiliary heating includes primary auxiliary heating, secondary auxiliary heating and tertiary auxiliary heating, wherein the power output rates of the primary auxiliary heating, secondary auxiliary heating and tertiary auxiliary heating are each independently selected from 40% to 70% of the maximum power of the auxiliary heating device, and the power output rate decreases step by step.

[0023] The constant temperature step of the coating process of the above-mentioned solar cell adopts an auxiliary heating process, which is conducive to quickly responding to the heating requirements of the coating equipment to achieve the target temperature; at the same time, the power output rate of the auxiliary heating process is 40% to 70%, which is conducive to ensuring the auxiliary heating effect, and effectively preventing the heating temperature from being too high, thereby avoiding the deposition of yellow dust near the contact end of the graphite boat and the electrode rod in the coating equipment, which is conducive to reducing the dust color difference of the silicon wafer, improving the coating quality of the silicon wafer, and reducing the maintenance frequency of the graphite boat, thereby improving production efficiency and reducing production costs; and the power output rates of the first-level auxiliary heating, the second-level auxiliary heating and the third-level auxiliary heating are gradually reduced, which effectively improves the uniformity of the coating temperature, thereby improving the uniformity of the film color, avoiding color difference between the upper and lower surfaces of the silicon wafer, and at the same time improving the EL yield of the solar cell, improving the quality of the solar cell, and reducing the rework rate.

[0024] It should be noted that the auxiliary heating equipment described in the present invention adopts the commonly used equipment in this field, and the power output rate indicates the percentage of the actual working power to the maximum power of the auxiliary heating equipment. For example, the full power of commonly used auxiliary heating is 6000W, that is, when the power output rate of the present invention is 50%, its actual working power is 3000W; the present invention does not limit the maximum power of the auxiliary heating equipment. When the maximum power is lower than or exceeds 6000W, the effect of the present invention can be achieved by adjusting the time of each level of auxiliary heating; at the same time, the present invention only performs auxiliary heating in the constant temperature step, turns on the auxiliary heating equipment when the temperature starts to rise, and turns off the auxiliary heating equipment after reaching the target temperature.

[0025] Specifically, the solar cell coating process includes the following steps:

[0026] S1. Start the coating equipment and fill the furnace tube with nitrogen to normal pressure;

[0027] S2, open the furnace door, transport the graphite boat loaded with silicon wafers into the furnace tube, and close the furnace door;

[0028] S3, turn on the auxiliary heating, raise the temperature to the target temperature and then keep the temperature constant, the auxiliary heating includes primary auxiliary heating, secondary auxiliary heating and tertiary auxiliary heating, wherein the power output rates of the primary auxiliary heating, the secondary auxiliary heating and the tertiary auxiliary heating are each independently selected from 40% to 70% of the maximum power of the auxiliary heating device, and the power output rate decreases step by step.

[0029] S4, turn off the auxiliary heating, perform slow main pumping, pump the furnace tube to vacuum and check for leaks;

[0030] S5, pre-filling to the target pressure and then maintaining the pressure to deposit the film;

[0031] S6. Fill the furnace tube with nitrogen to normal pressure, open the furnace door, take out the graphite boat loaded with silicon wafers, and close the furnace door.

[0032] It is understandable that the remaining steps of the solar cell coating process all adopt methods commonly used in the art, and the present invention does not limit this.

[0033] In step S2, during the period when the graphite boat enters the furnace tube, it is easy to cause a boat release alarm due to problems such as poor contact between the graphite boat and the electrode rod. The present invention only turns on the auxiliary heating in the constant temperature step, which is beneficial to prevent the temperature difference between the upper and lower surfaces of the silicon wafer from increasing due to the boat release alarm problem, thereby causing color difference between the upper and lower surfaces of the silicon wafer and reducing the quality of the silicon wafer.

[0034] It can be understood that the auxiliary heating device is usually located under the graphite boat. If the auxiliary heating is turned on during the boat placing stage, when the boat placing alarm occurs, the auxiliary heating time is too long due to handling the alarm problem, resulting in the bottom of the graphite boat being heated significantly higher than the top of the graphite boat. Accordingly, the temperature of the lower surface of the silicon wafer in the graphite boat is significantly higher than the upper surface of the silicon wafer, making the coating rate on the lower surface of the silicon wafer higher than that on the upper surface, color stratification occurs on the upper and lower surfaces of the silicon wafer, and the lower surface of the silicon wafer is darker after EL testing, thereby improving the quality of the silicon wafer.

[0035] Specifically, the temperature reached when the first-stage auxiliary heating ends is 85% to 90% of the target temperature of the constant temperature step; the temperature reached when the second-stage auxiliary heating ends is 90% to 95% of the target temperature of the constant temperature step.

[0036] It can be understood that the temperature reached when the secondary auxiliary heating ends is the target temperature of the constant temperature step.

[0037] In one embodiment, the power output rate difference between the first-stage auxiliary heating and the second-stage auxiliary heating is less than or equal to the power output rate difference between the second-stage auxiliary heating and the third-stage auxiliary heating.

[0038] In order to further improve the uniformity of the coating temperature and thus enhance the uniformity of the film color, and at the same time further reduce the temperature difference between the upper and lower surfaces of the silicon wafer to reduce the color difference between the upper and lower surfaces of the silicon wafer and improve the EL yield of the solar cell, the power output rate difference between the first-level auxiliary heating and the second-level auxiliary heating is preferably 5% to 10%.

[0039] In one embodiment, the power output rate difference between the second-stage auxiliary heating and the third-stage auxiliary heating is preferably 5% to 15%.

[0040] Preferably, the power output rate of the first-level auxiliary heating is 50% to 70%, which is conducive to ensuring the auxiliary heating effect and effectively preventing the heating temperature from being too high, thereby ensuring the uniformity of the silicon wafer film color.

[0041] In one embodiment, the power output rate of the first-level auxiliary heating is greater than or equal to 60% and less than or equal to 70%, the difference in power output rate between the first-level auxiliary heating and the second-level auxiliary heating is 5% to 8%, and the difference in power output rate between the second-level auxiliary heating and the third-level auxiliary heating is 5% to 12%.

[0042] In one embodiment, the power output rate of the first-level auxiliary heating is greater than or equal to 50% and less than 60%, the difference in power output rate between the first-level auxiliary heating and the second-level auxiliary heating is 5% to 7%, and the difference in power output rate between the second-level auxiliary heating and the third-level auxiliary heating is 5% to 10%.

[0043] It should be noted that the present invention has no special restrictions on the time of the first-stage auxiliary heating, the second-stage auxiliary heating and the third-stage auxiliary heating.

[0044] In one embodiment, before step S5, the process also includes: purging the surface of the silicon wafer with nitrogen at a constant temperature, and then evacuating the furnace tube to a vacuum, which is beneficial to removing dirt adhered to the surface of the silicon wafer and effectively improving the coating quality of the silicon wafer.

[0045] Specifically, when the deposition steps of the coating process include more than two deposition steps, a vacuuming step is further included between each deposition step, which is beneficial to improving the coating quality and coating efficiency.

[0046] It should be noted that step S5 can be prepared according to the existing method, and the target temperature and target pressure are set according to the film obtained in the deposition coating step, which is not elaborated in the present invention; the gas pre-filled in the pre-filling step can be special gases such as silane, nitrous oxide, and ammonia, which is beneficial to improve the gas uniformity during deposition coating, thereby improving the coating quality.

[0047] In one embodiment, the coating process includes at least one of a silicon oxide coating process, a silicon nitride coating process, a silicon oxynitride coating process, or an aluminum oxide coating process.

[0048] In one embodiment, the coating equipment is selected from PECVD equipment.

[0049] In one embodiment, before step S5, the process further includes: extracting excess gas in the furnace tube and purging with nitrogen to ensure that no reaction gas remains in the furnace tube.

[0050] It can be understood that the coating process of the solar cell of the present invention can be performed on the front side of the solar cell or on the back side of the solar cell; the solar cell includes but is not limited to PERC, TOPCon and other crystalline silicon solar cells.

[0051] The present invention also provides a process for preparing a solar cell, including the film coating process for the solar cell as described above.

[0052] It can be understood that the processes of texturing, diffusion, screen printing, etc. in the preparation process of the solar cell all adopt the commonly used methods in the art, and the present invention will not elaborate on them.

[0053] The present invention also provides a solar cell manufactured by the above-mentioned manufacturing method.

[0054] Hereinafter, the coating process, preparation process and solar cell of the solar cell will be further described through the following specific embodiments.

[0055] Example 1

[0056] (1) Start-up: Turn on the PECVD equipment for preheating, and do not turn on the auxiliary heating;

[0057] (2) Nitrogen filling: Nitrogen is filled into the furnace tube to keep the tube at normal pressure, and the auxiliary heating is not turned on;

[0058] (3) Boat entry: After the furnace door is opened, the graphite boat loaded with silicon wafers is transported into the furnace tube, the paddle is withdrawn to the starting point, the furnace door is closed, and the auxiliary heating is not turned on. Among them, the silicon wafer has completed the texturing, diffusion, tunneling layer and polysilicon thin film production and N + Layer production;

[0059] (4) Constant temperature: Turn on auxiliary heating, wherein the power output rate parameter of the first-level auxiliary heating is set to 65%. When the temperature reaches 494°C, it is adjusted to the second-level auxiliary heating. The power output rate parameter of the second-level auxiliary heating is set to 60%. When the temperature reaches 520°C, it is adjusted to the third-level auxiliary heating. The power output rate parameter of the third-level auxiliary heating is set to 55%. When the temperature reaches 550°C, the auxiliary heating is turned off and the temperature is kept constant, and the auxiliary heating is not turned on in the subsequent steps;

[0060] (5) Slow extraction: extract the air in the furnace tube to make the furnace tube into a vacuum state;

[0061] (6) Leak detection: Check the tightness of the furnace tube;

[0062] (7) Nitrogen purge: Use nitrogen to purge the surface of the silicon wafer to remove dirt adhering to the surface of the silicon wafer;

[0063] (8) Vacuuming: extract the air from the furnace tube to make the furnace tube into a vacuum state;

[0064] (9) Constant pressure: SiH4 and N2O are introduced for pre-gassing to ensure uniform gas during coating;

[0065] (10) First deposition coating: SiH4 and N2O are introduced to coat a silicon oxide film on the surface of the silicon wafer, wherein the SiH4 flow rate is 900 sccm, the time is 50 s, the N2O flow rate is 4500 sccm, the time is 50 s, and the pressure is 200 Pa;

[0066] (11) Vacuuming: extract the excess special gas in the furnace tube so that there is no special gas left in the furnace tube;

[0067] (12) Second deposition coating: using SiH4 and NH3 to coat a silicon nitride film on the surface of the silicon wafer, wherein the flow rate of SiH4 is 1200 sccm, the time is 200 s, the flow rate of NH3 is 4800 sccm, the time is 200 s, and the pressure is 220 Pa;

[0068] (13) Vacuuming: extract the excess special gas in the furnace tube so that no special gas remains in the furnace tube;

[0069] (14) Third deposition coating: using SiH4 and NH3 to coat a low-refractive silicon nitride film on the surface of the silicon wafer, wherein the flow rate of SiH4 is 900 sccm, the time is 450 s, the flow rate of NH3 is 10800 sccm, the time is 450 s, and the pressure is 220 Pa;

[0070] (15) Vacuuming and nitrogen purging: remove excess special gas in the furnace tube and purge with nitrogen to ensure that there is no special gas remaining in the furnace tube;

[0071] (16) Nitrogen filling: Close the main pumping valve, fill with nitrogen, and restore the furnace tube from a vacuum state to a normal pressure state;

[0072] (17) Taking out the boat and ending: Take out the graphite boat in the furnace tube and place it on a shelf to cool.

[0073] Example 2

[0074] (1) Start-up: Turn on the PECVD equipment for preheating, and do not turn on the auxiliary heating;

[0075] (2) Nitrogen filling: Nitrogen is filled into the furnace tube to keep the tube at normal pressure, and the auxiliary heating is not turned on;

[0076] (3) Boat entry: After the furnace door is opened, the graphite boat loaded with silicon wafers is transported into the furnace tube, the paddle is withdrawn to the starting point, the furnace door is closed, and the auxiliary heating is not turned on. Among them, the silicon wafer has completed the texturing, diffusion, tunneling layer and polysilicon thin film production and N + Layer production;

[0077] (4) Constant temperature: Turn on auxiliary heating, wherein the power output rate parameter of the first-level auxiliary heating is set to 59%. When the temperature reaches 493°C, it is adjusted to the second-level auxiliary heating. The power output rate parameter of the second-level auxiliary heating is set to 52%. When the temperature reaches 517°C, it is adjusted to the third-level auxiliary heating. The power output rate parameter of the third-level auxiliary heating is set to 44%. When the temperature reaches 548°C, the auxiliary heating is turned off and the temperature is kept constant, and the auxiliary heating is not turned on in the subsequent steps;

[0078] (5) Slow extraction: extract the air in the furnace tube to make the furnace tube into a vacuum state;

[0079] (6) Leak detection: Check the tightness of the furnace tube;

[0080] (7) Nitrogen purge: Use nitrogen to purge the surface of the silicon wafer to remove dirt adhering to the surface of the silicon wafer;

[0081] (8) Vacuuming: extract the air from the furnace tube to make the furnace tube into a vacuum state;

[0082] (9) Constant pressure: SiH4 and N2O are introduced for pre-gassing to ensure uniform gas during coating;

[0083] (10) First deposition coating: SiH4 and N2O are introduced to coat a silicon oxide film on the surface of the silicon wafer, wherein the SiH4 flow rate is 900 sccm, the time is 50 s, the N2O flow rate is 4500 sccm, the time is 50 s, and the pressure is 200 Pa;

[0084] (11) Vacuuming: extract the excess special gas in the furnace tube so that there is no special gas left in the furnace tube;

[0085] (12) Second deposition coating: using SiH4 and NH3 to coat a silicon nitride film on the surface of the silicon wafer, wherein the flow rate of SiH4 is 1200 sccm, the time is 200 s, the flow rate of NH3 is 4800 sccm, the time is 200 s, and the pressure is 220 Pa;

[0086] (13) Vacuuming: extract the excess special gas in the furnace tube so that no special gas remains in the furnace tube;

[0087] (14) Third deposition coating: using SiH4 and NH3 to coat a low-refractive silicon nitride film on the surface of the silicon wafer, wherein the flow rate of SiH4 is 900 sccm, the time is 450 s, the flow rate of NH3 is 10800 sccm, the time is 450 s, and the pressure is 220 Pa;

[0088] (15) Vacuuming and nitrogen purging: remove excess special gas in the furnace tube and purge with nitrogen to ensure that there is no special gas remaining in the furnace tube;

[0089] (16) Nitrogen filling: Close the main pumping valve, fill with nitrogen, and restore the furnace tube from a vacuum state to a normal pressure state;

[0090] (17) Taking out the boat and ending: Take out the graphite boat in the furnace tube and place it on a shelf to cool.

[0091] Comparative Example 1

[0092] (1) Start-up: Preheat the PECVD equipment, turn on the auxiliary heating, and set the auxiliary heating power output rate parameter to 10%;

[0093] (2) Nitrogen filling: Nitrogen is filled into the furnace tube to keep the tube at normal pressure, the auxiliary heating is turned on, and the auxiliary heating power output rate parameter is set to 30%;

[0094] (3) Boat entry: After the furnace door is opened, the graphite boat loaded with silicon wafers is transported into the furnace tube, the paddle is withdrawn to the starting point, the furnace door is closed, and the auxiliary heating is turned on. The auxiliary heating power output rate parameter is set to 60%. Among them, the silicon wafer has completed the texturing, diffusion, tunneling layer and polysilicon film production and N + Layer production;

[0095] (4) Constant temperature: Auxiliary heating is turned on, and the auxiliary heating power output rate parameter is set to 60%. The temperature is raised to 550°C and then kept constant;

[0096] (5) Slow extraction: The air in the furnace tube is extracted to make the furnace tube into a vacuum state, the auxiliary heating is turned on, and the auxiliary heating power output rate parameter is set to 60%. After the vacuum is evacuated, the auxiliary heating is turned off, and the auxiliary heating is not turned on in the subsequent steps;

[0097] (6) Leak detection: Check the tightness of the furnace tube;

[0098] (7) Nitrogen purge: Use nitrogen to purge the surface of the silicon wafer to remove dirt adhering to the surface of the silicon wafer;

[0099] (8) Vacuuming: empty the gas in the tube to make the furnace tube in a vacuum state;

[0100] (9) Constant pressure: SiH4 and N2O are introduced for pre-gassing to ensure uniform gas during coating;

[0101] (10) First deposition coating: SiH4 and N2O are introduced to coat a silicon oxide film on the surface of the silicon wafer, wherein the SiH4 flow rate is 900 sccm, the time is 50 s, the N2O flow rate is 4500 sccm, the time is 50 s, and the pressure is 200 Pa;

[0102] (11) Vacuuming: extract the excess special gas in the furnace tube so that there is no special gas left in the furnace tube;

[0103] (12) Second deposition coating: using SiH4 and NH3 to coat a silicon nitride film on the surface of the silicon wafer, wherein the flow rate of SiH4 is 1200 sccm, the time is 200 s, the flow rate of NH3 is 4800 sccm, the time is 200 s, and the pressure is 220 Pa;

[0104] (13) Vacuuming: extract the excess special gas in the furnace tube so that no special gas remains in the furnace tube;

[0105] (14) Third deposition coating: using SiH4 and NH3 to coat a low-refractive silicon nitride film on the surface of the silicon wafer, wherein the flow rate of SiH4 is 900 sccm, the time is 450 s, the flow rate of NH3 is 10800 sccm, the time is 450 s, and the pressure is 220 Pa;

[0106] (15) Vacuuming and nitrogen purging: remove excess special gas in the furnace tube and purge with nitrogen to ensure that there is no special gas remaining in the furnace tube;

[0107] (16) Nitrogen filling: Close the main pumping valve, fill with nitrogen, and restore the furnace tube from a vacuum state to a normal pressure state;

[0108] (17) Taking out the boat and ending: Take out the graphite boat in the furnace tube and place it on a shelf to cool.

[0109] Comparative Example 2

[0110] (1) Start-up: Preheat the PECVD equipment, turn on the auxiliary heating, and set the auxiliary heating power output rate parameter to 10%;

[0111] (2) Nitrogen filling: Nitrogen is filled into the furnace tube to keep the tube at normal pressure, the auxiliary heating is turned on, and the auxiliary heating power output rate parameter is set to 30%;

[0112] (3) Boat entry: After the furnace door is opened, the graphite boat loaded with silicon wafers is transported into the furnace tube, the paddle is withdrawn to the starting point, the furnace door is closed, and the auxiliary heating is turned on. The auxiliary heating power output rate parameter is set to 60%. Among them, the silicon wafer has completed the texturing, diffusion, tunneling layer and polysilicon film production and N + Layer production;

[0113] (4) Constant temperature: Turn on auxiliary heating, wherein the power output rate parameter of the first-level auxiliary heating is set to 65%. When the temperature reaches 492°C, it is adjusted to the second-level auxiliary heating. The power output rate parameter of the second-level auxiliary heating is set to 60%. When the temperature reaches 518°C, it is adjusted to the third-level auxiliary heating. The power output rate parameter of the third-level auxiliary heating is set to 55%. When the temperature reaches 547°C, the auxiliary heating is turned off and the temperature is kept constant, and the auxiliary heating is not turned on in the subsequent steps;

[0114] (5) Slow extraction: extract the air in the furnace tube to make the furnace tube into a vacuum state;

[0115] (6) Leak detection: Check the tightness of the furnace tube;

[0116] (7) Nitrogen purge: Use nitrogen to purge the surface of the silicon wafer to remove dirt adhering to the surface of the silicon wafer;

[0117] (8) Vacuuming: extract the air from the furnace tube to make the furnace tube into a vacuum state;

[0118] (9) Constant pressure: SiH4 and N2O are introduced for pre-gassing to ensure uniform gas during coating;

[0119] (10) First deposition coating: SiH4 and N2O are introduced to coat silicon oxide or high-refractive silicon nitride film on the surface of the silicon wafer, wherein the SiH4 flow rate is 900 sccm, the time is 50 s, the N2O flow rate is 4500 sccm, the time is 50 s, and the pressure is 200 Pa;

[0120] (11) Vacuuming: extract the excess special gas in the furnace tube so that there is no special gas left in the furnace tube;

[0121] (12) Second deposition coating: using SiH4 and NH3 to coat a silicon nitride film on the surface of the silicon wafer, wherein the flow rate of SiH4 is 1200 sccm, the time is 200 s, the flow rate of NH3 is 4800 sccm, the time is 200 s, and the pressure is 220 Pa;

[0122] (13) Vacuuming: extract the excess special gas in the furnace tube so that no special gas remains in the furnace tube;

[0123] (14) Third deposition coating: using SiH4 and NH3 to coat a low-refractive silicon nitride film on the surface of the silicon wafer, wherein the flow rate of SiH4 is 900 sccm, the time is 450 s, the flow rate of NH3 is 10800 sccm, the time is 450 s, and the pressure is 220 Pa;

[0124] (15) Vacuuming and nitrogen purging: remove excess special gas in the furnace tube and purge with nitrogen to ensure that there is no special gas remaining in the furnace tube;

[0125] (16) Nitrogen filling: Close the main pumping valve, fill with nitrogen, and restore the furnace tube from a vacuum state to a normal pressure state;

[0126] (17) Taking out the boat and ending: Take out the graphite boat in the furnace tube and place it on a shelf to cool.

[0127] Comparative Example 3

[0128] The difference between Comparative Example 3 and Example 1 is that during the constant temperature step, auxiliary heating is turned on, wherein the first-level auxiliary heating power output rate parameter is set to 80%, and when the temperature reaches 492°C, it is adjusted to the second-level auxiliary heating, and the second-level auxiliary heating power output rate parameter is set to 40%, and when the temperature reaches 517°C, it is adjusted to the third-level auxiliary heating, and the third-level auxiliary heating power output rate parameter is set to 30%, and when the temperature reaches 548°C, the auxiliary heating is turned off and the temperature is kept constant, and auxiliary heating is not turned on in any subsequent steps.

[0129] Comparative Example 4

[0130] The difference between Comparative Example 4 and Example 1 is that during the constant temperature step, auxiliary heating is turned on, wherein the power output rate parameter of the first-level auxiliary heating is set to 60%, and when the temperature reaches 493°C, it is adjusted to the second-level auxiliary heating, and the power output rate parameter of the second-level auxiliary heating is set to 65%, and when the temperature reaches 519°C, it is adjusted to the third-level auxiliary heating, and the power output rate parameter of the third-level auxiliary heating is set to 70%, and when the temperature reaches 548°C, the auxiliary heating is turned off and the temperature is kept constant, and the auxiliary heating is not turned on in the subsequent steps;

[0131] The silicon wafers after coating in all the embodiments and comparative examples were tested, and 20,000 wafers were produced respectively. The ratio of the number of unqualified silicon wafers to the total number of silicon wafers after coating was the silicon wafer rework rate, and the ratio of the number of silicon wafers with dust color difference to the total number of silicon wafers was the silicon wafer dust color difference ratio. The coated silicon wafers were screen-printed and then subjected to EL testing, and the EL yield of the silicon wafers was calculated. All test results are shown in Table 1.

[0132] Table 1

[0133] Rework rate (%) Dust color difference ratio (%) EL yield (%) Example 1 0.42 0 98.66 Example 2 0.41 0 98.62 Comparative Example 1 0.92 0.7 97.75 Comparative Example 2 0.75 0.3 98.10 Comparative Example 3 0.79 0.5 97.81 Comparative Example 4 0.85 0.6 97.73

[0134] It can be seen from Table 1 that under the same test conditions, the silicon wafer rework rate of the embodiment is low, there is no dust color difference, and the EL yield is high, while the rework rate, dust color difference ratio and EL yield of the comparative example are all lower than those of the embodiment. Therefore, the coating process of the solar cell provided by the present invention is conducive to avoiding color difference between the upper and lower surfaces of the silicon wafer, while avoiding dust color difference, effectively improving the uniformity of the film color, and improving the EL yield of the solar cell.

[0135] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0136] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A solar cell coating process, characterized in that: The constant temperature step of the coating process adopts auxiliary heating equipment for auxiliary heating, and the auxiliary heating includes primary auxiliary heating, secondary auxiliary heating and tertiary auxiliary heating, wherein the power output rates of the primary auxiliary heating, the secondary auxiliary heating and the tertiary auxiliary heating are each independently selected from 40% to 70% of the maximum power of the auxiliary heating equipment, and the power output rate decreases step by step.

2. The solar cell coating process according to claim 1, characterized in that: The temperature reached when the first-stage auxiliary heating is finished is 85% to 90% of the target temperature of the constant temperature step; the temperature reached when the second-stage auxiliary heating is finished is 90% to 95% of the target temperature of the constant temperature step.

3. The solar cell coating process according to claim 1, characterized in that: The power output rate difference between the first-level auxiliary heating and the second-level auxiliary heating is less than or equal to the power output rate difference between the second-level auxiliary heating and the third-level auxiliary heating.

4. The solar cell coating process according to claim 3, characterized in that: The power output rate difference between the first-stage auxiliary heating and the second-stage auxiliary heating is 5% to 10%; And / or, the power output rate difference between the second-stage auxiliary heating and the third-stage auxiliary heating is 5% to 15%.

5. The solar cell coating process according to any one of claims 1 to 4, characterized in that: The power output rate of the first-stage auxiliary heating is 50% to 70%.

6. The solar cell coating process according to claim 5, characterized in that: The power output rate of the first-level auxiliary heating is greater than or equal to 60% and less than or equal to 70%, the difference in power output rate between the first-level auxiliary heating and the second-level auxiliary heating is 5% to 8%, and the difference in power output rate between the second-level auxiliary heating and the third-level auxiliary heating is 5% to 12%; Alternatively, the power output rate of the first-level auxiliary heating is greater than or equal to 50% and less than 60%, the difference in power output rate between the first-level auxiliary heating and the second-level auxiliary heating is 5% to 7%, and the difference in power output rate between the second-level auxiliary heating and the third-level auxiliary heating is 5% to 10%.

7. The solar cell coating process according to claim 1, characterized in that: In the deposition steps of the coating process, when more than two deposition steps are included, a vacuuming step is further included between each deposition step.

8. The solar cell coating process according to claim 1, characterized in that: The coating process includes at least one of a silicon oxide coating process, a silicon nitride coating process, a silicon oxynitride coating process or an aluminum oxide coating process.

9. A process for preparing a solar cell, characterized in that: The preparation process includes the solar cell coating process as claimed in any one of claims 1 to 8.

10. A solar cell manufactured by the process for manufacturing a solar cell according to claim 9.

Citation Information

Cited By

  • PECVD process for improving membrane explosion of TOPCON battery

    CN119506848A

  • A PECVD process to improve TOPCON battery film explosion

    CN119506848B