Lithium manganese iron phosphate positive electrode material as well as preparation method and application thereof

By introducing a lithium phosphate coating layer and an amorphous carbon coating layer into the lithium iron manganese phosphate cathode material and forming a conductive carbon network, the problem of insufficient cycle stability and voltage stability of the lithium manganese iron phosphate cathode material at high temperatures is solved. , achieving high energy density material properties.

CN118763201AInactive Publication Date: 2024-10-11TIANJIN RONBAY SKYLAND TECHNOLOGY CO LTD

Patent Information

Application Number
CN202410966769.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The current lithium iron manganese phosphate cathode materials have poor cycle stability and voltage stability in high temperature environments and cannot meet the demand for high energy density cathode materials in the new energy field.

Method used

A lithium iron manganese phosphate cathode material is used, which includes a lithium iron manganese phosphate core and a lithium phosphate coating layer and an amorphous carbon coating layer covering part of the surface. It is prepared through ball milling and high-temperature calcination to form a conductive carbon network. to improve electronic conductivity and structural stability.

Benefits of technology

The capacity retention rate after 200 cycles at 1C/2-4.3V at 45°C is no less than 92%, and the voltage retention rate is no less than 90%, which significantly improves the cycle stability and voltage stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763201A_ABST
    Figure CN118763201A_ABST
Patent Text Reader

Abstract

The invention provides a lithium manganese iron phosphate positive electrode material as well as a preparation method and application thereof. The lithium manganese iron phosphate positive electrode material comprises secondary particles connected by a conductive network, wherein the secondary particle comprises a lithium manganese iron phosphate inner core and a coating layer coating at least part of the surface of the lithium manganese iron phosphate inner core; the coating layer comprises a lithium phosphate coating layer and an amorphous carbon coating layer covering at least part of the surface of the lithium phosphate coating layer; the lithium manganese iron phosphate positive electrode material has a capacity retention rate of not less than 92% and a voltage retention rate of not less than 90% after 200 cycles at 45 DEG C under 1C / 2-4.3 V. The lithium manganese iron phosphate positive electrode material prepared by the invention shows excellent capacity retention rate and voltage retention rate, can give full play to high energy density brought by Mn on a high-voltage platform, and greatly meets the use requirements of the current market on high-energy-density batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a lithium manganese iron phosphate positive electrode material and a preparation method and application thereof, belonging to the field of lithium ion batteries. Background Art

[0002] With the continuous development of the new energy industry, LiFePO4 batteries can no longer meet people's growing demand for high energy density batteries. LiFePO4 batteries with the same structure as LiFePO4 have Mn 2+ / Mn 3+ The reaction potential of up to 4.1V can increase the overall energy density by 21%, making it the next generation new lithium-ion battery positive electrode material.

[0003] While the introduction of Mn into lithium manganese iron phosphate improves its energy density, it also brings a series of problems. 2+ Mn obtained by oxidation during charging 3+ There will be Jahn-Teller effect, which will damage its structure; Mn generated during the charge and discharge process 3+ A disproportionation reaction will occur to generate Mn 2+ and Mn 4+ , Mn 2+ It is easy to precipitate. On the one hand, it will migrate to the negative electrode of the whole battery for deposition, thus causing a series of problems such as SEI film thickening, lithium consumption, and dendrites. On the other hand, Mn 2+ Precipitation can cause the collapse of the material structure, thus deteriorating its structural stability; in high-temperature application scenarios, trace amounts of H2O in the electrolyte can cause PF6 - Decomposition produces HF, F - Combined with Mn, it increases 2+ Dissolution in electrolyte. In addition, Yamada et al. calculated the electron transition energy gap by first principles, and the results showed that the electron transition energy gap of LiFePO4 is 0.3 eV, which is a semiconductor, while the electron transition energy gap of LiMnPO4 is 2 eV, which is almost an insulator. Therefore, LiMnPO4 has extremely poor electronic conductivity and ionic conductivity. During the charge and discharge process, obvious polarization will occur, resulting in the inability to exert capacity; and because Li + When the LiMnPO4 part diffuses, its kinetics are poor, which will cause Mn 3+ Cannot be fully reduced to Mn in the high voltage range 2+ , part of Mn 3+ Reduction at lower voltages prevents the energy density advantage of Mn at the high voltage platform of 4.1V from being fully utilized.

[0004] The above situation is particularly serious in high temperature environments. Therefore, the poor cycle stability of lithium manganese iron phosphate and the gradually decreasing platform voltage during charging and discharging cannot meet the demand for high energy density positive electrode materials in various new energy fields. How to improve the cycle stability and voltage stability of lithium manganese iron phosphate positive electrode materials in high temperature environments has become a technical problem that needs to be solved urgently in this field. Summary of the invention

[0005] The invention provides a lithium iron manganese phosphate positive electrode material, which has excellent cycle stability and voltage stability at high temperature.

[0006] The present invention also provides a method for preparing a lithium iron manganese phosphate positive electrode material. The preparation method can be used to prepare the above-mentioned lithium iron manganese phosphate positive electrode material. The preparation method is simple to operate and can prepare a lithium iron manganese phosphate positive electrode material with excellent cycle stability and voltage stability.

[0007] The present invention also provides a positive electrode sheet, which has excellent cycle stability and voltage stability.

[0008] The present invention also provides a battery having excellent cycle stability and voltage stability.

[0009] In one aspect, the present invention provides a lithium iron manganese phosphate positive electrode material, comprising a lithium iron manganese phosphate core and a coating layer coated on at least a portion of the surface of the lithium iron manganese phosphate core; The coating layer includes a lithium phosphate coating layer and an amorphous carbon coating layer covering at least a portion of the surface of the lithium phosphate coating layer; The capacity retention rate of the lithium manganese iron phosphate positive electrode material after 200 cycles at 45° C. and 1C / 2-4.3V conditions is not less than 92%, and the voltage retention rate is not less than 90%.

[0010] The lithium iron manganese phosphate positive electrode material as described above has a capacity retention rate of not less than 94% after 200 cycles under 1C / 2-4.3V conditions at 45°C.

[0011] In the lithium manganese iron phosphate positive electrode material as described above, at least a portion of the surface of the amorphous carbon coating layer is covered with a conductive carbon network.

[0012] In the lithium manganese iron phosphate positive electrode material as described above, the median particle size D50 of the lithium manganese iron phosphate core is 0.4-0.5 μm.

[0013] In the lithium iron manganese phosphate positive electrode material as described above, the mass ratio of the lithium iron manganese phosphate core, the lithium phosphate coating layer, the amorphous carbon coating layer and the conductive carbon mesh is 100:1:5:0.5.

[0014] The present invention also provides a method for preparing the lithium manganese iron phosphate positive electrode material as described above, comprising the following steps: 1) ball milling a mixture including a lithium iron manganese phosphate precursor, Li3PO4, and an amorphous carbon source at 200-2000 r / min for 2-13 hours, and then drying at 80-120° C. for 6-24 hours to obtain a precursor powder; 2) The precursor powder is heated to 600-900° C. at a heating rate of 3-5° C. / min and calcined for 5-15 hours to obtain the lithium manganese iron phosphate positive electrode material.

[0015] In the preparation method as described above, in step 1), the mixture further includes a conductive carbon source.

[0016] The preparation method as described above, between step 1) and step 2), further comprises subjecting the powder to a thermal shock treatment, wherein the thermal shock treatment comprises the following steps: The powder was mixed according to 10 3 -10 5 The temperature was raised to 300-500℃ at a heating rate of 10℃ / s and maintained for 1-60s. 3 -10 5 The temperature was cooled to room temperature at a cooling rate of ℃ / s.

[0017] The present invention also provides a positive electrode sheet, comprising the lithium iron manganese phosphate positive electrode material as described above or the lithium iron manganese phosphate positive electrode material prepared by the preparation method as described above.

[0018] The present invention also provides a battery, comprising the lithium manganese iron phosphate positive electrode material or the positive electrode sheet as described above.

[0019] The lithium iron manganese phosphate positive electrode material provided by the present invention is composed of a special coating structure. The lithium iron manganese phosphate positive electrode material still has a high capacity retention rate and voltage retention rate at 45° C. and has excellent cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a voltage decay diagram of the lithium manganese iron phosphate positive electrode material prepared in Example 1 of the present invention after 200 cycles at a high temperature of 45°C and 1C; Figure 2 This is a graph showing the capacity retention rate of the lithium manganese iron phosphate positive electrode material prepared in Example 1 of the present invention after 200 cycles at a high temperature of 45° C. and 1C; Figure 3 The voltage decay diagram of the lithium manganese iron phosphate positive electrode material prepared in Example 2 of the present invention after 200 cycles at a high temperature of 45°C and 1C; Figure 4This is a graph showing the capacity retention rate of the lithium manganese iron phosphate positive electrode material prepared in Example 2 of the present invention after 200 cycles at a high temperature of 45° C. and 1C; Figure 5 The voltage decay diagram of the lithium manganese iron phosphate positive electrode material provided in Comparative Example 1 of the present invention after 200 cycles at a high temperature of 45°C and 1C; Figure 6 The capacity retention rate diagram of the lithium manganese iron phosphate positive electrode material provided in Comparative Example 1 of the present invention after 200 cycles at a high temperature of 45°C and 1C; Figure 7 The voltage decay diagram of the lithium manganese iron phosphate positive electrode material prepared in Example 3 of the present invention after 200 cycles at a high temperature of 45°C and 1C; Figure 8 This is a graph showing the capacity retention rate of the lithium manganese iron phosphate positive electrode material prepared in Example 3 of the present invention after 200 cycles at a high temperature of 45° C. and 1C; Fig. 9 The voltage decay diagram of the lithium manganese iron phosphate positive electrode material prepared in Example 4 of the present invention after 200 cycles at a high temperature of 45°C and 1C; Fig.10 This is a graph showing the capacity retention rate of the lithium manganese iron phosphate positive electrode material prepared in Example 4 of the present invention after 200 cycles at a high temperature of 45° C. and 1C; Fig.11 This is a voltage decay diagram of the lithium manganese iron phosphate positive electrode material prepared in Example 5 of the present invention after 200 cycles at a high temperature of 45°C and 1C; Fig.12 This is a graph showing the capacity retention rate of the lithium manganese iron phosphate positive electrode material prepared in Example 5 of the present invention after 200 cycles at a high temperature of 45° C. and 1C; Fig.13 The voltage decay diagram of the lithium manganese iron phosphate positive electrode material prepared in Comparative Example 2 of the present invention after 200 cycles at a high temperature of 45°C and 1C; Fig.14 This is a graph showing the capacity retention rate of the lithium manganese iron phosphate positive electrode material prepared in Comparative Example 2 of the present invention after 200 cycles at a high temperature of 45°C and 1C; Fig.15 It is a CITT comparison diagram of the lithium iron manganese phosphate positive electrode material prepared in Example 3 of the present invention and the lithium iron manganese phosphate positive electrode material prepared in Comparative Example 1; Fig.16 Transmission electron microscope (TEM) images of the lithium manganese iron phosphate positive electrode material prepared in Example 3 of the present invention at different magnifications; Fig.17 The XRD diagram of the lithium manganese iron phosphate positive electrode material prepared in Comparative Example 1 of the present invention before and after 200 cycles at 45°C; Fig.18The XRD diagram of the lithium manganese iron phosphate positive electrode material prepared in Example 3 of the present invention before and after 200 cycles at 45°C; Fig.19 This is a transmission electron microscope (TEM) image of the lithium manganese iron phosphate positive electrode material prepared in Example 3 of the present invention; Fig. 20 The transmission electron microscope (TEM) spectrum of the high-performance lithium manganese iron phosphate positive electrode material prepared in Example 3 of the present invention after cycling 200 times at a high temperature of 45° C. and 1C; Fig.21 This is a transmission electron microscope (TEM) spectrum of the lithium manganese iron phosphate positive electrode material prepared in Comparative Example 1 of the present invention after cycling 200 times at a high temperature of 45°C and 1C. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] In one aspect, the present invention provides a lithium iron manganese phosphate positive electrode material, comprising a lithium iron manganese phosphate core and a coating layer coated on at least a portion of the surface of the lithium iron manganese phosphate core; The coating layer includes a lithium phosphate coating layer and an amorphous carbon coating layer covering at least a portion of the surface of the lithium phosphate coating layer; The capacity retention rate of the lithium manganese iron phosphate positive electrode material after 200 cycles at 45° C. and 1C / 2-4.3V conditions is not less than 92%, and the voltage retention rate is not less than 90%.

[0023] The lithium iron manganese phosphate positive electrode material provided by the present invention is a material with a core-shell structure, wherein the core is a lithium iron manganese phosphate core, and the shell is a lithium phosphate coating layer and an amorphous carbon coating layer.

[0024] The specific structure and composition characteristics of the lithium manganese iron phosphate positive electrode material provided by the present invention can be characterized by transmission electron microscopy.

[0025] The electrochemical parameters of the present invention are obtained based on the button battery under the conditions of a test voltage of 2-4.3V, a test temperature of 45°C, and a test rate of 1C. The preparation method of the button battery is to prepare a slurry of the lithium manganese iron phosphate positive electrode material, carbon black, and PVDF provided by the present invention in a mass ratio of 90:5:5, apply it on an aluminum foil, vacuum dry it at 110°C, slice it, and make a 14mm diameter and 10mg cm-1 battery. -2The positive electrode sheet is used, and lithium metal is used as the negative electrode; the electrolyte is 1M LiPF6 electrolyte, and its solvent is EC:DEC:DMC (1:1:1), and the button battery is assembled in a glove box.

[0026] The capacity retention rate refers to the ratio of the initial capacity that a lithium battery can maintain after a certain charge and discharge cycle. The capacity retention rate of the present invention refers to the ratio between the discharge specific capacity of the button battery after 200 cycles under the conditions of 2-4.3V voltage range and 1C rate to the first cycle discharge specific capacity.

[0027] Voltage retention rate refers to the ratio of the initial voltage that a lithium battery can maintain after a certain charge and discharge cycle. Specifically, it refers to the ratio between the current voltage and the initial voltage.

[0028] The present invention does not limit the thickness of the lithium phosphate coating layer and the amorphous carbon coating layer. In a specific embodiment of the present invention, the thickness of the lithium phosphate coating layer is 2-4 nm, and the thickness of the amorphous carbon coating layer is 2-4 nm.

[0029] The thickness of the lithium phosphate coating layer in the present invention refers to the average thickness, and the thickness of the amorphous carbon coating layer in the present invention also refers to the average thickness. The thickness can be obtained by transmission electron microscopy.

[0030] In detail, the thickness of the lithium phosphate coating layer includes but is not limited to 2nm, 2.2nm, 2.4nm, 2.6nm, 2.8nm, 3nm, 3.2nm, 3.4nm, 3.6nm, 3.8nm, 4nm or a range consisting of any two of them.

[0031] The thickness of the amorphous carbon coating layer includes but is not limited to 2 nm, 2.2 nm, 2.4 nm, 2.6 nm, 2.8 nm, 3 nm, 3.2 nm, 3.4 nm, 3.6 nm, 3.8 nm, 4 nm or a range consisting of any two thereof.

[0032] The present invention does not limit the method for controlling the thickness. It is understood that the thickness of the two can be controlled by controlling the addition amount of lithium phosphate and amorphous carbon source during the preparation process and the preparation conditions.

[0033] When the thickness of the lithium phosphate coating layer is within the above range, it can effectively serve as a fast ion conductor layer to accelerate the Li + Diffusion rate. When the thickness of the amorphous carbon coating layer is within the above range, it can effectively serve as a surface coating layer, accelerate electronic conductivity and enhance the stability of the interface during the cycle.

[0034] In one embodiment of the present invention, the chemical formula of the lithium manganese iron phosphate core is LiMn x Fe 1-x PO4, x is 0.6.

[0035] When x is within the above range, the Mn 3+ The reduction stage has a larger Li + Diffusion coefficient, Mn 3+ Can be more fully reduced to Mn under high pressure 2+ , giving full play to the advantages of energy density.

[0036] The lithium iron manganese phosphate positive electrode material provided by the present invention has an excellent capacity retention rate at 45°C. Therefore, the lithium iron manganese phosphate positive electrode material provided by the present invention has excellent cycle performance in a high temperature environment. The inventor analyzed that the reason may be that the nano-scale lithium iron manganese phosphate cores coated with Li3PO4 are bonded together under the action of Li3PO4, providing a basis for the subsequent double carbon coating. The presence of the Li3PO4 coating layer can well separate the nano-scale lithium iron manganese phosphate cores from each other, while the lithium iron manganese phosphate cores are bonded to each other, retaining their original size without melting and growing, so that it has a faster Li + Diffusion kinetics, Mn 3+ It is fully reduced at the high voltage platform of 4.1V, retaining its advantage of high energy density. At the same time, Li3PO4 has good electronic conductivity and structural stability. Its coating on the surface of lithium manganese iron phosphate particles can effectively prevent the dissolution of Mn and the contact between the outermost interface and the electrolyte, thus stabilizing the lattice. The amorphous carbon produced by the decomposition of organic carbon sources at high temperatures forms a uniform carbon coating layer on the surface of secondary particles, which can effectively separate the lithium manganese iron phosphate core from the electrolyte, protect its interface structure, and thus improve the cycle stability and voltage stability of the lithium manganese iron phosphate positive electrode material.

[0037] Furthermore, in a specific embodiment of the present invention, the capacity retention rate of the lithium manganese iron phosphate positive electrode material after 200 cycles at 1C / 2-4.3V at 45°C is not less than 94%.

[0038] When the capacity retention rate is within the above range, the lithium manganese iron phosphate positive electrode material has better cycle stability.

[0039] Furthermore, in a specific embodiment of the present invention, at least a portion of the surface of the amorphous carbon coating layer is covered with a conductive carbon network.

[0040] The conductive carbon mesh in the present invention achieves connection with the lithium iron manganese phosphate particles by covering at least part of the surface of the coating layer, wherein the lithium iron manganese phosphate particles refer to particles including a lithium iron manganese phosphate core and a coating layer covering at least part of the surface of the lithium iron manganese phosphate core.

[0041] The lithium iron manganese phosphate particles are connected by a conductive carbon mesh to form a conductive network between the particles, which further improves the electronic conductivity, reduces the polarization generated during the charging and discharging process, and ensures that the material capacity is fully utilized. This can not only improve the cycle stability of the lithium iron manganese phosphate positive electrode material, but also further inhibit voltage decay.

[0042] Furthermore, in a specific embodiment of the present invention, the median particle size D50 of the lithium manganese iron phosphate core is 0.4-0.5 μm.

[0043] It can be understood that D50 is usually used to indicate the average particle size of the lithium iron manganese phosphate core, that is, the particle size corresponding to when the cumulative particle size distribution percentage of the lithium iron manganese phosphate core reaches 50%.

[0044] Specifically, the particle size D50 of the lithium manganese iron phosphate core includes but is not limited to 0.4μm, 0.41μm, 0.42μm, 0.43μm, 0.44μm, 0.45μm, 0.46μm, 0.47μm, 0.48μm, 0.49μm, 0.5μm or a range consisting of any two of them.

[0045] When the D50 of the lithium iron manganese phosphate core is within the above range, the core has a larger specific surface area and provides more active surfaces. Lithium ions can be quickly deintercalated in the lithium iron manganese phosphate, which increases the transfer rate of lithium ions and further reduces the impedance of the lithium iron manganese phosphate, thereby making the cycle performance and rate performance of the lithium iron manganese phosphate better.

[0046] Furthermore, in a specific embodiment of the present invention, the mass ratio of the lithium manganese iron phosphate core, the lithium phosphate coating layer, the amorphous carbon coating layer and the conductive network is 100:1:5:0.5.

[0047] It can be understood that the quality relationship of each component can be controlled by controlling the addition amount of each type of raw material during the preparation process.

[0048] When the mass relationship between the various components of the lithium iron manganese phosphate positive electrode material is in line with the above range, lithium phosphate can fully bond the nano-scale lithium iron manganese phosphate cores together; and the amorphous carbon layer is evenly coated on the surface of the secondary particles; the conductive network is evenly dispersed between the particles, thereby obtaining a lithium iron manganese phosphate positive electrode material with good cycle stability and voltage stability.

[0049] In another aspect, the present invention provides a method for preparing the lithium manganese iron phosphate positive electrode material as described above, comprising the following steps: 1) ball milling a mixture including a lithium iron manganese phosphate precursor, Li3PO4, and an amorphous carbon source at 200-2000 r / min for 2-13 hours, and then drying at 80-120° C. for 6-24 hours to obtain a precursor powder; 2) The precursor powder is heated to 600-900°C at a heating rate of 3-5°C / min and calcined for 5-15h to obtain a lithium manganese iron phosphate positive electrode material.

[0050] The preparation method provided by the present invention is used to prepare the above-mentioned lithium manganese iron phosphate positive electrode material.

[0051] In detail, in step 1), the lithium iron manganese phosphate precursor, lithium phosphate and amorphous carbon source are placed in a ball mill, and ball milled at 200-2000 r / min for 2-13 hours in a ball milling aid, and the ball-milled powder is placed in an oven and dried at 80-120° C. for 6-24 hours to obtain a precursor powder.

[0052] The lithium iron manganese phosphate precursor in the present invention can use commercially available lithium iron manganese phosphate, or can be prepared by itself.

[0053] In one specific embodiment, the method for preparing the lithium manganese iron phosphate precursor comprises the following steps: The iron source, the manganese source, the lithium salt, the phosphate and the organic carbon source are first ball-milled and dried to obtain a precursor 1; The precursor 1 is placed in a nitrogen atmosphere for heat treatment to obtain a lithium manganese iron phosphate precursor, and the heat treatment temperature is 200-500°C.

[0054] The amorphous carbon source refers to a substance containing carbon elements that can be used to prepare lithium manganese iron phosphate positive electrode materials and form an amorphous carbon layer. The present invention does not specifically limit the selection of the amorphous carbon source, and commonly used substances in the art can be used. In one embodiment, the amorphous carbon source is selected from at least one of glucose, sucrose, and citric acid.

[0055] The present invention does not limit the specific type of the ball milling aid, as long as it is a solution that can play a dispersing role, such as ethanol, water, acetone, etc.

[0056] In step 2), the precursor powder is placed in a tubular furnace, heated to 600-900° C. at a heating rate of 3-5° C. / min, and calcined for 5-15 hours to obtain a lithium manganese iron phosphate positive electrode material.

[0057] In order to avoid the influence of impurities on the reaction, calcination can be carried out under a protective gas atmosphere. In a specific embodiment, the protective gas is selected from at least one of argon, helium and nitrogen.

[0058] In another specific embodiment, in step 2), the calcination temperature is 750° C. and the calcination time is 8 hours.

[0059] The inventors found that the lithium iron manganese phosphate positive electrode material prepared by the preparation method of the lithium iron manganese phosphate positive electrode material provided by the present invention has excellent cycle performance and voltage stability. The inventors speculate that the reason may be that the lithium iron manganese phosphate positive electrode material obtained in the present invention is a multi-coated lithium iron manganese phosphate positive electrode material. The nano-sized primary particles have faster Li + Diffusion kinetics, so that Mn 3+ It is fully reduced under a high voltage of 4.1V to ensure its energy density. The primary coating layer Li3PO4 and the secondary coating layer amorphous carbon layer on the surface stabilize the surface structure of the material, alleviate the structural collapse and capacity decay caused by Mn dissolution and side reactions between the electrolyte and the outermost interface of the material during the cycle, and improve the cycle stability of the material; at the same time, the amorphous carbon layer effectively improves the electronic conductivity of the lithium manganese iron phosphate positive electrode material from the secondary particle dimension. At the same time, the two-dimensional conductive network formed by the third layer of conductive carbon mesh coating between the secondary particles accelerates the electronic conductivity, reduces the polarization generated during the charge and discharge process, and ensures the full utilization of the material capacity.

[0060] Furthermore, in a specific embodiment of the present invention, in step 1), the mixture also includes a conductive carbon source.

[0061] The conductive carbon source refers to a substance containing carbon elements that can be used to prepare lithium manganese iron phosphate positive electrode materials and form a conductive network. The present invention does not specifically limit the selection of the conductive carbon source, and commonly used substances in the field can be used. In one embodiment, the conductive carbon source is selected from at least one of carbon nanotubes, acetylene black, and Ketjen black.

[0062] When the mixture in step 1) includes a conductive carbon source, the prepared lithium iron manganese phosphate positive electrode material includes a lithium iron manganese phosphate core and a coating layer coated on at least a portion of the surface of the lithium iron manganese phosphate core, and a conductive carbon mesh coated on at least a portion of the surface of the coating layer. Therefore, the lithium iron manganese phosphate positive electrode material not only has excellent cycle stability, but also can effectively inhibit voltage decay.

[0063] Furthermore, in a specific embodiment of the present invention, between step 1) and step 2), the precursor powder is subjected to a thermal shock treatment, and the thermal shock treatment comprises the following steps: The precursor powder was mixed at 10 3 -10 5 The temperature was raised to 300-500℃ at a heating rate of 10℃ / s and maintained for 1-60s. 3 -10 5 The temperature was cooled to room temperature at a cooling rate of ℃ / s.

[0064] Specifically, the precursor powder is placed on a heating substrate of a heating device under a protective atmosphere for 10 3 -105 The temperature was raised to 300-500℃ at a heating rate of 10℃ / s and maintained for 1-60s. 3 -10 5 The temperature was cooled to room temperature at a cooling rate of ℃ / s.

[0065] The present invention does not limit the specific type of the heating substrate, and a common heating substrate in the art can be selected according to actual conditions.

[0066] In one embodiment, the heating substrate is selected from at least one of carbon cloth, carbon paper, carbon felt, graphite sheet, nickel foil, cobalt foil, and stainless steel sheet.

[0067] After the powder is subjected to thermal shock treatment, the lithium iron manganese phosphate positive electrode material finally prepared has a more excellent capacity retention rate. The inventors analyzed that the reason may be that the amorphous carbon source decomposes rapidly during the ultra-fast heating process, generating a large amount of gas, and squeezing the lithium phosphate to make it more tightly combined with the lithium iron manganese phosphate precursor, which has the effect of grain boundary strengthening, and then rapidly cooling down to retain the dense structure of the lithium iron manganese phosphate precursor-lithium phosphate coating-amorphous carbon coating. Subsequently, the lithium iron manganese phosphate positive electrode material with a stable interface layer is finally formed through long-term calcination in a traditional tubular furnace.

[0068] In another aspect, the present invention provides a positive electrode sheet, comprising the lithium iron manganese phosphate positive electrode material as described above or the lithium iron manganese phosphate positive electrode material prepared by the preparation method as described above.

[0069] The positive electrode sheet of the present invention specifically comprises a positive electrode current collector and a positive electrode active layer formed of a lithium manganese iron phosphate positive electrode material and arranged on the surface of the positive electrode current collector.

[0070] When preparing the positive electrode sheet, for example, the lithium iron manganese phosphate positive electrode material of the present invention, the conductive agent and the binder can be dispersed in an appropriate amount of N-methylpyrrolidone (NMP) solvent, and the mixture is stirred and mixed to form a uniform positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode current collector, and the positive electrode sheet is obtained after drying, rolling and cutting. In a specific embodiment, the positive electrode active layer includes 70-99 wt% of the lithium iron manganese phosphate positive electrode material, 0.5-15 wt% of the conductive agent, and 0.5-15 wt% of the binder according to the mass percentage, and further includes 80-98 wt% of the lithium iron manganese phosphate positive electrode material, 1-10 wt% of the conductive agent, and 1-10 wt% of the binder.

[0071] Among them, the material of the positive electrode current collector can be at least one of aluminum foil and nickel foil; the conductive agent can be selected from at least one of carbon black, acetylene black, graphene, Ketjen black, and carbon fiber; the binder can be selected from at least one of polytetrafluoroethylene, polyvinylidene fluoride, polyvinyl fluoride, polyethylene, polypropylene, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, and polyurethane.

[0072] Since the lithium manganese iron phosphate positive electrode material provided by the present invention has the characteristic of excellent cycle performance, the positive electrode sheet provided by the present invention also has the characteristic of excellent cycle performance.

[0073] In another aspect, the present invention provides a battery, comprising the lithium manganese iron phosphate positive electrode material or the positive electrode sheet as described above.

[0074] It is conceivable that the battery provided by the present invention includes, in addition to the above-mentioned positive electrode sheet, a negative electrode sheet, an electrolyte and a separator.

[0075] The present invention does not strictly limit the negative electrode active material in the negative electrode sheet, and can be at least one of the negative electrode active materials commonly used in lithium-ion batteries, such as graphite, hard carbon, soft carbon, mesophase carbon microbeads, silicon-based negative electrode materials (mainly including silicon oxide, silicon-carbon negative electrode), tin-based negative electrode materials (mainly including tin, tin alloy), etc.

[0076] The present invention does not strictly limit the selection of the electrolyte, and may include one or more of the solvents commonly used in the current lithium-ion battery electrolyte, and the electrolyte lithium salts commonly used in the current lithium-ion electrolyte, for example: the solvent may be ethylene carbonate, propylene carbonate, butylene carbonate, fluoroethylene carbonate (FEC), dimethyl carbonate (DMC), diethyl carbonate (DEC), difluoroethylene carbonate (DFEC), dipropyl carbonate, ethyl methyl carbonate (EMC), ethyl acetate, ethyl propionate, propyl acetate, propyl propionate, cyclopentane, γ-butyrolactone, etc.; the lithium salt may be, for example, one or more of lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), and lithium bis(trifluoromethylsulfonyl)imide (LiTFSI).

[0077] The present invention does not strictly limit the material selection of the diaphragm, which can be a diaphragm material commonly used in lithium-ion batteries, such as a polypropylene diaphragm (PP), a polyethylene diaphragm (PE), a polypropylene / polyethylene double-layer composite film (PP / PE), a polyimide electrospinning diaphragm (PI), a polypropylene / polyethylene / polypropylene three-layer composite film (PP / PE / PP), a cellulose non-woven fabric diaphragm, or a diaphragm with a ceramic coating.

[0078] When preparing lithium-ion batteries, the positive electrode sheet, separator and negative electrode sheet are wound or stacked to obtain a bare cell, and the bare cell is packaged in a pre-stamped aluminum-plastic film bag. After the packaged battery is dried at 85°C, the electrolyte is injected into the dry battery, and the battery is placed, formed and sealed for the second time to complete the preparation of the lithium-ion battery.

[0079] The preparation method of the lithium manganese iron phosphate positive electrode material provided by the present invention will be described in detail below with reference to specific embodiments.

[0080] Example 1 The preparation method of the lithium manganese iron phosphate positive electrode material provided in this embodiment comprises the following steps: 1. Weigh the lithium manganese iron phosphate precursor (chemical formula LiMn 0.6 Fe 0.4 PO4), Li3PO4, sucrose and carbon nanotubes were placed in a ball mill and wet-milled in water at a speed of 600r / min for 4h. Finally, the powder obtained after ball milling was placed in a vacuum oven at 100℃ and dried for 8h to obtain a precursor powder.

[0081] 2. Place the precursor powder on a heated substrate on a heating device in a protective atmosphere and heat it for 10 3 The temperature was raised to 300℃ at a heating rate of 10℃ / s for 10s, and then 3 The cooling rate was ℃ / s down to room temperature; 3. The powder subjected to the thermal shock treatment was placed in a tubular furnace in an argon protective atmosphere, and the temperature was raised to 750° C. at 5° C. / min and calcined for 8 h to obtain a lithium manganese iron phosphate positive electrode material.

[0082] Tests show that the median particle size D50 of the lithium iron manganese phosphate core in the lithium iron manganese phosphate positive electrode material provided in this embodiment is 0.5 μm, the mass ratio of the lithium iron manganese phosphate core, the lithium phosphate coating layer, the amorphous carbon coating layer and the conductive carbon mesh is 100%:2%:10%:1%, the thickness of the lithium iron manganese phosphate coating layer is 4 nm, and the thickness of the amorphous carbon coating layer is 3.5 nm.

[0083] Example 2 The preparation process of the lithium manganese iron phosphate positive electrode material provided in this embodiment includes the following steps: 1. Weigh the lithium iron manganese phosphate precursor (chemical formula LiMn 0.6 Fe 0.4PO4), Li3PO4, glucose and carbon nanotubes were placed in a ball mill and wet-milled in water at a speed of 1000 r / min for 2 h. Finally, the powder obtained after ball milling was placed in a vacuum oven at 80 ° C and dried for 10 h to obtain a precursor powder; 2. Place the precursor powder on a heated substrate on a heating device in a protective atmosphere and heat it according to 10 5 The temperature was raised to 500°C at a heating rate of 10°C / s and held for 2s. 5 The temperature was cooled to room temperature at a cooling rate of ℃ / s; 3. The precursor powder after the thermal shock treatment is placed in a tubular furnace in a protective atmosphere, heated to 700° C. at a heating rate of 5° C. / min and calcined for 10 h to obtain a lithium manganese iron phosphate positive electrode material.

[0084] Tests show that the median particle size D50 of the lithium iron manganese phosphate core in the lithium iron manganese phosphate positive electrode material provided in this embodiment is 0.4 μm, the mass ratio of the lithium iron manganese phosphate core, the lithium phosphate coating layer, the amorphous carbon coating layer and the conductive carbon mesh is 100%:1%:10%:0.5%, the thickness of the lithium iron manganese phosphate coating layer is 2 nm, and the thickness of the amorphous carbon coating layer is 3.5 nm.

[0085] Example 3 The preparation method of the lithium manganese iron phosphate positive electrode material provided in this embodiment is basically the same as that in Example 2, except that: In step 1), the lithium iron manganese phosphate precursor (chemical formula LiMn 0.6 Fe 0.4 PO4), lithium phosphate, glucose and carbon nanotubes in a mass ratio of 100%:1%:5%:0.5%.

[0086] Tests show that the median particle size D50 of the lithium iron manganese phosphate core in the lithium iron manganese phosphate positive electrode material provided in this embodiment is 0.4 μm, the mass ratio of the lithium iron manganese phosphate core, the lithium phosphate coating layer, the amorphous carbon coating layer and the conductive carbon mesh is 100%:1%:5%:0.5%, the thickness of the lithium iron manganese phosphate coating layer is 2 nm, and the thickness of the amorphous carbon coating layer is 2 nm.

[0087] Example 4 The preparation method of the lithium manganese iron phosphate positive electrode material provided in this embodiment is basically the same as that in embodiment 3, except that: In step 1), the ball milling is performed at a speed of 600 r / min for 1 h.

[0088] Tests show that the median particle size D50 of the lithium iron manganese phosphate core in the lithium iron manganese phosphate positive electrode material provided in this embodiment is 0.5 μm, the mass ratio of the lithium iron manganese phosphate core, the lithium phosphate coating layer, the amorphous carbon coating layer and the conductive carbon mesh is 100%:1%:5%:0.5%, the thickness of the lithium phosphate coating layer is 2 nm, and the thickness of the amorphous carbon coating layer is 2 nm.

[0089] Example 5 The preparation method of the lithium manganese iron phosphate positive electrode material provided in this embodiment is basically the same as that in embodiment 3, except that: The heat shock treatment in step 2) was not performed.

[0090] The test results show that the median particle size D50 of the lithium iron manganese phosphate core in the lithium iron manganese phosphate positive electrode material provided in this embodiment is 0.4 μm, and the mass ratio of the lithium iron manganese phosphate core, the lithium phosphate coating layer, the amorphous carbon coating layer and the conductive carbon mesh is 100%: 1%: 5%: 0.5%. The thickness of the lithium iron manganese phosphate coating layer is 2 nm, and the thickness of the amorphous carbon coating layer is 2 nm.

[0091] Comparative Example 1 The preparation method of the lithium manganese iron phosphate positive electrode material provided in this comparative example is basically the same as that in Example 3, except that: In step 1), lithium iron manganese phosphate precursor (chemical formula LiMn 0.6 Fe 0.4 PO4) and glucose, that is, lithium phosphate and carbon nanotubes are not added, and the high temperature thermal shock treatment in step 2) is not performed.

[0092] Comparative Example 2 The preparation method of the lithium manganese iron phosphate positive electrode material provided in this comparative example is basically the same as that in Example 3, except that: In step 1), lithium iron manganese phosphate precursor (chemical formula: LiMn 0.6 Fe 0.4 PO4), ammonium fluoride, indium sulfide, sucrose and carbon nanotubes.

[0093] Test Case 1. Electrochemical performance test The lithium manganese iron phosphate positive electrode material prepared in each embodiment and comparative example is made into a positive electrode sheet, and then assembled with a negative electrode sheet, an electrolyte and a separator according to the following method to obtain a button battery. The method includes: The positive electrode materials in the examples and comparative examples were mixed with conductive carbon black (SP) and PVDF in a weight ratio of 90%:5%:5% respectively, and a positive electrode slurry was obtained by dispersion. The slurry was coated on an aluminum foil current collector and rolled to obtain a positive electrode slurry with a surface density of 10 mg / cm 2 The positive electrode sheet is then punched out into a small disc with a diameter of 14 mm using a film mold. After drying and weighing, a button battery is assembled together in a glove box under an Ar protective atmosphere using a 2025 button battery shell and a Li metal disc as the negative electrode, a 1M LiPF6 electrolyte, and an EC:DEC:DMC (1:1:1) solvent.

[0094] At 45°C, the battery was charged to 4.3V at a constant current of 1C, then charged to 4.3V at a constant voltage of 0.05C, and then discharged to 2.0V at a discharge rate of 1C. This charge and discharge cycle was repeated 200 times. The discharge capacity Q1 at the first cycle to the discharge capacity Q at the 200th cycle at different temperatures was measured. 200 , calculate the capacity retention rate, see Table 1 for details.

[0095] Among them, the capacity retention rate Q=Q 200 / Q1*100% Figure 1 The voltage decay diagram of the lithium manganese iron phosphate positive electrode material prepared in Example 1 of the present invention after 200 cycles at a high temperature of 45°C and 1C, Figure 2 This is a graph showing the capacity retention rate of the lithium manganese iron phosphate positive electrode material prepared in Example 1 of the present invention after 200 cycles at a high temperature of 45° C. and 1C; Figure 3 The voltage decay diagram of the lithium manganese iron phosphate positive electrode material prepared in Example 2 of the present invention after 200 cycles at a high temperature of 45°C and 1C, Figure 4 This is a graph showing the capacity retention rate of the lithium manganese iron phosphate positive electrode material prepared in Example 2 of the present invention after 200 cycles at a high temperature of 45° C. and 1C; Figure 5 The voltage decay diagram of the lithium manganese iron phosphate positive electrode material prepared in Comparative Example 1 of the present invention after 200 cycles at a high temperature of 45°C and 1C is shown in FIG. Figure 6 This is a graph showing the capacity retention rate of the lithium manganese iron phosphate positive electrode material prepared in Comparative Example 1 of the present invention after 200 cycles at a high temperature of 45°C and 1C; Figure 7 The voltage decay diagram of the lithium manganese iron phosphate positive electrode material prepared in Example 3 of the present invention after 200 cycles at a high temperature of 45°C and 1C, Figure 8 This is a graph showing the capacity retention rate of the lithium manganese iron phosphate positive electrode material prepared in Example 3 of the present invention after 200 cycles at a high temperature of 45° C. and 1C; Fig. 9 The voltage decay diagram of the lithium manganese iron phosphate positive electrode material prepared in Example 4 of the present invention after 200 cycles at a high temperature of 45°C and 1C, Fig.10This is a graph showing the capacity retention rate of the lithium manganese iron phosphate positive electrode material prepared in Example 4 of the present invention after 200 cycles at a high temperature of 45° C. and 1C; Fig.11 The voltage decay diagram of the lithium manganese iron phosphate positive electrode material prepared in Example 5 of the present invention after 200 cycles at a high temperature of 45°C and 1C, Fig.12 This is a graph showing the capacity retention rate of the lithium manganese iron phosphate positive electrode material prepared in Example 5 of the present invention after 200 cycles at a high temperature of 45° C. and 1C; Fig.13 The voltage decay diagram of the lithium manganese iron phosphate positive electrode material prepared in Comparative Example 2 of the present invention after 200 cycles at a high temperature of 45°C and 1C is shown in FIG. Fig.14 This is a graph of the capacity retention rate of the lithium manganese iron phosphate positive electrode material prepared in Comparative Example 2 of the present invention after 200 cycles at a high temperature of 45°C and 1C.

[0096] Table 1

[0097] 2. Volumetric Indirect Titration (CITT) The lithium iron manganese phosphate positive electrode material provided in Example 3 and the lithium iron manganese phosphate positive electrode material provided in Comparative Example 1 were subjected to a CITT test, which specifically includes the following steps: The test voltage range is 2-4.3 V. The battery is discharged at a current density of 0.05 C, and is left for 5 h after each 30 min discharge until it reaches the lower cut-off voltage. The test process for charging is similar to that for discharging.

[0098] Fig.15 This is a CITT comparison chart of the lithium iron manganese phosphate positive electrode material prepared in Example 3 of the present invention and the lithium iron manganese phosphate positive electrode material prepared in Comparative Example 1.

[0099] like Fig.15 As shown, the lithium manganese iron phosphate positive electrode material provided in Example 3 has Mn 3+ The reduction stage has a larger Li + This indicates that the nano-scale lithium manganese iron phosphate core, Li3PO4 coating layer, amorphous carbon coating layer and conductive carbon network in the present invention greatly improve the Li + diffusion coefficient, especially when the molar amount of Li in the lithium manganese iron phosphate core is between 0.05 and 0.55, compared with the lithium manganese iron phosphate positive electrode material provided in Comparative Example 1 obtained by the conventional method with only one layer of amorphous carbon coating and no high-temperature thermal shock treatment, the Mn in the lithium manganese iron phosphate positive electrode material provided in Example 3 is 3+ Can be more fully reduced to Mn under high pressure 2+ , giving full play to the advantages of energy density.

[0100] 3. Electron microscope detection Scanning electron microscopy and transmission electron microscopy were performed on the lithium manganese iron phosphate positive electrode materials of some embodiments and some comparative examples before and after cycling.

[0101] in, Fig.16 The transmission electron microscope (TEM) images of the lithium manganese iron phosphate positive electrode material prepared in Example 3 at different magnifications are shown. Fig.16 As shown in a, under the action of Li3PO4, the nano-scale lithium manganese iron phosphate cores are bonded together; Fig.16 As shown in b, the surface of the bonded lithium manganese iron phosphate core is coated with an amorphous carbon coating layer; Fig.16 As shown in c, carbon nanotubes connect numerous lithium manganese iron phosphate particles together to form a conductive network.

[0102] Fig.17 The XRD diagram of the lithium manganese iron phosphate positive electrode material prepared in Comparative Example 1 of the present invention before and after 200 cycles at 45°C. Fig.18 The XRD diagram of the lithium iron manganese phosphate positive electrode material prepared in Example 3 of the present invention before and after 200 cycles of high-temperature cycling at 45°C. It can be seen that the lithium iron manganese phosphate positive electrode material prepared in Example 3 does not show obvious peak shift phenomenon before and after the cycle and no impurity phase is generated, and has better structural stability during the high-temperature cycling process.

[0103] Fig.19 This is a transmission electron microscope (TEM) image of the lithium iron manganese phosphate positive electrode material prepared in Example 3 of the present invention. It can be clearly seen from the image that three different regions of lithium iron manganese phosphate-intermediate interface layer-peripheral protective layer are formed, and the three regions are closely connected. This shows that the ultra-fast thermal shock is used in the present invention to successfully achieve grain boundary strengthening.

[0104] Fig. 20 This is a transmission electron microscope (TEM) spectrum of the high-performance lithium manganese iron phosphate positive electrode material prepared in Example 3 of the present invention after 200 cycles at a high temperature of 45°C and 1C, wherein Fig. 20 a in the figure is a partial enlarged view of part A. Fig. 20 b is a partial enlarged view of part B; Fig.21 The transmission electron microscope (TEM) spectrum of the lithium manganese iron phosphate positive electrode material prepared in Comparative Example 1 of the present invention after 200 cycles at a high temperature of 45°C and 1C, wherein Fig.21 (a) is a partial enlarged view of part A. Fig.21 (b) is a partial enlarged view of part b. It is observed that the lithium manganese iron phosphate positive electrode material provided in Example 3 still has a perfect lattice structure after 200 cycles of high temperature cycling. In contrast, the lithium manganese iron phosphate positive electrode material provided in Comparative Example 1 has more amorphous areas on its surface, which indicates that its crystal structure is destroyed during the cycle.

[0105] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A lithium manganese iron phosphate positive electrode material, characterized in that: It comprises a lithium iron manganese phosphate core and a coating layer coated on at least a part of the surface of the lithium iron manganese phosphate core; The coating layer includes a lithium phosphate coating layer and an amorphous carbon coating layer covering at least a portion of the surface of the lithium phosphate coating layer; The capacity retention rate of the lithium manganese iron phosphate positive electrode material after 200 cycles at 45° C. and 1C / 2-4.3V conditions is not less than 92%, and the voltage retention rate is not less than 90%.

2. The lithium iron manganese phosphate positive electrode material according to claim 1, characterized in that: The capacity retention rate of the lithium manganese iron phosphate positive electrode material after 200 cycles at 45° C. and 1C / 2-4.3V conditions is not less than 94%.

3. The lithium iron manganese phosphate positive electrode material according to claim 1 or 2, characterized in that: At least a portion of the surface of the amorphous carbon coating layer covers the conductive carbon network.

4. The lithium iron manganese phosphate positive electrode material according to claim 2 or 3, characterized in that: The median particle size D50 of the lithium manganese iron phosphate core is 0.4-0.5 μm.

5. The lithium iron manganese phosphate positive electrode material according to any one of claims 2 to 4, characterized in that: The mass ratio of the lithium manganese iron phosphate core, the lithium phosphate coating layer, the amorphous carbon coating layer and the conductive carbon mesh is 100:1:5:0.

5.

6. A method for preparing the lithium manganese iron phosphate positive electrode material according to any one of claims 1 to 5, characterized in that: The following steps are involved: 1) ball milling a mixture including a lithium iron manganese phosphate precursor, Li3PO4, and an amorphous carbon source at 200-2000 r / min for 2-13 hours, and then drying at 80-120° C. for 6-24 hours to obtain a precursor powder; 2) The precursor powder is heated to 600-900° C. at a heating rate of 3-5° C. / min and calcined for 5-15 hours to obtain the lithium manganese iron phosphate positive electrode material.

7. The preparation method according to claim 6, characterized in that: In step 1), the mixture further includes a conductive carbon source.

8. The preparation method according to claim 6 or 7, characterized in that: Between step 1) and step 2), the powder is subjected to a thermal shock treatment, wherein the thermal shock treatment comprises the following steps: The powder was mixed according to 10 3 -10 5 The temperature was raised to 300-500℃ at a heating rate of 10℃ / s and maintained for 1-60s. 3 -10 5 The temperature was cooled to room temperature at a cooling rate of ℃ / s.

9. A positive electrode sheet, characterized in that: The invention comprises the lithium iron manganese phosphate positive electrode material as described in any one of claims 1 to 5 or the lithium iron manganese phosphate positive electrode material prepared by the preparation method as described in claims 6 to 8.

10. A battery, characterized in that: It comprises the lithium manganese iron phosphate positive electrode material as described in any one of claims 1 to 5 or the positive electrode sheet as described in claim 9.

Citation Information

Patent Citations

  • Manganese-iron-lithium phosphate material and preparation method thereof, battery paste, cathode and lithium battery

    CN106816600A

  • Preparation method and application of lithium ferric manganese phosphate positive electrode material

    CN115172681A

  • Preparation method of carbon and germanium-aluminum-lithium phosphate dual-coated lithium manganese iron phosphate positive electrode material

    CN115498162A

  • Preparation method and application of conductive carbon-coated additive for lithium battery positive electrode material

    CN117577810A

  • Lithium manganese iron phosphate composite material as well as preparation method and application thereof

    CN117747798A

Cited By

  • Positive electrode active material, battery, and method of producing positive electrode active material

    EP4738440A1

  • Positive electrode active material, electrode, and battery

    EP4769549A1