Polymer matrix composite silicon-based lithium ion battery negative electrode material and preparation method thereof

Through polymer matrix composite materials of polyethylene oxide, graphite and silicon or silicon oxide, the problems of volume expansion and conductive network stability of silicon-based lithium battery anode materials are solved, and lithium-ion batteries with high specific capacity and long cycle life are realized. negative electrode material.

CN118763205APending Publication Date: 2024-10-11INST OF ENERGY HEFEI COMPREHENSIVE NAT SCI CENT (ANHUI ENERGY LAB)
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411039060.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The volume expansion of silicon-based lithium battery anode materials during the lithiation/delithiation process leads to the crushing of active materials and instability of the SEI film, which limits its cycle performance and application. The existing inorganic coating methods are complex and difficult to form a stable conductive network.

Method used

Polyethylene oxide, graphite and silicon or silicon oxide are mixed to prepare polymer matrix composite materials. Through high temperature treatment, a uniform conductive layer is formed to buffer the volume effect and improve electronic conductivity, and establish structural stability.

Benefits of technology

A simplified preparation method and good cycle stability are achieved, and the specific capacity retention rate and battery cycle life of the anode material are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763205A_ABST
    Figure CN118763205A_ABST
Patent Text Reader

Abstract

The invention discloses a polymer matrix composite silicon-based lithium ion battery negative electrode material and a preparation method of the polymer matrix composite silicon-based lithium ion battery negative electrode material, and belongs to the technical field of lithium ion battery negative electrode materials. And mixing with a silicon-based material, and performing thermal high-temperature treatment to obtain the polymer matrix compounded silicon-based lithium ion battery negative electrode material. The material is characterized in that a uniform coating is established on the surface of silicon / graphite or silicon monoxide / graphite to prevent direct contact with an electrolyte, so that a conductive path is improved to the greatest extent, the integrity of a negative electrode active material is maintained through high structural stability, the electronic conductivity is improved, the formation of an SEI film is effectively controlled, and the service life of a battery is prolonged. The silicon carbon material coated with the polymer matrix has relatively high lithium storage capacity and good cycling stability, the cost of synthetic raw materials is low, and the preparation process is simple and controllable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of negative electrode materials for lithium batteries, and in particular relates to a polymer matrix composite silicon-based negative electrode material for lithium ion batteries and a preparation method thereof. Background Art

[0002] As an important secondary chemical power source, lithium-ion batteries have been widely used since they were put on the market. Lithium battery anode materials are one of the key indicators that affect the energy density and cycle performance of lithium-ion batteries. At present, graphite is the main anode material. The theoretical specific capacity of mainstream commercial graphite anode products is above 350mAh / g, which is close to the theoretical specific capacity upper limit of 372mAh / g. Therefore, it is urgent to develop a lithium battery anode material with higher specific capacity. The theoretical specific capacity of silicon is as high as 4200mAh / g, and it is considered to be the next generation of anode materials. Although silicon-based anodes have advantages such as high theoretical capacity and low cost, their large-scale application is still limited. The main obstacles to the application of silicon-based anodes are the volume expansion of silicon-based materials during the lithiation / delithiation process, the crushing of negative electrode active materials caused by volume changes, the formation of unstable SEI films on the surface, and the destruction of electronic conductive networks. In order to suppress the volume expansion of silicon-based anodes during lithium insertion, graphite is usually added to form silicon-carbon anodes and silicon-oxygen / carbon anodes. This doping strategy has been used in many patents and papers. In order to improve the cycle performance of the negative electrode, inorganic coating is usually performed on the surface. However, the coating method is complicated to operate and the process is cumbersome, and it is difficult to form a stable conductive network, resulting in its cycle life being unsatisfactory. Summary of the invention

[0003] In order to solve the problems existing in the above-mentioned prior art, the present invention provides a polymer matrix composite silicon-based lithium ion battery negative electrode material and a preparation method thereof, so that it has the advantages of simple preparation method and good cycle stability.

[0004] In order to achieve the purpose, the present invention adopts the following technical scheme: A method for preparing a polymer matrix composite silicon-based lithium ion battery negative electrode material is carried out according to the following steps: Step 1: Precursor synthesis Dissolving graphite and polyethylene oxide in a solvent at a mass ratio of 50:(0.1-1), stirring and mixing, and then heating and evaporating to obtain a dry dispersion, and then mixing the dry dispersion with silicon or silicon oxide to obtain a precursor, wherein the mass ratio of graphite to silicon or silicon oxide is (1-5):1; Step 2: High temperature treatment The precursor prepared in step 1 is placed in a corundum calcining boat and treated at high temperature to obtain a polymer matrix composite silicon-based lithium ion battery negative electrode material.

[0005] Furthermore, in step 1, the average molecular weight of the polyethylene oxide (PEO) is 500,000-900,000.

[0006] Furthermore, in step 1, the solvent is an ethanol-water solution, wherein the volume ratio of ethanol to water is 3:1.

[0007] Furthermore, in step 1, the dried dispersion is polyethylene oxide-coated graphite, and the silicon is nano silicon powder.

[0008] Furthermore, in step 1, the heating temperature is 60-80° C., and the heating time is 1-6 hours.

[0009] Furthermore, in step 2, the high temperature treatment atmosphere is high purity argon or high purity nitrogen.

[0010] Furthermore, in step 2, the high temperature treatment temperature is 700-1000° C., and the high temperature treatment time is 1-7 hours.

[0011] Furthermore, in step 2, the high temperature treatment heating rate is 1-10°C / min.

[0012] Compared with the prior art, the beneficial effects of the present invention are as follows: At present, the most common inorganic coating of silicon-carbon materials and silicon-oxygen / carbon materials is carbon coating. Due to the low permeability and limited contact with silicon particles, the carbon coating will break during the volume expansion process, thereby losing the inhibitory effect on the SEI film; recently, scholars have also designed several polymers as coatings for silicon-carbon materials, such as polypyrrole, polyacrylic acid and polyaniline, but these are all insulating materials or cannot be incorporated within the working voltage range of the silicon-carbon negative electrode, and finally show low capacity and short life. The present invention mixes polyethylene oxide, graphite with pure silicon and silicon oxide or with pure silicon / silicon oxide without graphite to synthesize a composite material, and establishes a uniform coating to prevent direct contact with the electrolyte to maximize the conductive path, improve the electronic conductivity, and maintain the integrity of the negative electrode active material through its high structural stability. On the one hand, the polymer matrix can form a polymer coating layer, which can better buffer the volume effect; on the other hand, by establishing a uniform conductive layer, an efficient electronic conductive network can be formed, which strengthens the structural stability of the composite material, and finally makes the obtained composite material have good cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is a cycle performance diagram of the polymer matrix composite silicon-based lithium-ion battery negative electrode material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0014] In order to have a better understanding of the technical features, purposes and beneficial effects of the present invention, the present invention is further described below in conjunction with the accompanying drawings and specific embodiments, but the present invention is not limited to the following embodiments.

[0015] In the following embodiments of the present invention, the following test method is used to test the cycle performance diagram of the polymer matrix composite silicon-based lithium ion battery negative electrode material prepared in each embodiment. The test method is: the composite material prepared in the embodiment is made into a slurry with lithium polyacrylate as a binder, acetylene black as a conductive agent, and water as a solvent according to a mass ratio of composite material: binder: conductive agent = 6:2:2, and then evenly coated on a copper foil with a coating thickness of 100 μm. After drying, it is cut into electrode sheets with a radius of 12 mm and assembled into a CR2032 type button battery in an argon-filled glove box. The order of assembling the battery is: negative electrode shell-lithium sheet (lithium sheet diameter 15.6 mm, thickness 0.45 mm)-100 μL electrolyte-diaphragm-20 μL electrolyte-electrode sheet-positive electrode shell. The electrolyte is lithium hexafluorophosphate (LiPF6) (LiPF6 is derived from 1 mol / L LiPF6 solution)-ethylene carbonate (EC) / dimethyl carbonate (DMC). The electrolyte is a mixture of 1 mol / L LiPF6 solution, EC and DMC in a volume ratio of 2:1:1. The diaphragm is a Celgard-2400 polypropylene diaphragm. The BTS-5V10mA charge and discharge tester produced by Shenzhen Xinwei Company was used at 1000 mAh g -1 The electrochemical performance of the material was tested in a voltage window of 0.01-3 V at a current density of 1.5 V. The cycle performance of the polymer matrix composite silicon-based lithium ion battery negative electrode material prepared in the test example was tested.

[0016] Example 1 In this example, a polymer matrix composite silicon-based lithium-ion battery negative electrode material is prepared, and the experimental steps are as follows: (a) Precursor synthesis 100 mg of commercial nano-silicon powder, 98 mg of commercial graphite and 2 mg of polyethylene oxide were weighed and added to 100 ml of ethanol aqueous solution for ultrasonic dispersion for 1.5 h, where the volume ratio of ethanol to water was 3:1. Then, the mixture was heated and stirred at 75°C for 4 h and evaporated to dryness to obtain the precursor.

[0017] (b) High temperature treatment Under Ar atmosphere, the temperature was first increased to 350°C at a heating rate of 5°C / min, and calcined at a constant temperature of 350°C for 240 min; then the temperature was increased to 1000°C at a heating rate of 5°C / min, and calcined at a constant temperature for 180 min; and then cooled to room temperature, and the obtained black powder was the polymer matrix composite silicon-based lithium-ion battery negative electrode material.

[0018] The polymer matrix composite silicon-based lithium ion battery negative electrode material obtained in this embodiment is made into a slurry with polypropylene lithium as a binder, acetylene black as a conductive agent, and water as a solvent according to the mass ratio of composite material: binder: conductive agent = 6:2:2, and then coated on copper foil. After drying, it is cut into electrode sheets with a radius of 12mm and assembled into CR2032 button batteries in a glove box filled with argon. The order of assembling the battery is: negative electrode shell-lithium sheet (diameter 15.6mm, thickness 0.45mm)-100μL electrolyte-diaphragm-20μL electrolyte-polymer matrix composite silicon carbon negative electrode material-positive electrode shell. The electrolyte is lithium hexafluorophosphate (LiPF6, 1mol / L)-ethylene carbonate (EC) / dimethyl carbonate (DMC). The electrolyte is a mixture of 1mol / L LiPF6 solution, EC and DMC in a volume ratio of 2:1:1; the diaphragm uses Celgard-2400 polypropylene diaphragm. The electrochemical properties of the materials were tested within the voltage window of 0.01~3V.

[0019] Figure 1 The long cycle performance diagram of the polymer matrix composite silicon-based lithium-ion battery negative electrode material prepared in this embodiment shows that the battery has a good cycle life at 1 A g -1 The material specific capacity can be maintained at 650 mAhg after 1000 cycles at a current density of -1 , the capacity retention rate is 108.6%.

[0020] Example 2 In this embodiment, the polymer matrix composite silicon-based lithium ion battery negative electrode material is prepared according to the following steps: (a) Precursor synthesis 100 mg of commercial nano-silicon oxide, 98 mg of artificial graphite and 2 mg of polyethylene oxide were added to 100 ml of ethanol-water solution and stirred for 1.5 h, wherein the volume ratio of ethanol to water was 3:1. Then, the mixture was heated and stirred at 75°C for 4 h and evaporated to dryness to obtain the precursor.

[0021] (b) High temperature treatment Under Ar atmosphere, the temperature was first increased to 350°C at a heating rate of 5°C / min, and calcined at a constant temperature of 350°C for 240 min; then the temperature was increased to 1000°C at a heating rate of 5°C / min, and calcined at a constant temperature for 180 min; and then cooled to room temperature, and the obtained black powder was the polymer matrix composite silicon-based lithium-ion battery negative electrode material.

[0022] Example 3 In this example, a polymer matrix composite silicon-based lithium-ion battery negative electrode material is prepared, and the experimental steps are as follows: (a) Precursor synthesis 198 mg of commercial nano-silicon powder and 2 mg of polyethylene oxide were weighed and added to 100 ml of ethanol-water solution for ultrasonic dispersion for 1.5 h, where the volume ratio of ethanol to water was 3:1. The precursor was then evaporated to dryness by heating and stirring at 75°C for 4 h.

[0023] (b) High temperature treatment Under Ar atmosphere, the temperature was first increased to 350°C at a heating rate of 5°C / min and calcined at a constant temperature for 240 min; then the temperature was increased to 1000°C at a heating rate of 5°C / min and calcined at a constant temperature for 180 min; and then cooled to room temperature. The resulting black powder was a polymer matrix composite silicon-based lithium-ion battery negative electrode material.

[0024] Example 4 In this example, a polymer matrix composite silicon-based lithium-ion battery negative electrode material is prepared, and the experimental steps are as follows: (a) Precursor synthesis 198 mg of commercial nano-silicon oxide and 2 mg of polyethylene oxide were weighed and added to 100 ml of ethanol aqueous solution for ultrasonic dispersion for 1.5 h, where the volume ratio of ethanol to water was 3:1. The precursor was then evaporated to dryness by heating and stirring at 75°C for 4 h.

[0025] (b) High temperature treatment Under Ar atmosphere, the temperature was first increased to 350°C at a heating rate of 5°C / min and calcined at a constant temperature for 240 minutes; then the temperature was increased to 1000°C at a heating rate of 5°C / min and calcined at a constant temperature for 180 minutes; and then cooled to room temperature. The obtained black powder is a polymer matrix composite silicon-based lithium-ion battery negative electrode material.

[0026] The present invention does not elaborate on some of the common technologies of those skilled in the art. The above-described embodiments are only descriptions of preferred implementations of the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementations described. Without departing from the design spirit of the present invention, various modifications and improvements made by ordinary technicians in this field to the technical solution of the present invention should fall within the scope of protection determined by the claims of the present invention.

Claims

1. A method for preparing a polymer matrix composite silicon-based lithium ion battery negative electrode material, characterized in that: The steps include: Step 1: Precursor synthesis Dissolving graphite and polyethylene oxide in a solvent at a mass ratio of 50:(0.1-1), stirring and mixing, and then heating and evaporating to obtain a dry dispersion, and then mixing the dry dispersion with silicon or silicon oxide to obtain a precursor, wherein the mass ratio of graphite to silicon or silicon oxide is (1-5):1; Step 2: High temperature treatment The precursor prepared in step 1 is placed in a corundum calcining boat and treated at high temperature to obtain a polymer matrix composite silicon-based lithium ion battery negative electrode material.

2. The method for preparing a polymer matrix composite silicon-based lithium ion battery negative electrode material according to claim 1, characterized in that: In step 1, the average molecular weight of the polyethylene oxide is 500,000-900,000.

3. The method for preparing a polymer matrix composite silicon-based lithium ion battery negative electrode material according to claim 1, characterized in that: In step 1, the solvent is an ethanol-water solution, wherein the volume ratio of ethanol to water is 3:

1.

4. The method for preparing a polymer matrix composite silicon-based lithium ion battery negative electrode material according to claim 1, characterized in that: In step 1, the dried dispersion is polyethylene oxide-coated graphite, and the silicon is nano silicon powder.

5. The method for preparing a polymer matrix composite silicon-based lithium ion battery negative electrode material according to claim 1, characterized in that: In step 1, the heating temperature is 60-80° C. and the heating time is 1-6 hours.

6. The method for preparing a polymer matrix composite silicon-based lithium ion battery negative electrode material according to claim 1, characterized in that: In step 2, the high temperature treatment atmosphere is high purity argon or high purity nitrogen.

7. The method for preparing a polymer matrix composite silicon-based lithium ion battery negative electrode material according to claim 1, characterized in that: In step 2, the high temperature treatment temperature is 700-1000° C., and the high temperature treatment time is 1-7 hours.

8. The method for preparing a polymer matrix composite silicon-based lithium ion battery negative electrode material according to claim 1, characterized in that: In step 2, the high temperature treatment heating rate is 1-10 °C / min.

9. A polymer matrix composite silicon-based lithium ion battery negative electrode material prepared by the preparation method according to any one of claims 1 to 8.

Citation Information

Cited By

  • Battery slurry suitable for high-specific-surface-area three-dimensional composite silicon negative electrode material, battery pole piece and preparation method of battery pole piece

    CN121172110A