Non-aqueous electrolyte and lithium ion battery containing same
By using carboxylate and cyano structural additives in non-aqueous electrolytes in lithium-ion batteries, the performance problems of lithium-ion batteries in high-temperature cycles and high-rate scenarios are solved, and the stability of SEI and the overall battery are improved. performance.
Patent Information
- Application Number
- CN202410997552.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-11
AI Technical Summary
Lithium-ion batteries have problems with uneven surface thickness of SEI and CEI films and low lithium ion conductivity under high-temperature cycling and high-rate discharge scenarios, which affects their performance.
Using a non-aqueous electrolyte, containing additive compounds with carboxylate and cyano structures, the electropolymerization of the negative electrode generates carboxylate lithium salts and cyano groups, which work synergistically to reduce SEI impedance and improve the high-temperature cycle and rate performance of lithium-ion batteries. .
By improving the stability and density of SEI, reducing the contact points between the electrolyte and the positive electrode, inhibiting the decomposition of the electrolyte, and significantly improving the high-temperature cycle performance and rate discharge performance of lithium-ion batteries.
Smart Images

Figure CN118763280A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a non-aqueous electrolyte and a lithium ion battery containing the non-aqueous electrolyte. Background Art
[0002] Lithium-ion batteries have the characteristics of wide operating temperature range, high voltage, no memory effect and long cycle life, and are widely used in daily electronic devices. In recent years, with the continuous expansion of lithium-ion battery application scenarios, the performance of lithium-ion batteries under extreme conditions such as high-temperature cycling and high-rate discharge scenarios needs to be continuously improved to meet the use of these scenarios.
[0003] As we all know, lithium-ion battery electrolyte is the key medium for lithium ions to move and deintercalate between the positive and negative electrodes. The type and content of additives are of great significance to the formation and quality of SEI and CEI films. In this regard, scientific research staff have also proposed many practical and effective film-forming additives, but there are still problems such as uneven surface thickness of SEI and CEI films, high-temperature cycle performance and low conductivity of SEI to lithium ions.
[0004] Therefore, a non-aqueous electrolyte and a lithium ion battery containing the non-aqueous electrolyte are urgently needed to solve the above problems. Summary of the invention
[0005] The object of the present invention is to provide a non-aqueous electrolyte and a lithium ion battery comprising the non-aqueous electrolyte. The non-aqueous electrolyte comprises an additive compound having a carboxylate group and a cyano group structure. The non-aqueous electrolyte comprising the additive compound is applied to a lithium ion battery, and the carboxylate lithium salt and the cyano group generated by negative electrode electropolymerization act synergistically to reduce SEI impedance and improve the high temperature cycle performance and rate performance of the lithium ion battery.
[0006] To achieve the above object, the present invention provides a non-aqueous electrolyte, including a lithium salt, a non-aqueous organic solvent and an additive, wherein the additive includes at least one of Formula 1 and Formula 2:
[0007]
[0008] Wherein, R1, R2, R3 are each independently selected from hydrogen, hydroxyl, ether, trialkylsilyloxy, ester, amide, fluoroalkoxy, substituted or unsubstituted C1-C12 alkyl, and n is a natural number of 0-5. Specifically, the C1-C12 alkyl of the present invention refers to a straight or branched saturated hydrocarbon group containing 1 to 12 carbon atoms, and these groups can be methyl (CH3-), ethyl (CH3CH2-), propyl (CH3CH2CH2-), butyl (which can be CH3CH2CH2CH2- or CH3CH(CH3)CH2-, etc.). Substituted C1-C12 alkyl refers to one or more hydrogen atoms in these alkyl groups replaced by other atoms or groups (referred to as substituents), and the substituents can be halogens (such as fluorine, chlorine, bromine, iodine), hydroxyl, amino, nitro, alkoxy or aryl; for example, a methyl group can be substituted by a chlorine atom to form a chloromethyl group (-CH2Cl) or by a hydroxyl group to form a hydroxymethyl group (-CH2OH). An unsubstituted C1-C12 alkyl group refers to an alkyl group in which no hydrogen atom is replaced by other atoms or groups.
[0009] Compared with the prior art, the non-aqueous electrolyte of the present invention includes a lithium salt, a non-aqueous organic solvent and an additive, wherein the additive includes a compound containing a carboxylate group and a cyano structure as shown in Formula 1 or Formula 2, and the polar group cyano and the carboxylate functional group are combined. The SEI formed by the carboxylate is rich in inorganic components such as carboxylate lithium, which can improve the organic components of the SEI, make the SEI more stable and dense, and prevent the electrolyte from reacting with the negative electrode. At the same time, due to the presence of the cyano polar functional group, the solubility of the lithium salt can be improved. Further, based on the strong complexing ability of the cyano group, the metal (such as nickel, cobalt, manganese, etc.) ions generated by the electrolyte in the high temperature cycle can be captured, and the contact sites between the electrolyte and the positive electrode can be reduced, thereby inhibiting the decomposition of the electrolyte, and then improving the high temperature cycle performance of the battery. Therefore, the additive is used in the non-aqueous electrolyte of the lithium ion battery, which can improve the high temperature cycle performance and rate discharge performance of the lithium ion battery.
[0010] As a preferred technical solution, R1 is selected from hydrogen, substituted or unsubstituted C1-C6 alkyl, R2 and R3 are each independently selected from trimethylsilyloxy, substituted or unsubstituted C1-C6 alkyl, and n is a natural number of 0-3.
[0011] As a preferred technical solution, R1 is selected from hydrogen or unsubstituted C1-C6 alkyl, and at least one of R2 and R3 is halogen-substituted C1-C3 alkyl, unsubstituted C1-C3 alkyl or trimethylsilyloxy.
[0012] As a preferred technical solution, the compound with the structure shown in Formula 1 is selected from at least one of Compounds 1 to 5:
[0013]
[0014] The preparation of compound 4 may include: reacting raw material trifluoroacetyl ester (CAS: 372-31-6) and raw material trimethylsilyl cyanide (CAS: 7677-24-9) under heating conditions at 110° C. to generate a crude product compound 4, and then performing reduced pressure distillation to obtain compound 4 with a purity of 99.9%, a brown-red liquid, NMR 1 H (400MHz,CDCl3):4.12(q,2H);2.73(s,2H);1.30(t,3H);0.08(s,12H), the preparation route can be shown as follows:
[0015]
[0016] As a preferred technical solution, the mass percentage of the additive in the non-aqueous electrolyte is 0.05% to 5%. Preferably, the mass percentage of the additive in the non-aqueous electrolyte is 0.05% to 4%, and more preferably, the mass percentage of the additive in the non-aqueous electrolyte is 0.1% to 2%. As an example, the mass percentage of the additive in the non-aqueous electrolyte is 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0017] As a preferred technical solution, the lithium salt is selected from at least one of lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium trifluoromethanesulfonate (LiCF3SO3), bistrifluoromethanesulfonyl lithium (LiTFSI), lithium bisoxalate borate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium trifluoromethanesulfonate (LiSO3CF3), lithium bisoxalate borate (LiBOB), lithium difluorooxalate borate (LiDFOB), lower aliphatic carboxylic acid lithium, lithium difluorobisoxalate phosphate (LiDFBP) and lithium bisfluorosulfonyl imide (LiFSI). Further, lower aliphatic carboxylic acid lithium includes but is not limited to lithium chloroborane, lithium tetraphenylborate, lithium imide salts, etc. As an example, the lithium salt is lithium hexafluorophosphate (LiPF6), but is not limited thereto. Furthermore, the lithium salt is a mixture of lithium hexafluorophosphate (LiPF6) and lithium bis(oxalatoborate) (LiBOB), but is not limited thereto.
[0018] As a preferred technical solution, the mass percentage of the lithium salt in the non-aqueous electrolyte is 5-25%. Further, the mass percentage of the lithium salt in the non-aqueous electrolyte is 8-20%. More preferably, the mass percentage of the lithium salt in the non-aqueous electrolyte is 10-15%. By way of example, the mass percentage of the lithium salt in the non-aqueous electrolyte may be but is not limited to 5%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 20%, 25%, but is not limited to the listed values, and other values not listed within the numerical range are equally applicable.
[0019] As a preferred technical solution, the non-aqueous organic solvent is selected from γ-butyrolactone (GBL), γ-valerolactone (GVL), δ-valerolactone (DVL), methyl acetate (MA), ethyl acetate (EA), ethyl propionate (EP), butyl acetate (BAC), propyl propionate (PP), butyl propionate (PRB), ethylene carbonate (EC), propylene carbonate (PCA), butylene carbonate (BC), vinylene carbonate (VEC), dimethyl carbonate (DMC), diethyl carbonate (DEC), At least one of ethyl methyl carbonate (EMC), propylene carbonate (PC), 1,3-dioxolane (DOL), 1,4-dioxolane (DX), crown ether, tetrahydrofuran (THF), 2-methyltetrahydrofuran (2-CH3-THF), 2-trifluoromethyltetrahydrofuran (2-CF3-THF), dimethoxymethane (DMM), diethoxymethane (DEM), ethoxymethoxymethane (DCE), ethylene glycol di-n-butyl ether (EDB) and diethylene glycol dimethyl ether (DEGME).
[0020] As a preferred technical solution, the mass percentage of the non-aqueous organic solvent in the non-aqueous electrolyte is 65-90%, preferably, the mass percentage of the non-aqueous organic solvent in the non-aqueous electrolyte is 75-89%, and more preferably, the mass percentage of the non-aqueous organic solvent in the non-aqueous electrolyte is 78-88%. As an example, the mass percentage of the non-aqueous organic solvent in the non-aqueous electrolyte can be, but is not limited to, 65%, 70%, 80%, 85%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 90%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0021] As a preferred technical solution, the non-aqueous electrolyte of the present invention also includes an auxiliary agent, which is selected from at least one of fluoroethylene carbonate (FEC), vinyl sulfite (ES), 1,3-propane sultone (PS), 1,3-propene sultone (PST), 1,4-butane sultone (1,4-BS), vinyl sulfate (DTD) and succinic anhydride (SA).
[0022] As a preferred technical solution, the mass percentage of the auxiliary agent in the non-aqueous electrolyte is 0.05-5%. By way of example, the mass percentage of the auxiliary agent in the non-aqueous electrolyte can be, but is not limited to, 0.05%, 0.1%, 0.2%, 0.4%, 0.6%, 0.8%, 1.0%, 1.5%, 2.0%, 3.0%, 4.0%, 4.5%, 5.0%.
[0023] On the other hand, the present invention provides a lithium ion battery, which includes a positive electrode material, a negative electrode material and the above-mentioned non-aqueous electrolyte.
[0024] As a preferred technical solution, the positive electrode material is selected from at least one of nickel cobalt manganese oxide, lithium cobaltate and nickel cobalt aluminum oxide. Specifically, the positive electrode material can be nickel cobalt manganese oxide, and its chemical formula can be LiNi8Co1Mn1O2, LiNi5Co2Mn3O2, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 or LiNi x Co y Mn z M (1xyz) O2; for another example, the positive electrode material can be nickel cobalt aluminum oxide, and its chemical formula can be LiNi x Co y Al z N (1xyz) O2, where M and N are each independently selected from at least one of Mg, Cu, Zn, Al, Sn, B, Ga, Cr, Sr, V and Ti, 0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z ≤ 1; for another example, the positive electrode material is lithium cobaltate, and its chemical formula is LiCoO2.
[0025] As a preferred technical solution, the negative electrode material is selected from at least one of artificial graphite, natural graphite, lithium titanate, silicon-carbon composite material and silicon monoxide. By way of example, the negative electrode material is artificial graphite, but is not limited thereto. Detailed implementation manners
[0026] To better illustrate the purpose, technical solution and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation methods are further explanatory descriptions of the present invention and should not be regarded as limitations on the present invention.
[0027] Example 1
[0028] (1) Prepare non-aqueous electrolyte
[0029] In a glove box filled with argon (O2 <1ppm, H2O <1ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) were mixed in a weight ratio of EC:EMC:DEC=3:5:2 to obtain 85g of a non-aqueous organic solvent, and then 0.5g of compound 1 was added as an additive, dissolved and stirred thoroughly, and then 14.5g of lithium hexafluorophosphate was added and mixed evenly to obtain a non-aqueous electrolyte.
[0030] (2) Preparation of positive electrode
[0031] NCM811, adhesive PVDF and conductive agent SuperP were mixed evenly in a mass ratio of 95:1:4 to prepare a positive electrode slurry for a lithium-ion battery with a certain viscosity. The mixed slurry was coated on both sides of an aluminum foil, and then dried and rolled to obtain a positive electrode sheet.
[0032] (3) Preparation of negative electrode
[0033] Artificial graphite, conductive agent SuperP, thickener CMC, and adhesive SBR (styrene-butadiene rubber latex) are made into slurry in a mass ratio of 95:1.5:1.0:2.5, mixed evenly, coated on both sides of copper foil with the mixed slurry, and then dried and rolled to obtain a negative electrode sheet.
[0034] (4) Preparation of lithium-ion batteries
[0035] The positive electrode, the separator and the negative electrode are wound into a soft-pack battery cell, which is packaged with a polymer aluminum-plastic film and filled with the prepared lithium-ion battery non-aqueous electrolyte. After the processes of formation and capacity separation, a lithium-ion battery with a capacity of 1000 mAh is manufactured.
[0036] The formulations of the non-aqueous electrolytes of Examples 1-20 and Comparative Examples 1-4 are shown in Table 1, wherein the steps of preparing the electrolytes and preparing the batteries of Examples 2-20 and Comparative Examples 1-4 are the same as those of Example 1.
[0037] Table 1 Formula of non-aqueous electrolyte
[0038]
[0039]
[0040] The lithium ion batteries prepared in Examples 1 to 20 and Comparative Examples 1 to 4 were subjected to high temperature cycle tests and rate discharge performance tests, respectively. The specific test conditions are as follows. The performance test results are shown in Table 2.
[0041] Lithium-ion battery room temperature rate discharge performance test
[0042] At room temperature (25°C), the lithium-ion battery was fully charged at 0.2C (the battery charging capacity was recorded as C0), and then the charge and discharge tests were performed at 0.2C / 0.2C, 0.2C / 0.5C, 0.2C / 1C, 0.2C / 2C, 0.2C / 3C, and 0.2C / 5C, respectively. The different discharge rate stages were cycled 5 times, and then the above six stages were repeated for two large cycles. After the cycle was completed, the capacity-voltage curve was recorded (the battery discharge capacity was recorded as C1). After the cycle was completed, the capacity retention rate and capacity recovery rate of the lithium-ion battery were calculated using the following formula:
[0043] Capacity retention rate = (C1 / C0) · 100%
[0044] Lithium-ion battery high temperature cycle performance test
[0045] Place the lithium-ion battery in a 45℃ constant temperature box and let it stand for 30 minutes to make the lithium-ion battery reach a constant temperature. Charge it at a constant current of 1C to a voltage of 4.50V, then charge it at a constant voltage of 4.50V to a current of 0.05C, and then discharge it at a constant current of 1C to a voltage of 3.0V. Record the first discharge capacity of the battery as C0, which is a charge and discharge cycle. Then charge and discharge at 1C / 1C for 300 cycles at 45℃, record the discharge capacity as C1, and use the following formula to calculate the capacity retention rate of the lithium-ion battery.
[0046] Capacity retention rate = (C1 / C0) · 100%
[0047] Cyclic internal resistance growth rate test
[0048] Internal resistance growth rate after 300 cycles of high-temperature cycling: At 45°C, the divided battery is charged at 0.5C constant current and constant voltage at room temperature to a cut-off voltage of 4.2V, and then discharged at constant current and constant voltage until the capacity drops to 50% SOC, the internal resistance of the battery is tested, and then charged to 4.2V at 1C constant current. After 300 cycles, the internal resistance of the battery at the first full charge and the internal resistance of the battery after the last full charge are recorded.
[0049] The internal resistance growth rate of the battery after 300 cycles of high-temperature cycling = (the internal resistance of the battery after the last full charge - the internal resistance of the battery after the first full charge) / the internal resistance of the battery after the first full charge × 100%.
[0050] Table 2 Lithium-ion battery performance test results
[0051]
[0052]
[0053] Specifically, as shown in Table 2, by comparing the performance data of Examples 1 to 20 with the performance data of Comparative Examples 1 to 4, it can be seen that the lithium ion batteries of Examples 1 to 20 have good high-temperature cycle performance, rate discharge performance and lower internal resistance growth rate. This may be because the additive of the present invention is a compound comprising a carboxylate group and a cyano structure, and the polar group cyano and the carboxylate functional group are combined. The SEI formed by the carboxylate is rich in inorganic components such as carboxylate lithium, which can improve the organic components of the SEI, make the SEI more stable and dense, and prevent the electrolyte from reacting with the negative electrode. At the same time, due to the presence of the cyano polar functional group, the solubility of the lithium salt is improved. Furthermore, based on the strong complexing ability of the cyano group, the nickel, cobalt and manganese ions generated by the non-aqueous electrolyte of the present invention during high-temperature cycling can be captured, and the contact sites between the non-aqueous electrolyte and the positive electrode are reduced, thereby inhibiting the decomposition of the non-aqueous electrolyte, and then improving the high-temperature cycle performance of the battery.
[0054] By comparing Examples 1 to 6 with each other and Examples 13 to 20 with each other, it can be seen that Compound 3 and Compound 4 of the present invention have more excellent high-temperature cycle performance and rate performance. This may be because: Compound 3 and Compound 4 also have a trimethylsilyl structure compared to other compounds. The siloxane structure can combine with acidic substances such as HF generated in the non-aqueous electrolyte to form a Si-F-containing component, which improves the film quality and enhances the stability of the solid electrolyte interface film, while reducing the reaction probability of HF on the SEI film components, providing a better lithium ion transmission channel, thereby improving the high-temperature cycle and rate performance. By comparing the performance data of compound 3 and compound 4, it can be seen that the high temperature cycle performance and rate performance of compound 4 are better. The inventor speculates that this may be because compared with compound 3, compound 4 also contains a trifluoroalkyl structure. This may be because the fluorine atoms contained in the trifluoroalkyl structure can reduce the HOMO and LUMO energy levels of the molecule and enhance the antioxidant property, but are more easily reduced at the negative electrode to generate LiF inorganic components, which improves and enhances the content of inorganic components in the SEI film, making the SEI film denser, preventing the side reaction between the electrolyte and the negative electrode, and thus improving the high temperature cycle and rate performance.
[0055] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A non-aqueous electrolyte comprising a lithium salt, a non-aqueous organic solvent and an additive, characterized in that: The additive comprises at least one of Formula 1 and Formula 2: Wherein, R1, R2, and R3 are each independently selected from hydrogen, hydroxyl, ether, trialkylsilyl, ester, amide, fluoroalkoxy, substituted or unsubstituted C1-C12 alkyl, and n is a natural number of 0-5.
2. The non-aqueous electrolyte according to claim 1, characterized in that R1 is selected from hydrogen, substituted or unsubstituted C1-C6 alkyl, R2 and R3 are each independently selected from trimethylsilyloxy, substituted or unsubstituted C1-C6 alkyl, and n is a natural number of 0-3.
3. The non-aqueous electrolyte according to claim 1, characterized in that The compound of the structure shown in Formula 1 is selected from at least one of Compounds 1 to 5:
4. The non-aqueous electrolyte according to claim 1, characterized in that The mass percentage of the additive in the non-aqueous electrolyte is 0.05% to 5%.
5. The non-aqueous electrolyte according to claim 1, characterized in that The lithium salt is selected from at least one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium trifluoromethanesulfonate, lithium bistrifluoromethanesulfonyl imide, lithium bisoxalatoborate, lithium difluorophosphate, lithium trifluoromethanesulfonate, lithium bisoxalatoborate, lithium difluorooxalatoborate, lithium lower aliphatic carboxylate, lithium difluorobisoxalatophosphate and lithium bisfluorosulfonyl imide.
6. The non-aqueous electrolyte according to claim 1, characterized in that The non-aqueous organic solvent is selected from at least one of γ-butyrolactone, γ-valerolactone, δ-valerolactone, methyl acetate, ethyl acetate, ethyl propionate, butyl acetate, propyl propionate, butyl propionate, ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, propylene carbonate, 1,3-dioxolane, 1,4-dioxane, crown ether, tetrahydrofuran, 2-methyltetrahydrofuran, 2-trifluoromethyltetrahydrofuran, dimethoxymethane, diethoxymethane, ethoxymethoxymethane, ethylene glycol di-n-butyl ether and diethylene glycol dimethyl ether.
7. The non-aqueous electrolyte according to claim 1, characterized in that The invention also comprises an auxiliary agent, which is selected from at least one of fluoroethylene carbonate, vinyl sulfite, 1,3-propane sultone, 1,3-propylene sultone, 1,4-butane sultone, vinyl sulfate and succinic anhydride.
8. A lithium-ion battery comprising a positive electrode material and a negative electrode material, characterized in that: It also includes the non-aqueous electrolyte according to any one of claims 1 to 7.
9. The lithium-ion battery according to claim 8, characterized in that: The positive electrode material is selected from at least one of nickel cobalt manganese oxide, nickel cobalt aluminum oxide and lithium cobalt oxide.
10. The lithium ion battery according to claim 8, characterized in that The negative electrode material is selected from at least one of artificial graphite, natural graphite, lithium titanate, silicon-carbon composite material and silicon monoxide.
Citation Information
Cited By
Non-aqueous electrolyte solution and lithium secondary battery
CN119920977A