Electrolyte and lithium ion battery containing same
By using fluorinated solvents of fluorinated cyclic carbonates and fluorinated carboxylates in lithium-ion batteries, combined with diluents and film-forming additives, the problem of poor stability of traditional batteries at high voltages and high rates is solved and achieved The high voltage resistance and fast charging performance of lithium batteries improve the overall performance of the battery and are suitable for electric vehicle applications.
Patent Information
- Application Number
- CN202411045156.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional lithium-ion batteries have problems such as poor anode stability, unstable interface layer, and reduced battery capacity under high voltage and high rate conditions. The existing high-voltage electrolyte design still has flaws and is difficult to meet the application needs of electric vehicles.
A fluorinated solvent containing fluorinated cyclic carbonate and fluorinated carboxylic acid ester is used as the organic solvent of the electrolyte, combined with a diluent and a film-forming additive, to improve the oxidation potential and interface of the electrolyte through the strong electron-withdrawing property of fluorine atoms layer mechanical properties, regulate the solvation structure of lithium ions, and enhance the high voltage resistance and fast charging performance of the battery.
It achieves the high voltage resistance and fast charging performance of lithium batteries under high voltage and high rate conditions, extends the cycle life of the battery, improves the overall performance of the battery, and solves the "range anxiety" and "charging anxiety" problems of electric vehicles. .
Smart Images

Figure CN118763286A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to an electrolyte and a lithium ion battery containing the electrolyte. Background Art
[0002] Lithium metal ternary cathode battery is an important high-energy battery system, and its development is of great significance to the further development of electric vehicles. However, with the increase of nickel content in high-nickel ternary materials, although the specific capacity of the material is significantly improved, it is still difficult to achieve good performance at high voltage (≥4.5V vs Li / Li + ) and high rate (≥4C) have many serious problems that restrict the application and development of this battery system.
[0003] The conventional commercial electrolyte is mainly composed of carbonate solvent, which has poor compatibility with lithium metal. + The anode stability is less than 4.3V. At the same time, the high catalytic activity of carbonate organic molecules in nickel-rich cathode materials causes redox decomposition during the charge and discharge process to form a solid electrolyte interlayer (SEI / CEI) of polycarbonate substances. This type of SEI / CEI rich in organic polycarbonates is still not stable enough under high voltage and high current, resulting in excessive oxidation of the electrolyte and continuous deterioration of the interface, forming a thicker organic-rich interface layer that affects lithium ion transmission, while the battery capacity continues to decrease. Therefore, under high-rate conditions, traditional carbonate electrolytes are difficult to desolvate at the battery negative electrode interface, and the highly polarized interface formed leads to a decrease in battery capacity or growth of lithium diameter.
[0004] The existing design strategy for high-voltage resistant electrolytes is mainly to design new organic solvents, including sulfone solvents, nitrile solvents, etc., but the high-voltage resistant electrolytes obtained by solvent improvement still have certain defects.
[0005] For example, the current mainstream electrolyte solvents use ether / ester mixed solvents or mixed ester solvents. Ether substances have good compatibility with lithium negative electrodes, high ionic conductivity, and low viscosity, but their low oxidation potential causes them to decompose under high pressure or continuous oxidation;
[0006] Sulfone and nitrile solvents have high antioxidant stability, but they have disadvantages such as poor wettability and inability to form a stable SEI on the negative electrode surface;
[0007] Phosphate solvents are flame retardant and non-flammable, but their high viscosity and incompatibility with the negative electrode result in a significant decrease in their cycle life and battery capacity;
[0008] Carboxylate solvents have good ion conductivity, low viscosity and high solubility, but carboxylate electrolytes are highly polar and have strong activity towards lithium, resulting in poor cycling performance of lithium electrodes.
[0009] Therefore, it is necessary and urgent to research and develop a new type of electrolyte with high voltage resistance and high rate performance.
[0010] In view of this, the present invention is proposed. Summary of the invention
[0011] The purpose of the present invention is to provide an electrolyte which has the performance of high voltage resistance and high rate resistance, while also taking into account film-forming properties. It has the application prospect of high-voltage fast-charging electrolyte and is expected to solve the "range anxiety" and "charging anxiety" of electric vehicles.
[0012] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0013] The present invention provides an electrolyte, which comprises: an electrolyte salt, an organic solvent and a diluent, wherein:
[0014] The organic solvent is a fluorinated solvent, and the fluorinated solvent comprises a fluorinated cyclic carbonate and a fluorinated carboxylic acid ester.
[0015] Further, the electrolyte salt is a lithium salt;
[0016] Preferably, the lithium salt includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorooxalatophosphate, lithium trifluoromethanesulfonate, lithium hexafluoroarsenate, lithium nitrate, and lithium perchlorate.
[0017] Furthermore, the molar concentration of the electrolyte salt in the electrolyte is 0.1 to 5.0M.
[0018] Furthermore, the diluent includes at least one of fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, 1,3,4-trifluorobenzene, 1,3,5-trifluorobenzene, 1,2,3,4-tetrafluorobenzene, 1,2,3,5-tetrafluorobenzene, 1,2,4,5-tetrafluorobenzene, 1,2,3,4,5-pentafluorobenzene and hexafluorobenzene.
[0019] Furthermore, the volume ratio of the fluorinated cyclic carbonate, the fluorinated carboxylic acid ester and the diluent in the electrolyte is 1:(0.1-10):(0.1-10).
[0020] Furthermore, the electrolyte also includes a film-forming additive;
[0021] The film-forming additive includes at least one of vinylene carbonate, lithium difluorooxalatoborate, lithium nitrate, 1,3-propanesulfonate, lithium difluorophosphate, vinyl sulfate, and vinyl sulfite.
[0022] Furthermore, the mass fraction of the film-forming additive in the electrolyte is 0 to 5.0 wt %.
[0023] The present invention provides an application of the above electrolyte in the preparation of lithium ion batteries.
[0024] The present invention provides a lithium ion battery, which comprises the above-mentioned electrolyte.
[0025] Furthermore, the lithium-ion battery is a high-nickel ternary lithium-ion battery, and the positive electrode material of the high-nickel ternary lithium-ion battery includes LiNi (0.8~0.9) Co (0.05~0.15) Mn (0.05~0.15) O2.
[0026] Furthermore, the voltage of the lithium-ion battery is 3.0-4.7V, and the rate is 0.2-5C.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] The electrolyte provided by the present invention includes an electrolyte salt, an organic solvent and a diluent, wherein the organic solvent is a fluorinated solvent comprising a fluorinated cyclic carbonate and a fluorinated carboxylate. The electrolyte of the present invention utilizes a fluorinated solvent comprising a fluorinated cyclic carbonate and a fluorinated carboxylate to dissolve the electrolyte salt, and through the strong electron-withdrawing property of fluorine atoms, the HOMO (Highest Occupied Molecular Orbital, the highest occupied molecular orbital) energy level of the solvent is reduced, the oxidation potential is increased, and the electrolyte anode stability performance is improved; at the same time, the fluorinated solvent produces an interface layer rich in LiF after oxidation and decomposition, which can enhance the mechanical properties of the interface layer, so that the lithium metal battery has high voltage resistance. In addition, the present invention utilizes the strong electron-withdrawing property of fluorine atoms to fluorinate and modify the cyclic carbonate and carboxylate solvent molecules, regulate the solvation structure of lithium ions, and then also promote the transmission of lithium ions in the electrolyte liquid phase and the interface layer, so that the lithium battery has fast charging performance.
[0029] The electrolyte provided in the present application can be widely used in the preparation process of lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1A leakage current data diagram of the Li||NCM811 battery assembled in Examples 1 to 3 and Comparative Example 1 provided by the present invention during 4.7V constant voltage charging;
[0032] Figure 2 The rate performance data graph of Li||NCM811 batteries assembled in Examples 1 to 3 and Comparative Example 1 provided by the present invention at 0.2C, 0.5C, 1C, 2C, 3C, 4C, 5C, 0.5C, and 1C;
[0033] Figure 3 A graph showing the lithium ion diffusion coefficient of the Li||Li battery assembled in Example 1 and Comparative Example 1 provided by the present invention;
[0034] Figure 4 A graph showing the lithium ion diffusion coefficient of the Li||Li battery assembled in Example 2 provided by the present invention;
[0035] Figure 5 A graph showing the lithium ion diffusion coefficient of the Li||Li battery assembled in Example 3 provided by the present invention;
[0036] Figure 6 A graph showing the lithium ion diffusion coefficient of the Li||Li battery assembled in Comparative Example 1 provided by the present invention;
[0037] Figure 7 The coulombic efficiency diagram of the Li||Cu battery assembled in Examples 1 to 3 and Comparative Example 1 provided by the present invention. DETAILED DESCRIPTION
[0038] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] According to one aspect of the present invention, an electrolyte solution comprises: an electrolyte salt, an organic solvent and a diluent, wherein:
[0040] The organic solvent is a fluorinated solvent, and the fluorinated solvent comprises a fluorinated cyclic carbonate and a fluorinated carboxylic acid ester.
[0041] The electrolyte provided by the present invention includes an electrolyte salt, an organic solvent and a diluent, wherein: the organic solvent includes a fluorinated solvent of a fluorinated cyclic carbonate and a fluorinated carboxylic acid ester. The electrolyte of the present invention utilizes a fluorinated solvent including a fluorinated cyclic carbonate and a fluorinated carboxylic acid ester to dissolve the electrolyte salt, and through the strong electron-withdrawing property of the fluorine atom, the HOMO energy level of the solvent is effectively reduced, the oxidation potential is increased, and the anode stability of the electrolyte is improved; at the same time, the fluorinated solvent produces a LiF-rich interface layer after oxidation and decomposition, which can enhance the mechanical properties of the interface layer and enable the lithium metal battery to have high-voltage resistance. In addition, the present invention utilizes the strong electron-withdrawing property of fluorine atoms to fluorinate and modify the cyclic carbonate and carboxylic acid ester solvent molecules, regulate the solvation structure of lithium ions, and further promote the transmission of lithium ions in the electrolyte liquid phase and the interface layer, so that the lithium battery has fast charging performance.
[0042] It should be noted that the rate is inversely proportional to the charging time. For example, the charging time is 1h for 1C current charging and 1 / 5h, or 12min for 5C current charging. The higher the rate, the shorter the charging time. But at the same time, the capacity will be reduced. The fast charging performance of the lithium battery in this application refers to the fast charging performance at high voltage (≥4.5V vs Li / Li + ) and high rate (≥4C) conditions, high nickel ternary material lithium-ion batteries can be fully charged to 80% within 15 minutes.
[0043] It should be noted that the present invention aims to solve the problem that carbonate and carboxylate solvent molecules have poor stability under high pressure, are easy to decompose, and form a poor quality solid electrolyte interface film on the electrode surface. It proposes to introduce fluorine atoms to modify the solvent molecules so that they have excellent film-forming properties and enhance the high-pressure resistance of the solvent molecules. The oxygen atom in the carbonyl group (C=O) of carbonate and carboxylate solvents contains a lone pair of electrons, which usually react with Li + When fluorine atoms are introduced near the carbonyl group, the electron cloud density of the carbonyl group will be further reduced due to the strong electron-withdrawing and inductive effects of fluorine, thereby weakening the coordination ability of the carbonyl oxygen and reducing the Li + The energy barrier of the desolvation process promotes Li + Transmission and transfer, thereby improving the rate performance of lithium batteries.
[0044] As a preferred embodiment, the structure of the fluorinated cyclic carbonate is shown in formula (I):
[0045]
[0046] In formula (I), R1 and R2 can be optionally C1-C5 fluorinated fatty chains, or C x ≥3 fluorinated, non-fluorinated fatty chain structures and isomeric structures thereof, at least one of R1 and R2 is a fluorinated structure, wherein the fluorinated structure may be mono-fluorinated, di-fluorinated, poly-fluorinated, or even per-fluorinated.
[0047] As a preferred embodiment, the structure of the fluorinated carboxylic acid ester is shown in formula (II):
[0048]
[0049] In formula (II), R1 and R2 can be optionally C1-C4 fluorinated fatty chains, or C x ≥5 fluorinated, non-fluorinated fatty chain structures and isomeric structures thereof, at least one of R1 and R2 is a fluorinated structure, wherein the fluorinated structure may be mono-fluorinated, di-fluorinated, poly-fluorinated, or even per-fluorinated.
[0050] In a preferred embodiment of the present invention, the electrolyte salt is a lithium salt;
[0051] Preferably, the lithium salt includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorooxalatophosphate, lithium trifluoromethanesulfonate, lithium hexafluoroarsenate, lithium nitrate, and lithium perchlorate.
[0052] In the above preferred embodiment, the molar concentration of the lithium salt in the electrolyte is 0.1-5.0M.
[0053] As a preferred embodiment, the molar concentration of the lithium salt in the electrolyte is 0.1 to 5.0 M. Above this concentration, the viscosity of the electrolyte increases, resulting in a decrease in the ion migration number, and some lithium salts may have solubility problems at high concentrations, resulting in precipitation or precipitation; below this concentration, the electrolyte ion conductivity decreases, the ion transmission efficiency slows down, affecting the charge and discharge efficiency of the battery, and affecting the capacity and cycle life of the battery.
[0054] In a preferred embodiment of the present invention, the diluent includes at least one of fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, 1,3,4-trifluorobenzene, 1,3,5-trifluorobenzene, 1,2,3,4-tetrafluorobenzene, 1,2,3,5-tetrafluorobenzene, 1,2,4,5-tetrafluorobenzene, 1,2,3,4,5-pentafluorobenzene and hexafluorobenzene.
[0055] As a preferred embodiment, the above-mentioned diluents of the present application are all selected as active diluents with low viscosity, low coordination, low LUMO (Lowest Unoccupied Molecular Orbital), and high fluorine supply characteristics. The main function of the active diluent in the electrolyte is to change the electrolyte solvation structure, promote more anions to participate in the solvation configuration coordination, so that more anions are redox-decomposed during the charge and discharge process to form an inorganic SEI. At the same time, in addition to acting as a diluent, the active diluent also has characteristics that inert diluents do not have, such as low LUMO energy level and high fluorine supply characteristics.
[0056] Specific:
[0057] The low viscosity of the above diluents can reduce the Li + The resistance to movement in the electrolyte makes Li + Migrate faster in the electrolyte, improving rate performance.
[0058] The low coordination of the above diluents determines the difficulty in reacting with Li + Mutually coordinated, unable to enter Li + Solvation sheath, but the diluent can interact with the solvent molecules and "drag" the Li + The coordinated solvent molecules move to the outer solvation layer, allowing more anions to enter the Li + Solvation sheath; when anions enter the solvation sheath, they will be oxidized and reduced on the electrode surface to form a dense and stable SEI / CEI layer, which protects the side reactions of the electrode material and the electrolyte. At the same time, some inorganic components such as LiF and Li3N have high ionic conductivity, which helps lithium ions pass through SEI / CEI, reduce interfacial resistance, and improve battery rate performance.
[0059] In addition, in the electrolyte liquid phase, the low LUMO and high fluorine supply characteristics can enable the active diluent to be preferentially reduced to form a dense SEI / CEI with good mechanical properties, inhibiting further reaction between the solvent and the electrode and improving the battery's oxidation resistance.
[0060] It can be seen from this that the present application prepares the electrolyte by using a fluorinated organic solvent and a highly active diluent, wherein the fluorinated organic solvent and the highly active diluent produce a synergistic effect, the strong electron-withdrawing property of the fluorine atom reduces the HOMO energy level of the solvent and improves the stability of the electrolyte anode; at the same time, the active diluent can regulate the electrolyte solvation structure and interface, and promote the entry of anions into the first solvation sheath. In addition, the two can work together to form a SEI / CEI rich in inorganic substances such as LiF and Li3N during the first charge and discharge process, and realize interface regulation, reduce interface impedance, promote the transmission of lithium ions in the electrolyte liquid phase, the positive and negative electrodes and the electrolyte interface layer, and improve the battery's high voltage resistance and rate performance.
[0061] In a preferred embodiment of the present invention, the volume ratio of the fluorinated cyclic carbonate, the fluorinated carboxylic acid ester and the diluent in the electrolyte is 1:(0.1-10):(0.1-10).
[0062] As a preferred embodiment, the volume ratio of the fluorinated cyclic carbonate, fluorinated carboxylic acid ester and diluent in the electrolyte is as follows. When the volume ratio is lower than this, the fluorinated solvent is less, and the lithium salt may not be dissolved, resulting in precipitation or precipitation, which affects the stability and life of the battery. When the volume ratio is higher than this, the diluent is less, and the solvent and Li + The binding is strong, which affects the desolvation process and its rate performance decreases.
[0063] In a preferred embodiment of the present invention, the electrolyte further comprises a film-forming additive;
[0064] The film-forming additive includes at least one of vinylene carbonate, lithium difluorooxalatoborate, lithium nitrate, 1,3-propanesulfonate, lithium difluorophosphate, vinyl sulfate, and vinyl sulfite.
[0065] In the above preferred embodiment, the mass fraction of the film-forming additive in the electrolyte is 0 to 5.0 wt %.
[0066] According to one aspect of the present invention, the above electrolyte is used in preparing a lithium ion battery.
[0067] The electrolyte provided in the present application can be widely used in the preparation process of lithium-ion batteries.
[0068] It should be noted that the electrolyte of the present invention can be applied to lithium metal, graphite, silicon, and silicon-carbon negative electrodes, can be applied to various types of ternary positive electrodes, lithium cobalt oxide, and lithium iron phosphate positive electrode batteries, and may also be applied to low-temperature batteries, with a usage range of -40 to 60°C.
[0069] According to one aspect of the present invention, a lithium-ion battery comprises the above-mentioned electrolyte.
[0070] Preferably, the lithium-ion battery is a high-nickel ternary lithium-ion battery, and the positive electrode material of the high-nickel ternary lithium-ion battery includes LiNi (0.8~0.9) Co (0.05~0.15) Mn (0.05~0.15) O2.
[0071] In a preferred embodiment of the present invention, the voltage of the lithium ion battery is 3.0-4.7V, and the rate is 0.2-5C.
[0072] The technical solution of the present invention will be further described below in conjunction with embodiments.
[0073] Example 1
[0074] A lithium ion battery electrolyte, wherein the preparation method of the electrolyte comprises:
[0075] (1) In a glove box filled with argon (H2O <1 ppm, O2 <1 ppm), fluoroethylene carbonate (FEC), methyl difluoroacetate (MDFA) and 1,3,5-trifluorobenzene (TFB) were mixed in a volume ratio of 1:2:2 to prepare a solvent;
[0076] (2) adding lithium bis(trifluoromethanesulfonyl imide) to the solvent of step (1) to prepare a 1 M lithium bis(trifluoromethanesulfonyl imide) (LiTFSI) solution to obtain an intermediate solution;
[0077] (3) Add 0.2 wt % of lithium difluorooxalatoborate to the intermediate solution and stir evenly to obtain an electrolyte.
[0078] Example 2
[0079] This embodiment is the same as Example 1 except that methyl difluoroacetate (MDFA) in step (1) is replaced by methyl trifluoroacetate (MTFA).
[0080] Example 3
[0081] This embodiment is the same as Example 1 except that methyl difluoroacetate (MDFA) in step (1) is replaced by ethyl trifluoroacetate (ETFA).
[0082] Example 4
[0083] This embodiment is the same as Embodiment 1 except that 1,3,5-trifluorobenzene (TFB) in step (1) is replaced by fluorobenzene (FB).
[0084] Example 5
[0085] This embodiment is the same as Embodiment 1 except that “1,3,5-trifluorobenzene in step (1) is replaced by fluorobenzene; and lithium difluorooxalatoborate in step (3) is replaced by vinylene carbonate”.
[0086] Example 6
[0087] This embodiment is the same as Embodiment 1 except that “the fluoroethylene carbonate in step (1) is replaced by 3,3,3-trifluoropropylene carbonate; and the lithium difluorooxalatoborate in step (3) is replaced by vinylene carbonate”.
[0088] Example 7
[0089] A lithium ion battery electrolyte, wherein the preparation method of the electrolyte comprises:
[0090] (1) Same as Example 1;
[0091] (2) adding lithium bis(trifluoromethanesulfonyl imide) to the solvent of step (1) to prepare a 0.1 M lithium bis(trifluoromethanesulfonyl imide) (LiTFSI) solution to obtain an intermediate solution;
[0092] (3) Same as Example 1.
[0093] Example 8
[0094] A lithium ion battery electrolyte, wherein the preparation method of the electrolyte comprises:
[0095] (1) Same as Example 1;
[0096] (2) adding lithium bis(trifluoromethanesulfonyl imide) to the solvent of step (1) to prepare a 5.0 M lithium bis(trifluoromethanesulfonyl imide) (LiTFSI) solution to obtain an intermediate solution;
[0097] (3) Same as Example 1.
[0098] Example 9
[0099] A lithium ion battery electrolyte, wherein the preparation method of the electrolyte comprises:
[0100] (1) In a glove box filled with argon (H2O <1 ppm, O2 <1 ppm), fluoroethylene carbonate (FEC), methyl difluoroacetate (MDFA) and 1,3,5-trifluorobenzene (TFB) were mixed in a volume ratio of 1:10:10 to prepare a solvent;
[0101] (2) Same as Example 1;
[0102] (3) Same as Example 1.
[0103] Example 10
[0104] A lithium ion battery electrolyte, wherein the preparation method of the electrolyte comprises:
[0105] (1) In a glove box filled with argon (H2O <1 ppm, O2 <1 ppm), fluoroethylene carbonate (FEC), methyl difluoroacetate (MDFA) and 1,3,5-trifluorobenzene (TFB) were mixed in a volume ratio of 1:.0.1:0.1 to prepare a solvent;
[0106] (2) Same as Example 1;
[0107] (3) Same as Example 1.
[0108] Embodiment 11
[0109] A lithium ion battery electrolyte, wherein the preparation method of the electrolyte comprises:
[0110] (1) Same as Example 1;
[0111] (2) adding lithium bis(trifluoromethanesulfonyl imide) to the solvent of step (1) to prepare a 0.05 M lithium bis(trifluoromethanesulfonyl imide) (LiTFSI) solution to obtain an intermediate solution;
[0112] (3) Same as Example 1.
[0113] Example 12
[0114] A lithium ion battery electrolyte, wherein the preparation method of the electrolyte comprises:
[0115] (1) Same as Example 1;
[0116] (2) adding lithium bis(trifluoromethanesulfonyl imide) to the solvent of step (1) to prepare a 6M lithium bis(trifluoromethanesulfonyl imide) (LiTFSI) solution to obtain an intermediate solution;
[0117] (3) Same as Example 1.
[0118] Embodiment 13
[0119] A lithium ion battery electrolyte, wherein the preparation method of the electrolyte comprises:
[0120] (1) In a glove box filled with argon (H2O <1 ppm, O2 <1 ppm), fluoroethylene carbonate (FEC), methyl difluoroacetate (MDFA) and 1,3,5-trifluorobenzene (TFB) were mixed in a volume ratio of 1:10:20 to prepare a solvent;
[0121] (2) Same as Example 1;
[0122] (3) Same as Example 1.
[0123] Embodiment 14
[0124] A lithium ion battery electrolyte, wherein the preparation method of the electrolyte comprises:
[0125] (1) In a glove box filled with argon (H2O <1 ppm, O2 <1 ppm), fluoroethylene carbonate (FEC), methyl difluoroacetate (MDFA) and 1,3,5-trifluorobenzene (TFB) were mixed in a volume ratio of 3:10:10 to prepare a solvent;
[0126] (2) Same as Example 1;
[0127] (3) Same as Example 1.
[0128] Comparative Example 1
[0129] A lithium ion battery electrolyte, wherein the preparation method of the electrolyte comprises:
[0130] (1) In a glove box filled with argon (H2O <1 ppm, O2 <1 ppm), ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1 to prepare a solvent;
[0131] (2) Add lithium hexafluorophosphate to the solvent of step (1) to prepare a 1 M lithium hexafluorophosphate solution to obtain an electrolyte.
[0132] Comparative Example 2
[0133] A lithium ion battery electrolyte, wherein the preparation method of the electrolyte comprises:
[0134] (1) In a glove box filled with argon (H2O <1 ppm, O2 <1 ppm), ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed in a volume ratio of 3:7 to prepare a solvent;
[0135] (2) Same as Comparative Example 2.
[0136] Comparative Example 3
[0137] A lithium ion battery electrolyte, wherein the preparation method of the electrolyte comprises:
[0138] (1) In a glove box filled with argon (H2O <1 ppm, O2 <1 ppm), ethylene carbonate (EC), diethyl carbonate (DEC), and 1,3,5-trifluorobenzene (TFB) were mixed in a volume ratio of 1:2:2 to prepare a solvent;
[0139] (2) Same as Example 1;
[0140] (3) Same as Example 1.
[0141] Comparative Example 4
[0142] A lithium ion battery electrolyte, wherein the preparation method of the electrolyte comprises:
[0143] (1) In a glove box filled with argon (H2O <1 ppm, O2 <1 ppm), fluoroethylene carbonate (FEC) and methyl difluoroacetate (MDFA) were mixed in a volume ratio of 1:2 to prepare a solvent;
[0144] (2) Same as Example 1;
[0145] (3) Same as Example 1.
[0146] Comparative Example 5
[0147] A lithium ion battery electrolyte, wherein the preparation method of the electrolyte comprises:
[0148] (1) In a glove box filled with argon (H2O <1 ppm, O2 <1 ppm), fluoroethylene carbonate (FEC), methyl difluoroacetate (MDFA) and 1,3,5-trifluorobenzene (TFB) were mixed in a volume ratio of 1:2:2 to prepare a solvent;
[0149] (2) adding lithium bis(trifluoromethanesulfonyl)imide to the solvent of step (1) to prepare a 1 M lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) solution to obtain an electrolyte.
[0150] This comparative example is the same as Example 1 except that no film-forming additive is added.
[0151] Test Example 1
[0152] The electrolytes prepared in Examples 1 to 14 and Comparative Examples 1 to 5 were respectively assembled into button batteries (Li||NCM811 battery, Li||Li symmetric battery and Li||Cu battery) to test the performance of the electrolytes.
[0153] Among them: Li||NCM battery is used to test rate performance and high voltage resistance; Li||Li symmetric battery is used to test Li + The larger the migration number, the better the rate performance. Li||Cu battery is used to test the coulombic efficiency of different electrolytes.
[0154] Li||NCM811 battery is assembled in the order of negative electrode shell, spring, gasket, lithium sheet, electrolyte, diaphragm, electrolyte, positive electrode sheet, and positive electrode shell, and is used to test leakage current and rate performance. The steps for testing leakage current are as follows: first, use 0.2C constant current to charge and discharge at 3.0-4.3V, and cycle 3 times as an activation step; then charge to 4.7V with 1C constant current, and keep constant voltage at 4.7V for 410h, and record the change of current over time at this time. The steps for testing rate performance are as follows: use 0.2C, 0.5C, 1C, 2C, 3C, 4C, and 5C constant currents for charge and discharge tests, and cycle 5 times for each current condition, and finally use 0.5C and 1C constant currents for charge and discharge, cycle 5 times, and check the capacity recovery of each electrolyte battery.
[0155] Li||Li symmetrical battery is assembled in the order of negative electrode shell, spring, gasket, lithium sheet, electrolyte, diaphragm, electrolyte, lithium sheet, and positive electrode shell. + Migration number, the steps for testing leakage current are as follows: first use 0.5mA / cm 2 The constant current was charged for 2 h, and then 0.5 mA / cm 2 Charge for 2 h, cycle 10 times, and then use the classic EIS-constant voltage polarization method to test Li +The migration number is measured by the following method: using an electrochemical workstation to test the AC impedance before polarization, recorded as R0; applying a small but constant potential difference △V of 5mV to the symmetrical battery, and recording the change of current over time, the initial current is recorded as I0, as the polarization progresses, the battery system current gradually stabilizes, and the current at this time is recorded as I ss ; After completion, conduct AC impedance test, recorded as R ss Finally, Li is calculated using the following formula + Migration number (t + ):
[0156] t + =I ss (ΔV-R0I0 / I0(ΔV-R ss I ss ).
[0157] Note: The Li||Li symmetric battery structure is chosen to eliminate the impact of differences between electrodes.
[0158] The Li||Cu battery is assembled in the order of negative electrode shell, spring, gasket, lithium sheet, electrolyte, diaphragm, electrolyte, copper foil, and positive electrode shell to test the reversibility of Li deposition / stripping on copper foil. The improved Aurbach method is used for testing, and the steps are as follows: the first step is to use 0.5mA / cm 2 The constant current discharge was 10 h to deposit lithium on the copper foil, and then 0.5 mA / cm 2 The constant current is charged to 1V to strip the lithium from the copper foil. The second step is to use 0.5mA / cm 2 The lithium was deposited on the copper foil by constant current discharge for 10 h. In the third step, 0.5 mA / cm 2 Constant current charging for 2h, 0.5mA / cm 2 The constant current was discharged for 2 h, and the cycle was repeated 10 times. Finally, 0.5 mA / cm 2 Charge at a constant current to 1 V. Finally, calculate the average coulombic efficiency (CE) using the following formula:
[0159] CE=Q (总充电容量) / Q (总放电容量) .
[0160] (I) Using Examples 1 to 14 and Comparative Examples 1 to 5 to assemble Li||NCM811 batteries, leakage current data was detected during constant voltage charging at 4.7V.
[0161] The specific test results are shown in Tables 1 and 2 below:
[0162] Table 1:
[0163]
[0164]
[0165] Table 2:
[0166]
[0167] For a more intuitive comparison, this test example plotted the leakage current data of Examples 1 to 3 and Comparative Example 1 during 4.7V constant voltage charging.
[0168] Figure 1 This is a leakage current data diagram of the Li||NCM811 battery assembled in Examples 1 to 3 and Comparative Example 1 during constant voltage charging at 4.7V.
[0169] (ii) The rate performance data of the Li||NCM811 batteries assembled in Examples 1 to 14 and Comparative Examples 1 to 5 were tested at 0.2C, 0.5C, 1C, 2C, 3C, 4C, 5C, 0.5C, and 1C.
[0170] The specific test results are shown in Tables 3 and 4 below:
[0171] Table 3:
[0172] Group Rate performance Example 1 166.77 Example 2 139.78 Example 3 144.02 Example 4 156.01 Example 5 161.92 Example 6 159.7 Example 7 134.25 Example 8 137.02 Example 9 139.9 Example 10 148.89 Embodiment 11 128.92 Example 12 140.20 Embodiment 13 138.42 Embodiment 14 146.04
[0173] Table 4:
[0174] Group Rate performance Comparative Example 1 110.96 Comparative Example 2 99.40 Comparative Example 3 122.47 Comparative Example 4 151.08 Comparative Example 5 151.03
[0175] For a more intuitive comparison, this test example plots the rate performance data of Examples 1 to 3 and Comparative Example 1 at 0.2C, 0.5C, 1C, 2C, 3C, 4C, 5C, 0.5C, and 1C.
[0176] Figure 2 This is a graph of rate performance data of the Li||NCM811 battery assembled in Examples 1 to 3 and Comparative Example 1 at 0.2C, 0.5C, 1C, 2C, 3C, 4C, 5C, 0.5C, and 1C.
[0177] (III) Using Examples 1 to 3 and Comparative Example 1 to assemble a Li||Li symmetric battery, the lithium ion diffusion coefficient was tested.
[0178] Figures 3 to 6 The lithium ion diffusion coefficient diagram of the Li||Li symmetric battery assembled in Examples 1 to 3 and Comparative Example 1. Figures 3 to 6 It can be seen that the Li + A high migration number means that Li + can quickly move to the electrode surface, indicating that Li +The high transfer efficiency in weakly solvated electrolytes helps improve the battery's rapid charging and discharging capabilities.
[0179] (IV) Li||Cu batteries were assembled using Examples 1 to 3 and Comparative Example 1 to test the coulombic efficiency of different electrolytes.
[0180] Figure 7 The coulombic efficiency diagram of the Li||Cu battery assembled in Examples 1 to 3 and Comparative Example 1. Figure 7 It can be seen that the initial coulombic efficiency and average coulombic efficiency of LiCu in the weakly solvated electrolyte in the embodiment are higher than those in the comparative example, indicating that the battery has less energy loss, fewer side reactions, and good stability during the charge and discharge process, especially the reversibility of the lithium metal electrode deposition / stripping process is high.
[0181] In summary, the electrolyte of the present invention has the following beneficial effects:
[0182] 1. Compared with the existing electrolyte, the electrolyte of the present invention utilizes the antioxidant property of fluorine atoms and has high-voltage resistance. Through the floating charge voltage test of NCM811||Li batteries assembled with different electrolytes at 4.7V constant voltage for 10h, the commercial electrolyte has a large leakage current, which means that the battery polarization is serious, while the leakage current of the emerging electrolyte battery is small, indicating that the new electrolyte has better oxidation stability.
[0183] 2. Compared with the existing electrolyte, the electrolyte of the present invention can improve the kinetic migration process of lithium ions and has excellent rate performance. By assembling NCM811||Li batteries with different electrolytes and testing the charge and discharge at different rates, it is found that the discharge specific capacity of the new electrolyte at high rates is significantly higher than that of the commercial electrolyte.
[0184] 3. Compared with existing electrolytes, the high-voltage resistant and high-rate performance electrolyte of the present invention takes into account film-forming performance, has application prospects in high-voltage fast-charging electrolytes, and is expected to solve the "range anxiety" and "charging anxiety" of electric vehicles.
[0185] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. An electrolyte, It is characterized in that The electrolyte comprises: an electrolyte salt, an organic solvent and a diluent, wherein: The organic solvent is a fluorinated solvent, and the fluorinated solvent comprises a fluorinated cyclic carbonate and a fluorinated carboxylic acid ester.
2. The electrolyte according to claim 1, It is characterized in that The electrolyte salt is a lithium salt; Preferably, the lithium salt includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorooxalatophosphate, lithium trifluoromethanesulfonate, lithium hexafluoroarsenate, lithium nitrate, and lithium perchlorate.
3. The electrolyte according to claim 1, It is characterized in that The molar concentration of the electrolyte salt in the electrolyte is 0.1-5.0M.
4. The electrolyte according to claim 1, It is characterized in that The diluent includes at least one of fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, 1,3,4-trifluorobenzene, 1,3,5-trifluorobenzene, 1,2,3,4-tetrafluorobenzene, 1,2,3,5-tetrafluorobenzene, 1,2,4,5-tetrafluorobenzene, 1,2,3,4,5-pentafluorobenzene and hexafluorobenzene.
5. The electrolyte according to claim 1, It is characterized in that The volume ratio of the fluorinated cyclic carbonate, the fluorinated carboxylic acid ester and the diluent in the electrolyte is 1:(0.1-10):(0.1-10).
6. The electrolyte according to claim 1, It is characterized in that The electrolyte also includes a film-forming additive; The film-forming additive includes at least one of vinylene carbonate, lithium difluorooxalatoborate, lithium nitrate, 1,3-propanesulfonate, lithium difluorophosphate, vinyl sulfate, and vinyl sulfite.
7. The electrolyte according to claim 6, It is characterized in that The mass fraction of the film-forming additive in the electrolyte is 0-5.0 wt %.
8. Use of the electrolyte according to any one of claims 1 to 7 in the preparation of a lithium ion battery.
9. A lithium ion battery, It is characterized in that The lithium-ion battery comprises the electrolyte according to any one of claims 1 to 7.
10. The lithium ion battery according to claim 9, It is characterized in that The lithium-ion battery is a high-nickel ternary lithium-ion battery, and the positive electrode material of the high-nickel ternary lithium-ion battery includes LiNi (0.8~0.9) Co (0.05~0.15) Mn (0.05~0.15) O 2 .
Citation Information
Patent Citations
Lithium metal battery electrolyte accommodating aromatic compound as diluent
CN110890592A
High-performance lithium metal battery electrolyte and high-performance lithium metal battery
CN115810799A
High-voltage lithium battery electrolyte containing fluoro ester group and lithium battery
CN116435604A
Lithium ion battery fast charging electrolyte, preparation method and lithium ion battery
CN117638231A
Nonaqueous electrolytic solution for secondary batteries, and lithium ion secondary battery
JP2015064991A
Cited By
Electrolyte of high-voltage lithium ion battery and application of electrolyte
CN119230954A
Electrolyte for lithium metal battery and lithium metal battery
CN119742458A
Electrolyte for lithium metal battery and lithium metal battery
CN119742458B
Battery positive electrode, preparation method thereof and lithium ion battery
CN119864366A
Battery positive electrode and preparation method thereof, lithium ion battery
CN119864366B