Low-temperature battery and preparation method thereof

By using nano-lithium iron phosphate and conductive network materials, modified electrolytes and porous airgel outer membranes in lithium-ion batteries, the problem of poor endurance of lithium-ion batteries at low temperatures is solved and efficient low-temperature performance improvement is achieved.

CN118763296APending Publication Date: 2024-10-11HUNAN HANGRUI TIMES NEW ENERGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410801834.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Lithium-ion batteries exhibit poor endurance, reduced conductivity, and difficulty in inserting and deintercalating lithium ions in low-temperature environments, resulting in a decrease in effective discharge capacity and energy, limiting their applications.

Method used

Nano-lithium iron phosphate is used as the cathode material, and a conductive network formed by a combination of graphene, carbon nanotubes, conductive carbon black, etc. improves the shuttle efficiency of lithium ions and the liquid retention capacity of the electrode material; spherical graphite or non-conductive graphite is used on the negative electrode. Order carbon to form a stable structure; use low-viscosity linear carboxyl ester solvent and SEI film conductive stability additive to modify the electrolyte to improve conductivity; the outer shell is covered with porous nano-silica aerogel or silicon-based aerogel membrane , improve thermal insulation performance.

Benefits of technology

It significantly improves the charging efficiency and cycle performance of low-temperature batteries, enhances the migration pathways of lithium ions, ensures the normal operation of batteries at extreme low temperatures, and significantly improves low-temperature performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763296A_ABST
    Figure CN118763296A_ABST
Patent Text Reader

Abstract

The invention discloses a low-temperature battery and a preparation method thereof, and the preparation method comprises the following steps: preparing positive electrode slurry and negative electrode slurry, coating and rolling the positive electrode slurry and the negative electrode slurry, and then preparing a sheet to obtain a positive plate and a negative plate; the positive plate and the negative plate are wound and laminated and then assembled to obtain a packaged battery cell, and then the packaged battery cell is baked, injected with liquid, formed, graded in capacity and sleeved with a film to obtain the low-temperature battery. According to the positive electrode material, lithium iron phosphate coated with carbon, carbon nanotubes, acetylene black and graphene is adopted, the surface of lithium iron phosphate is coated with a layer of carbon film structure, shuttling of lithium ions is facilitated, the charging efficiency is improved, meanwhile, the coated carbon material can absorb harmful substances, moisture and oxides in an electrolyte, and the cycle performance of the battery is improved; a conductive agent is added into the negative electrode to form a three-dimensional conductive network for linking the current collector and the lithium iron phosphate material, so that the rate capability is improved; the nanocrystallization of the lithium iron material reduces the particle size of particles, and the migration path of lithium ions in a low-temperature state is short.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of batteries, and in particular relates to a low-temperature battery and a preparation method thereof. Background Art

[0002] my country's new energy vehicles have entered a period of rapid development, but for new energy vehicles, the constraints brought by the low-temperature performance of lithium-ion batteries are becoming more and more obvious, and the disadvantages of not being able to adapt to special low-temperature weather or extreme environments are becoming more and more obvious. In low-temperature environments, new energy batteries have poor endurance, because the viscosity of the electrolyte increases under low-temperature conditions, resulting in a decrease in the conductivity of lithium-ion batteries. At the same time, the kinetic performance of lithium ions in low-temperature environments is poor, and lithium ion embedding and de-embedding are difficult. The precipitated metallic lithium will react with the electrolyte and its products will be deposited in the electrolyte, resulting in an increase in the thickness of the solid electrolyte interface; the diffusion rate of lithium ions in the active material is reduced, and the charge transfer impedance is significantly increased. Under low-temperature conditions, the effective discharge capacity and effective discharge energy of lithium-ion batteries will decrease significantly, resulting in poor battery endurance, which seriously restricts the application of lithium-ion batteries. Therefore, a lithium iron phosphate battery with good low-temperature performance is needed.

[0003] Patent document with publication number CN112599726A discloses a gel polymer lithium ion capacitor battery, an electrode and a preparation method thereof. The invention prepares a lithium ion capacitor battery by introducing a PEO polymer, and swells the polymer with an electrolyte after high-temperature aging, thereby eliminating flammable organic solvents. The prepared gel polymer lithium ion capacitor battery does not contain free liquid electrolyte.

[0004] The patent document with publication number CN113540459A discloses a low-temperature resistant lithium-ion battery, including a positive electrode, a negative electrode, an electrolyte and a separator; it also includes a conductive agent added to the positive electrode and / or the negative electrode, and the conductive agent includes graphene aerogel; preferably, the mass of the graphene aerogel accounts for 1% to 3% of the mass of the positive electrode active material or the negative electrode active material; the invention utilizes graphene aerogel dispersed in the positive electrode or the negative electrode to cross-link with each other to form a porous structure, thereby increasing the liquid retention capacity of the electrode material and improving the low-temperature resistance.

[0005] However, none of the above patent documents discloses a technical solution for modifying the electrolyte to improve the low-temperature performance of the battery. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a low-temperature battery and a preparation method thereof.

[0007] The present invention is achieved through the following technical solutions.

[0008] The present invention provides a method for preparing a low-temperature battery, comprising the following steps:

[0009] S1: preparing positive electrode slurry and negative electrode slurry, coating and rolling the positive electrode slurry and negative electrode slurry to obtain positive electrode sheets and negative electrode sheets;

[0010] S2: The positive electrode sheets and the negative electrode sheets are wound and stacked, and then assembled to obtain packaged battery cells, which are then baked, injected, formed, divided and coated to obtain low-temperature batteries.

[0011] Preferably, in parts by weight, the positive electrode slurry comprises 92-96 parts of nano lithium iron phosphate, 2-3 parts of a binder, 2-5 parts of a conductive agent A and a solvent A, and the positive electrode slurry is a slurry with a solid content of 50-65%;

[0012] The lithium iron phosphate D50 is 1-3nm;

[0013] The conductive agent A comprises one or more combinations of graphene, carbon nanotubes, conductive carbon black, and carbon fibers to form a conductive network on the wire surface;

[0014] The binder includes polyvinylidene fluoride, the anti-settling agent includes polyvinylidene fluoride, and the solvent A includes N-methylpyrrolidone;

[0015] The positive electrode slurry preparation method comprises the following steps:

[0016] S1: Add lithium iron phosphate, polyvinylidene fluoride and acetylene black into a blender, rotate at 25 rpm and stir for 5-10 minutes;

[0017] S2: Continue to add N-methylpyrrolidone and stir for 60-80in at 20rpm and 1200rpm;

[0018] S3: After adding carbon nanotubes and graphene, stir at 20 rpm for 15 min; then stir at 25 rpm and 1200 rpm for 60 min;

[0019] S4: After adding NMP, the rotation was continued for 150-180 min at 35 rpm and 1500 rpm, during which the vacuum was maintained at -0.09 MPa;

[0020] S5: Finally, degassing was performed for 30 min at a revolution of 20 rp and a rotation of 600 rp, during which the vacuum was maintained at -0.09 MPa to obtain a positive electrode slurry.

[0021] Preferably, in parts by weight, the negative electrode slurry comprises 94-96 parts of carbon main material, 2-3 parts of binder, 1-2 parts of anti-settling agent, 1-2 parts of conductive agent B and solvent B, and the negative electrode slurry is a slurry with a solid content of 40-55%;

[0022] The carbon main material includes one or more of soft carbon, hard carbon and spherical graphite with a spacing of 0.3-0.4nm;

[0023] The binder comprises styrene-butadiene rubber, the anti-settling agent comprises sodium carboxymethyl cellulose, and the solvent B comprises water;

[0024] The conductive agent B includes one or more combinations of carbon nanotubes, acetylene black, and graphene to form a conductive network on the wire surface;

[0025] The negative electrode slurry preparation method comprises the following steps:

[0026] S1: Add soft carbon, sodium carboxymethyl cellulose and acetylene black into a mixer and stir for 10 min at 25 rpm;

[0027] S2: After adding water, stir at 25 rpm and 800 rpm for 60 min;

[0028] S3: Stir for 150-180 min at 25 rpm and 1200 rpm;

[0029] S4: After adding styrene-butadiene rubber, the mixture was stored at 35 rpm and 600 rpm for 180 min, during which the vacuum was maintained at -0.09 MPa.

[0030] S5: Finally, defoaming was performed for 30 min at a revolution of 20 rp and a rotation of 600 rp, during which the vacuum was maintained at -0.09 MPa to obtain a negative electrode slurry.

[0031] Preferably, the coating comprises the following steps: coating the positive electrode slurry on a 9-14 μm carbon-coated foil at a speed of 20-60 m / min, with a coating density of 180-350 g / ㎡, and then drying at 90-130°C and recovering the evaporated slurry; coating the negative electrode slurry on a 4-8 μm copper foil at a speed of 20-60 m / min, with a coating density of 90-180 g / ㎡, and drying at 60-110°C and recovering the evaporated slurry;

[0032] The rolling process includes the following steps: pressing the coated positive electrode sheet and negative electrode sheet to 80-155 μm, wherein the positive electrode compaction density is 2.2-2.4 g / cm 3 , negative electrode compaction density: 1.1-1.5g / cm 3 .

[0033] Preferably, the sheet making step comprises: cutting the rolled positive electrode sheet and the negative electrode sheet into multiple tabs or full tabs by laser die cutting;

[0034] Winding: The positive electrode sheet, negative electrode sheet and separator are placed on the winding needle according to the connection mode of separator, positive electrode sheet, separator and negative electrode sheet, and then they are wound. After winding, they are taped to obtain the winding core.

[0035] Stacking: After the separator, negative electrode, separator and positive electrode are stacked in a Z-shaped pattern, they are glued together with adhesive tape to obtain a stacked battery cell.

[0036] The diaphragm has a porosity of 40-60% and a thickness of 8-14 μm;

[0037] The assembly comprises the following steps: welding the wound or laminated positive electrode current collector to the aluminum pole ear, welding the negative electrode current collector ear to the copper-nickel pole ear, and then placing the welded core into an aluminum-plastic film package, and performing top and side sealing to obtain a packaged battery cell.

[0038] Preferably, the baking comprises the following steps: baking the assembled packaged battery cells under vacuum for 12 hours, wherein the baking temperature is 90-95°C, until the moisture value of the packaged battery cells is ≤300PPM, injecting electrolyte into the baked packaged battery cells, and circulating 2-8 times at a negative pressure of -0.08Mpa to -0.04Mpa.

[0039] Preferably, the electrolyte comprises the following components in mass percentage: 14.5-16.5% lithium hexafluorophosphate, 3.0-4.0% additive fluoroethylene carbonate, 2-3% propane sultone, 0.3-1.0% vinylene carbonate, 1.0-2.0% vinyl sulfate and solvent C, and the solvent C comprises the following components in mass percentage: 15-20% vinyl carbonate, 40-50% ethyl methyl carbonate, 5-10% linear carboxyl ester, wherein the linear carboxyl ester is one or more of methyl acetate, ethyl acetate, and ethyl propionate.

[0040] Preferably, the formation comprises the following steps: S1: charging the packaged battery cell to 3.1V with a current of 0.02C, and vacuumizing to -0.07Mpa after standing for 5 minutes;

[0041] S2: 0.2C current charges the packaged battery to 4.05V;

[0042] S3: Charge the packaged battery cells to 4.05V at a constant voltage of 0.3C, and then discharge the gas in the packaged battery cells.

[0043] The capacity division includes the following steps: charging the packaged battery cell to 3.65V at a constant current and voltage of 0.5C, cutting off the current to 0.02C, and then discharging the packaged battery cell to 2.5V at 0.5C.

[0044] Preferably, the sleeve film comprises the following steps: sleeve an outer film on the packaged battery core, the outer film comprises silica aerogel or silicon-based aerogel, the outer film has a thickness of 0.3-1.5 mm and a density of 0.16-0.23 mg / cm 3 , porosity 85-95%, thermal conductivity 0.012-0.016W / (mk).

[0045] A low-temperature battery prepared by the preparation method as described above.

[0046] The beneficial effects of the present invention are:

[0047] 1. Excellent low-temperature performance: The positive electrode material is made of lithium iron phosphate coated with carbon, carbon nanotubes, acetylene black, and graphene. A layer of carbon film structure is coated on the surface of lithium iron phosphate to increase the surface area, which is beneficial to the shuttle of lithium ions and improves the charging efficiency. At the same time, the coated carbon material can absorb harmful substances, moisture and oxides in the electrolyte to improve the battery cycle performance; carbon nanotubes, acetylene black, and graphene conductive agents are added to the negative electrode to form a three-dimensional conductive network connecting the current collector and the lithium iron phosphate material to improve the rate performance; nano-lithium iron material reduces the particle size and shortens the lithium ion migration path under low temperature conditions.

[0048] 2. The negative electrode material uses spherical graphite or disordered carbon with large interlayer structures and stable structure. Lithium ions can be embedded from all directions, and the structure is stable and the dynamic performance is excellent.

[0049] 3. The low-temperature modified electrolyte uses a low-viscosity linear carboxyl lipid solvent and a low-temperature additive, and adds an additive for the conductivity stability of the SEI membrane to improve the conductivity of the electrolyte. The electrolyte can normally transport lithium ions under extremely harsh low temperatures.

[0050] 4. The outer shell is covered with a layer of porous nano-silicon dioxide aerogel or silicon-based aerogel outer film. The aerogel material has the characteristics of low density, large specific surface area, and high porosity. These excellent internal structures make it have special thermal, optical, electrical, and acoustic properties such as high temperature resistance, low thermal conductivity, low refractive index, and low sound propagation speed. Aerogel has excellent thermal insulation performance through no convection effect, infinite shielding effect, and infinite long loose path effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 is a low-temperature discharge capacity curve of the low-temperature batteries prepared in the embodiment and the comparative example;

[0052] Figure 2 It is a structural schematic diagram of the battery body of the present invention;

[0053] Figure 3 It is a schematic diagram of the structure of the present invention;

[0054] In the figure: 1-battery body, 2-outer membrane DETAILED DESCRIPTION

[0055] The technical solution of the present invention is further described below, but the scope of protection claimed is not limited to the description.

[0056] Embodiment 1:

[0057] A method for preparing a low-temperature battery comprises the following steps:

[0058] S1: preparing positive electrode slurry and negative electrode slurry, coating and rolling the positive electrode slurry and negative electrode slurry to obtain positive electrode sheets and negative electrode sheets;

[0059] S2: The positive electrode sheet and the negative electrode sheet are wound and assembled to obtain a packaged battery cell, and then a low-temperature battery is obtained after baking, liquid injection, formation, capacity division and film coating.

[0060] In parts by weight, the positive electrode slurry includes 92 parts of nano lithium iron phosphate, 2 parts of a binder, 2 parts of a conductive agent A and a solvent A, and the positive electrode slurry is a slurry with a solid content of 50%;

[0061] The lithium iron phosphate D50 is 1nm;

[0062] The conductive agent A comprises a conductive network formed on the wire surface by combining graphene and carbon nanotubes;

[0063] The binder includes polyvinylidene fluoride, the anti-settling agent includes polyvinylidene fluoride, and the solvent A includes N-methylpyrrolidone;

[0064] The positive electrode slurry preparation method comprises the following steps:

[0065] S1: Add lithium iron phosphate, polyvinylidene fluoride and acetylene black into a blender, rotate at 25 rpm and stir for 5 minutes;

[0066] S2: Continue to add N-methylpyrrolidone and stir for 60-80in at 20rpm and 1200rpm;

[0067] S3: After adding carbon nanotubes and graphene, stir at 20 rpm for 15 min; then stir at 25 rpm and 1200 rpm for 60 min;

[0068] S4: After adding NMP, the rotation was continued for 150 min at 35 rpm and 1500 rpm, during which the vacuum was maintained at -0.09 MPa;

[0069] S5: Finally, degassing was performed for 30 min at a revolution of 20 rp and a rotation of 600 rp, during which the vacuum was maintained at -0.09 MPa to obtain a suspended non-Newtonian fluid positive electrode slurry.

[0070] In parts by weight, the negative electrode slurry includes 94 parts of carbon main material, 2 parts of binder, 1 part of anti-settling agent, 1 part of conductive agent B and solvent B, and the negative electrode slurry is a slurry with a solid content of 40%;

[0071] The carbon main material includes soft carbon with a spacing of 0.3nm;

[0072] The binder comprises styrene-butadiene rubber, the anti-settling agent comprises sodium carboxymethyl cellulose, and the solvent B comprises water;

[0073] The conductive agent B includes acetylene black;

[0074] The negative electrode slurry preparation method comprises the following steps:

[0075] S1: Add soft carbon, sodium carboxymethyl cellulose and acetylene black into a mixer and stir for 10 min at 25 rpm;

[0076] S2: After adding water, stir at 25 rpm and 800 rpm for 60 min;

[0077] S3: Stir for 150-180 min at 25 rpm and 1200 rpm;

[0078] S4: After adding styrene-butadiene rubber, the mixture was stored at 35 rpm and 600 rpm for 180 min, during which the vacuum was maintained at -0.09 MPa.

[0079] S5: Finally, degassing was performed for 30 min at a revolution of 20 rp and a rotation of 600 rp, during which the vacuum was maintained at -0.09 MPa to obtain a suspended non-Newtonian fluid negative electrode slurry.

[0080] The coating comprises the following steps: coating the positive electrode slurry on a 9μm carbon-coated foil at a speed of 20m / min, with a coating density of 180g / ㎡, and then drying at 90°C and recovering the evaporated slurry; coating the negative electrode slurry on a 4μm copper foil at a speed of 20m / min, with a coating density of 90g / ㎡, and then drying at 60°C and recovering the evaporated slurry;

[0081] The rolling process includes the following steps: pressing the coated positive electrode sheet and negative electrode sheet to 80 μm, wherein the positive electrode compaction density is 2.25 g / cm 3 , negative electrode compaction density: 1.1g / cm 3 , the pole piece is compacted to a suitable thickness to ensure that the material particles are not damaged, and the thickness of the pole piece is reduced to shorten the distance that the lithium-ion battery travels.

[0082] The sheet making step comprises: cutting the rolled positive electrode sheet and the negative electrode sheet into multiple tabs or full tabs by laser die cutting;

[0083] Winding: The positive electrode sheet, negative electrode sheet and separator are placed on the winding needle according to the connection mode of separator, positive electrode sheet, separator and negative electrode sheet, and then they are wound. After winding, they are taped to obtain the winding core.

[0084] The diaphragm has a porosity of 40% and a thickness of 8 μm;

[0085] The assembly comprises the following steps: welding the wound core positive electrode current collector to the aluminum pole ear, welding the negative electrode current collector ear to the copper-nickel pole ear, and then placing the welded core into an aluminum-plastic film package, and performing top and side sealing to obtain a packaged battery cell.

[0086] The baking comprises the following steps: baking the assembled packaged battery cell under vacuum for 12 hours, wherein the baking temperature is 90° C., until the moisture value of the packaged battery cell is ≤300 PPM, injecting electrolyte into the baked packaged battery cell, and performing a breathing cycle 4 times under a negative pressure of -0.08 MPa to -0.04 MPa, so that the electrolyte is fully absorbed by the electrode;

[0087] The electrolyte comprises the following components in mass percentage: 14.5% lithium hexafluorophosphate, 3.0% additive fluoroethylene carbonate, 2% propane sultone, 0.3% vinylene carbonate, 1% vinyl sulfate and solvent C, and the solvent C comprises the following components in mass percentage: 15% vinyl carbonate, 40% ethyl methyl carbonate, and 5% linear carboxyl ester, wherein the linear carboxyl ester is methyl acetate.

[0088] The formation comprises the following steps: S1: charging the packaged battery cell to 3.1V with a current of 0.02C, and vacuumizing to -0.07Mpa after standing for 5 minutes;

[0089] S2: 0.2C current charges the packaged battery to 4.05V;

[0090] S3: Charge the packaged battery cells to 4.05V at a constant voltage of 0.3C, and then discharge the gas in the packaged battery cells.

[0091] The capacity division includes the following steps: charging the battery cell to 3.65V at a constant current and voltage of 0.5C, cutting off the current to 0.02C, and then discharging the packaged battery cell to 2.5V at 0.5C.

[0092] The sleeve film comprises the following steps: sleeve an outer film on the packaged battery core, the outer film comprises silica aerogel, the outer film has a thickness of 0.3 mm and a density of 0.16 mg / cm 3 , porosity 85%, thermal conductivity 0.012W / (mk).

[0093] Embodiment 2:

[0094] A method for preparing a low-temperature battery comprises the following steps:

[0095] S1: preparing positive electrode slurry and negative electrode slurry, coating and rolling the positive electrode slurry and negative electrode slurry to obtain positive electrode sheets and negative electrode sheets;

[0096] S2: After stacking the positive and negative electrode sheets, they are assembled to obtain packaged cells, and then after baking, liquid injection, formation, capacity division and film coating, a low-temperature battery is obtained.

[0097] In parts by weight, the positive electrode slurry includes 96 parts of nano lithium iron phosphate, 3 parts of a binder, 5 parts of a conductive agent A and a solvent A, and the positive electrode slurry is a slurry with a solid content of 65%;

[0098] The lithium iron phosphate D50 is 3nm;

[0099] The conductive agent A comprises a conductive network formed on the wire surface by combining conductive carbon black and carbon fiber;

[0100] The binder includes polyvinylidene fluoride, the anti-settling agent includes polyvinylidene fluoride, and the solvent A includes N-methylpyrrolidone;

[0101] The positive electrode slurry preparation method comprises the following steps:

[0102] S1: Add lithium iron phosphate, polyvinylidene fluoride and acetylene black into a blender, rotate at 25 rpm and stir for 10 minutes;

[0103] S2: Continue to add N-methylpyrrolidone and stir for 80 minutes at 20 rpm and 1200 rpm;

[0104] S3: After adding conductive carbon black and carbon fiber, stir at 20 rpm for 15 min; then stir at 25 rpm and 1200 rpm for 60 min;

[0105] S4: After adding NMP, the rotation was continued for 180 min at 35 rpm and 1500 rpm, during which the vacuum was maintained at -0.09 MPa;

[0106] S5: Finally, degassing was performed for 30 min at a revolution of 20 rp and a rotation of 600 rp, during which the vacuum was maintained at -0.09 MPa to obtain a suspended non-Newtonian fluid positive electrode slurry.

[0107] In parts by weight, the negative electrode slurry includes 96 parts of carbon main material, 3 parts of binder, 2 parts of anti-settling agent, 2 parts of conductive agent B and solvent B, and the negative electrode slurry is a slurry with a solid content of 55%;

[0108] The carbon main material includes hard carbon with a spacing of 0.3-0.4nm;

[0109] The binder comprises styrene-butadiene rubber, the anti-settling agent comprises sodium carboxymethyl cellulose, and the solvent B comprises water;

[0110] The conductive agent B includes carbon nanotubes;

[0111] The negative electrode slurry preparation method comprises the following steps:

[0112] S1: After adding hard carbon, sodium carboxymethyl cellulose and carbon nanotubes into a blender, stir at 25 rpm for 10 min;

[0113] S2: After adding water, stir at 25 rpm and 800 rpm for 60 min;

[0114] S3: stirring for 180 min at 25 rpm and 1200 rpm;

[0115] S4: After adding styrene-butadiene rubber, the mixture was stored at 35 rpm and 600 rpm for 180 min, during which the vacuum was maintained at -0.09 MPa.

[0116] S5: Finally, degassing was performed for 30 min at a revolution of 20 rp and a rotation of 600 rp, during which the vacuum was maintained at -0.09 MPa to obtain a suspended non-Newtonian fluid negative electrode slurry.

[0117] The coating comprises the following steps: coating the positive electrode slurry on a 14 μm carbon-coated foil at a speed of 60 m / min, with a coating density of 350 g / ㎡, and then drying at 130°C and recovering the evaporated slurry; coating the negative electrode slurry on an 8 μm copper foil at a speed of 60 m / min, with a coating density of 180 g / ㎡, and then drying at 110°C and recovering the evaporated slurry;

[0118] The rolling process includes the following steps: pressing the coated positive electrode sheet and negative electrode sheet to 155 μm, wherein the positive electrode compaction density is 2.45 g / cm 3 , negative electrode compaction density: 1.5g / cm 3 , the pole piece is compacted to a suitable thickness to ensure that the material particles are not damaged, and the thickness of the pole piece is reduced to shorten the distance that the lithium-ion battery travels.

[0119] The sheet making step comprises: cutting the rolled positive electrode sheet and the negative electrode sheet into multiple tabs or full tabs by laser die cutting;

[0120] Stacking: After stacking the separator, negative electrode, separator and positive electrode in a Z-shaped pattern, use tape to stick the stacked cells together.

[0121] The diaphragm has a porosity of 60% and a thickness of 14 μm;

[0122] The assembly comprises the following steps: welding the laminated positive electrode current collector to the aluminum pole ear, welding the negative electrode current collector ear to the copper-nickel pole ear, and then placing the welded battery cell into an aluminum-plastic film package, and performing top and side sealing to obtain a packaged battery cell.

[0123] The baking comprises the following steps: baking the assembled packaged battery cell under vacuum for 12 hours, wherein the baking temperature is 95° C., until the moisture value of the packaged battery cell is ≤300 PPM, injecting electrolyte into the baked packaged battery cell, and performing a breathing cycle 8 times under a negative pressure of -0.08 MPa to -0.04 MPa, so that the electrolyte is fully absorbed by the electrode;

[0124] The electrolyte comprises the following components in mass percentage: 16.5% lithium hexafluorophosphate, 4.0% additive fluoroethylene carbonate, 3% propane sultone, 1.0% vinylene carbonate, 2.0% vinyl sulfate and solvent C, and the solvent C comprises the following components in mass percentage: 20% vinyl carbonate, 50% ethyl methyl carbonate, and 10% linear carboxyl ester, wherein the linear carboxyl ester is ethyl acetate.

[0125] The formation comprises the following steps: S1: charging the packaged battery cell to 3.1V with a current of 0.02C, and vacuumizing to -0.07Mpa after standing for 5 minutes;

[0126] S2: 0.2C current charges the packaged battery to 4.05V;

[0127] S3: Charge the packaged battery cells to 4.05V at a constant voltage of 0.3C, and then discharge the gas in the packaged battery cells.

[0128] The capacity division includes the following steps: charging the packaged battery cell to 3.65V at a constant current and voltage of 0.5C, cutting off the current to 0.02C, and then discharging the packaged battery cell to 2.5V at 0.5C.

[0129] The sleeve film comprises the following steps: sleeve an outer film on the packaged battery core, the outer film comprises silica aerogel, the outer film has a thickness of 1.5 mm and a density of 0.23 mg / cm 3 , porosity 95%, thermal conductivity 0.016W / (mk).

[0130] Embodiment 3:

[0131] A method for preparing a low-temperature battery comprises the following steps:

[0132] S1: preparing positive electrode slurry and negative electrode slurry, coating and rolling the positive electrode slurry and negative electrode slurry to obtain positive electrode sheets and negative electrode sheets;

[0133] S2: The positive electrode sheet and the negative electrode sheet are wound and assembled to obtain a packaged battery cell, and then a low-temperature battery is obtained after baking, liquid injection, formation, capacity division and film coating.

[0134] In parts by weight, the positive electrode slurry includes 94 parts of nano lithium iron phosphate, 2.5 parts of a binder, 2.5 parts of a conductive agent A and a solvent A, and the positive electrode slurry is a slurry with a solid content of 58%;

[0135] The lithium iron phosphate D50 is 12nm;

[0136] The conductive agent A comprises a conductive network formed on the wire surface by combining carbon nanotubes and carbon fibers;

[0137] The binder includes polyvinylidene fluoride, the anti-settling agent includes polyvinylidene fluoride, and the solvent A includes N-methylpyrrolidone;

[0138] The positive electrode slurry preparation method comprises the following steps:

[0139] S1: Add lithium iron phosphate, polyvinylidene fluoride and acetylene black into a blender, rotate at 25 rpm and stir for 8 minutes;

[0140] S2: Continue to add N-methylpyrrolidone and stir for 70 minutes at 20 rpm and 1200 rpm;

[0141] S3: After adding carbon nanotubes and carbon fibers, stir at 20 rpm for 15 min; then stir at 25 rpm and 1200 rpm for 60 min;

[0142] S4: After adding NMP, the rotation was continued for 170 min at 35 rpm and 1500 rpm, during which the vacuum was maintained at -0.09 MPa;

[0143] S5: Finally, degassing was performed for 30 min at a revolution of 20 rp and a rotation of 600 rp, during which the vacuum was maintained at -0.09 MPa to obtain a suspended non-Newtonian fluid positive electrode slurry.

[0144] In parts by weight, the negative electrode slurry includes 94-96 parts of carbon main material, 2-3 parts of binder, 1-2 parts of anti-settling agent, 1-2 parts of conductive agent B and solvent B, and the negative electrode slurry is a slurry with a solid content of 40-55%;

[0145] The carbon main material includes spherical graphite with a spacing of 0.3-0.4nm;

[0146] The binder comprises styrene-butadiene rubber, the anti-settling agent comprises sodium carboxymethyl cellulose, and the solvent B comprises water;

[0147] The conductive agent B includes graphene;

[0148] The negative electrode slurry preparation method comprises the following steps:

[0149] S1: After adding spherical graphite, sodium carboxymethyl cellulose and graphene into a blender, stir at 25 rpm for 10 min;

[0150] S2: After adding water, stir at 25 rpm and 800 rpm for 60 min;

[0151] S3: Stir for 150-180 min at 25 rpm and 1200 rpm;

[0152] S4: After adding styrene-butadiene rubber, the mixture was stored at 35 rpm and 600 rpm for 180 min, during which the vacuum was maintained at -0.09 MPa.

[0153] S5: Finally, degassing was performed for 30 min at a revolution of 20 rp and a rotation of 600 rp, during which the vacuum was maintained at -0.09 MPa to obtain a suspended non-Newtonian fluid negative electrode slurry.

[0154] The coating comprises the following steps: coating the positive electrode slurry on a 11 μm carbon-coated foil at a speed of 40 m / min, with a coating density of 250 g / ㎡, and then drying at 110°C and recovering the evaporated slurry; coating the negative electrode slurry on a 6 μm copper foil at a speed of 40 m / min, with a coating density of 140 g / ㎡, and then drying at 90°C and recovering the evaporated slurry;

[0155] The rolling process includes the following steps: pressing the coated positive electrode sheet and negative electrode sheet to 120 μm, wherein the positive electrode compaction density is 2.35 g / cm 3 , negative electrode compaction density: 1.3g / cm 3 , the pole piece is compacted to a suitable thickness to ensure that the material particles are not damaged, and the thickness of the pole piece is reduced to shorten the distance that the lithium-ion battery travels.

[0156] The sheet making step comprises: cutting the rolled positive electrode sheet and the negative electrode sheet into multiple tabs or full tabs by laser die cutting;

[0157] Winding: The positive electrode sheet, negative electrode sheet and separator are placed on the winding needle according to the connection mode of separator, positive electrode sheet, separator and negative electrode sheet, and then they are wound. After winding, they are taped to obtain the winding core.

[0158] The diaphragm has a porosity of 50% and a thickness of 11 μm;

[0159] The assembly comprises the following steps: welding the wound core positive electrode current collector to the aluminum pole ear, welding the negative electrode current collector ear to the copper-nickel pole ear, and then placing the welded core into an aluminum-plastic film package, and performing top and side sealing to obtain a packaged battery cell.

[0160] The baking comprises the following steps: baking the assembled packaged battery cell under vacuum for 12 hours, wherein the baking temperature is 93° C., until the moisture value of the packaged battery cell is ≤300 PPM, injecting electrolyte into the baked packaged battery cell, and performing a breathing cycle 4 times under a negative pressure of -0.08 MPa to -0.04 MPa, so that the electrolyte is fully absorbed by the electrode;

[0161] The electrolyte comprises the following components in mass percentage: 15.5% lithium hexafluorophosphate, 3.5% additive fluoroethylene carbonate, 2.5% propane sultone, 0.7% vinylene carbonate, 1.5% vinyl sulfate and solvent C. The solvent C comprises the following components in mass percentage: 18% vinyl carbonate, 46% ethyl methyl carbonate, and 7% linear carboxyl ester, wherein the linear carboxyl ester is ethyl propionate.

[0162] The formation comprises the following steps: S1: charging the packaged battery cell to 3.1V with a current of 0.02C, and vacuumizing to -0.07Mpa after standing for 5 minutes;

[0163] S2: 0.2C current charges the packaged battery to 4.05V;

[0164] S3: Charge the packaged battery cells to 4.05V at a constant voltage of 0.3C, and then discharge the gas in the packaged battery cells.

[0165] The capacity division includes the following steps: charging the packaged battery cell to 3.65V at a constant current and voltage of 0.5C, cutting off the current to 0.02C, and then discharging the packaged battery cell to 2.5V at 0.5C.

[0166] The sleeve film comprises the following steps: sleeve an outer film on the packaged battery core, the outer film comprises a silicon-based aerogel, the outer film has a thickness of 0.9 mm and a density of 0.19 mg / cm 3 , porosity 90%, thermal conductivity 0.014W / (mk).

[0167] like Figure 2 , 3 As shown, the low-temperature battery prepared in Examples 1-3 includes a battery body 1 and an outer membrane 2, and the outer membrane 2 is attached to the outer wall of the battery body 1.

[0168] Comparative Example 1:

[0169] The soft-pack battery prepared by the prior art has a model of 15215316-100Ah.

[0170] The batteries prepared in Example 3 and Comparative Example 1 were placed in 25±2°C, -20±2°C and -40±2°C environments, respectively, and 0.5C charge and discharge tests were performed. The ratio of the discharge capacity at low temperature to the discharge capacity at room temperature was calculated. The batteries charged at low temperature were disassembled to observe the lithium deposition at the negative electrode. The data obtained are shown in the following table and Figure 1 shown.

[0171]

[0172] Through the above table and Figure 1 It can be seen that the low-temperature battery prepared in Example 3 has a discharge efficiency of 99.8% at -20°C and a discharge efficiency of 77.6% at -40°C, and no lithium electrolysis occurs. The low-temperature battery prepared in Comparative Example 1 has a discharge efficiency of 66.1% at -20°C, no lithium electrolysis occurs, and a discharge efficiency of 21.2% at -40°C, but severe lithium electrolysis occurs.

Claims

1. A method for preparing a low-temperature battery, characterized in that: The following steps are involved: S1: preparing positive electrode slurry and negative electrode slurry, coating and rolling the positive electrode slurry and negative electrode slurry to obtain positive electrode sheets and negative electrode sheets; S2: The positive electrode sheets and the negative electrode sheets are wound and stacked, and then assembled to obtain packaged battery cells, which are then baked, injected, formed, divided and coated to obtain low-temperature batteries.

2. A method for preparing a low-temperature battery according to claim 1, characterized in that: In parts by weight, the positive electrode slurry includes 92-96 parts of nano lithium iron phosphate, 2-3 parts of a binder, 2-5 parts of a conductive agent A and a solvent A, and the positive electrode slurry is a slurry with a solid content of 50-65%; The lithium iron phosphate D50 is 1-3nm; The conductive agent A includes one or more of graphene, carbon nanotubes, conductive carbon black, and carbon fiber; The binder includes polyvinylidene fluoride, the anti-settling agent includes polyvinylidene fluoride, and the solvent A includes N-methylpyrrolidone; The positive electrode slurry preparation method comprises the following steps: S1: Add lithium iron phosphate, polyvinylidene fluoride and acetylene black into a blender, rotate at 25 rpm and stir for 5-10 minutes; S2: Continue to add N-methylpyrrolidone and stir for 60-80in at 20rpm and 1200rpm; S3: After adding carbon nanotubes and graphene, stir at 20 rpm for 15 min; then stir at 25 rpm and 1200 rpm for 60 min; S4: After adding NMP, the rotation was continued for 150-180 min at 35 rpm and 1500 rpm, during which the vacuum was maintained at -0.09 MPa; S5: Finally, degassing was performed for 30 min at a revolution of 20 rp and a rotation of 600 rp, during which the vacuum was maintained at -0.09 MPa to obtain a positive electrode slurry.

3. The method for preparing a low-temperature battery according to claim 1, characterized in that: In parts by weight, the negative electrode slurry includes 94-96 parts of carbon main material, 2-3 parts of binder, 1-2 parts of anti-settling agent, 1-2 parts of conductive agent B and solvent B, and the negative electrode slurry is a slurry with a solid content of 40-55%; The carbon main material includes one or more of soft carbon, hard carbon and spherical graphite with a spacing of 0.3-0.4nm; The binder comprises styrene-butadiene rubber, the anti-settling agent comprises sodium carboxymethyl cellulose, and the solvent B comprises water; The conductive agent B includes one or more of carbon nanotubes, acetylene black, and graphene; The negative electrode slurry preparation method comprises the following steps: S1: Add soft carbon, sodium carboxymethyl cellulose and acetylene black into a mixer and stir for 10 min at 25 rpm; S2: After adding water, stir at 25 rpm and 800 rpm for 60 min; S3: Stir for 150-180 min at 25 rpm and 1200 rpm; S4: After adding styrene-butadiene rubber, the mixture was stored at 35 rpm and 600 rpm for 180 min, during which the vacuum was maintained at -0.09 MPa. S5: Finally, defoaming was performed for 30 min at a revolution of 20 rp and a rotation of 600 rp, during which the vacuum was maintained at -0.09 MPa to obtain a negative electrode slurry.

4. The method for preparing a low-temperature battery according to claim 1, characterized in that: The coating comprises the following steps: coating the positive electrode slurry on a 9-14 μm carbon-coated foil at a speed of 20-60 m / min, with a coating density of 180-350 g / ㎡, and then drying at 90-130° C. and recovering the evaporated slurry; coating the negative electrode slurry on a 4-8 μm copper foil at a speed of 20-60 m / min, with a coating density of 90-180 g / ㎡, and drying at 60-110° C. and recovering the evaporated slurry; The rolling process includes the following steps: pressing the coated positive electrode sheet and negative electrode sheet to 80-155 μm, wherein the positive electrode compaction density is 2.2-2.4 g / cm 3 , negative electrode compaction density: 1.1-1.5g / cm 3 .

5. The method for preparing a low-temperature battery according to claim 1, characterized in that: The sheet making step comprises: cutting the rolled positive electrode sheet and the negative electrode sheet into multiple tabs or full tabs by laser die cutting; Winding: The positive electrode sheet, negative electrode sheet and separator are placed on the winding needle according to the connection mode of separator, positive electrode sheet, separator and negative electrode sheet, and then they are wound. After winding, they are taped to obtain the winding core. Stacking: After the separator, negative electrode, separator and positive electrode are stacked in a Z-shaped pattern, they are glued together with adhesive tape to obtain a stacked battery cell. The diaphragm has a porosity of 40-60% and a thickness of 8-14 μm; The assembly comprises the following steps: welding the wound or laminated positive electrode current collector to the aluminum pole ear, welding the negative electrode current collector ear to the copper-nickel pole ear, and then placing the welded core into an aluminum-plastic film package, and performing top and side sealing to obtain a packaged battery cell.

6. A method for preparing a low-temperature battery according to claim 1, characterized in that: The baking comprises the following steps: baking the assembled packaged battery cells under vacuum for 12 hours, wherein the baking temperature is 90-95° C., until the moisture value of the packaged battery cells is ≤300 PPM, injecting electrolyte into the baked packaged battery cells, and circulating 2-8 times under a negative pressure of -0.08 Mpa to -0.04 Mpa.

7. The method for preparing a low-temperature battery according to claim 1, characterized in that: The electrolyte comprises the following components in mass percentage: 14.5-16.5% lithium hexafluorophosphate, 3.0-4.0% additive fluoroethylene carbonate, 2-3% propane sultone, 0.3-1.0% vinylene carbonate, 1.0-2.0% vinyl sulfate and solvent C. The solvent C comprises the following components in mass percentage: 15-20% vinyl carbonate, 40-50% ethyl methyl carbonate, 5-10% linear carboxyl ester, wherein the linear carboxyl ester is one or more of methyl acetate, ethyl acetate and ethyl propionate.

8. The method for preparing a low-temperature battery according to claim 1, characterized in that: The formation The following steps are involved: S1: Charge the packaged battery to 3.1V with a current of 0.02C, place it aside for 5 minutes, and then evacuate it to -0.07Mpa; S2: 0.2C current charges the packaged battery to 4.05V; S3: Charge the packaged battery cells to 4.05V at a constant voltage of 0.3C, and then discharge the gas in the packaged battery cells. The capacity division includes the following steps: charging the packaged battery cell to 3.65V at a constant current and voltage of 0.5C, cutting off the current to 0.02C, and then discharging the packaged battery cell to 2.5V at 0.5C.

9. The method for preparing a low-temperature battery according to claim 1, characterized in that: The sleeve film comprises the following steps: sleeve an outer film on the packaged battery core, the outer film comprises silica aerogel or silicon-based aerogel, the outer film has a thickness of 0.3-1.5 mm and a density of 0.16-0.23 mg / cm 3 , porosity 85-95%, thermal conductivity 0.012-0.016W / (mk).

10. A low-temperature battery prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Positive electrode slurry and positive electrode plate of low-temperature power type lithium ion battery and battery

    CN119480878A