Lithium-sulfur battery diaphragm, preparation method and application thereof, and lithium-sulfur battery

By using a double-layer composite separator of polymer/halloysite nanotube electrospinning membrane and polypyrrole membrane layer in lithium-sulfur batteries, the problem of polysulfide 'shuttle effect' in lithium-sulfur batteries is solved and the efficiency is improved. Electrochemical performance and cycle stability, achieving higher battery performance and longer cycle capacity retention.

CN118763357AActive Publication Date: 2024-10-11HUIZHOU LIWINON NEW ENERGY TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410709038.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-10-11
Estimated Expiration
2044-06-03

AI Technical Summary

Technical Problem

The severe polysulfide ‘shuttle effect’ in lithium-sulfur batteries leads to poor electrochemical performance and cycle stability, affecting its commercial application.

Method used

A high molecular polymer/halloysite nanotube electrospinning membrane is used as the base layer, and a polypyrrole film layer is grown on the surface of the halloysite nanotube carbonized film layer to form a double-layer composite separator to adsorb and convert soluble polysulfide. substances, improve the utilization rate of active substances and weaken the 'shuttle effect'.

Benefits of technology

Effectively suppresses the 'shuttle effect' of polysulfides, improves the electrochemical performance and cycle stability of lithium-sulfur batteries, improves the utilization of positive active materials, and prolongs the battery's cycle capacity retention rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763357A_ABST
    Figure CN118763357A_ABST
Patent Text Reader

Abstract

The invention discloses a lithium-sulfur battery diaphragm as well as a preparation method and application thereof and a lithium-sulfur battery, the lithium-sulfur battery diaphragm comprises a substrate layer and a functional layer, a high-molecular polymer / halloysite nanotube electrostatic spinning membrane is used as a substrate insulating layer, and polypyrrole is grown on the surface of a carbonized halloysite nanotube carbonized membrane in situ to serve as the functional layer. From the perspective of modification of the lithium-sulfur battery electrostatic spinning diaphragm, the double-layer composite electrostatic spinning diaphragm is prepared, one layer of electrostatic spinning diaphragm is carbonized, polysulfide in an electrolyte is adsorbed and dissolved by using HNTs, and the shuttle effect of the polysulfide is improved; meanwhile, conductive polymer polypyrrole grows on the HNTs carbonized film fiber in situ, and soluble polysulfide can be converted and utilized into insoluble polysulfide by the polypyrrole, so that the utilization rate of active substances is increased, the shuttle effect of the polysulfide is effectively inhibited, and the electrochemical performance and the cycling stability of the lithium-sulfur battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a lithium-sulfur battery separator and a preparation method and application thereof, and a lithium-sulfur battery. Background Art

[0002] Lithium-sulfur battery (LSB) has the advantages of high theoretical energy density, low cost and environmental friendliness, and has received extensive attention and research. It is one of the most promising candidates for the next generation of energy storage systems. It has a high theoretical specific capacity of up to 1675mAh / g and a high theoretical energy density of 2600Wh / kg, which is several times that of lithium-ion batteries (LIB). In addition, its active material sulfur also has the advantages of abundant reserves, low cost, environmental protection, non-toxicity and high safety.

[0003] However, the commercialization of lithium-sulfur batteries still faces many problems, such as the serious polysulfide "shuttle effect", poor electrochemical reversibility and rapid capacity decay of lithium-sulfur batteries. x ,x≥4) is the most critical factor that reduces the electrochemical performance and cycle stability of LSBs.

[0004] Therefore, it is of great significance to solve the serious problem of polysulfide "shuttle effect" in lithium-sulfur batteries and improve the electrochemical performance and cycle stability of lithium-sulfur batteries. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes a lithium-sulfur battery separator and a preparation method and application thereof, and a lithium-sulfur battery, aiming to solve the serious polysulfide "shuttle effect" problem existing in the current lithium-sulfur battery and improve the electrochemical performance and cycle stability of the lithium-sulfur battery.

[0006] In a first aspect of the present invention, a lithium-sulfur battery separator is proposed, comprising a base layer and a functional layer arranged on the base layer; the base layer comprises a polymer / halloysite nanotube electrospinning film layer; the functional layer comprises a halloysite nanotube carbonized film layer, and a polypyrrole film layer grown on the surface of the halloysite nanotube carbonized film layer.

[0007] The lithium-sulfur battery separator according to the embodiment of the present invention has at least the following beneficial effects: The present invention proposes an integrated double-layer lithium-sulfur battery separator, comprising a base layer and a functional layer. Among them, the polymer / halloysite nanotube electrospinning membrane is used as the base insulating layer, and polypyrrole (PPy) is grown on the surface of the carbonized halloysite nanotube (HNTs) carbonized film layer after carbonization as the functional layer. In the functional layer, the conductive polymer polypyrrole is attached to the carbonized fiber surface of the halloysite nanotube carbonized film layer, which can convert soluble polysulfides into insoluble polysulfides, thereby improving the utilization rate of active substances. In addition, due to its tubular structure and nuclear power state of positive inside and negative outside, the silicate mineral halloysite can adsorb and dissolve polysulfides in the electrolyte, weaken the "shuttle effect" of the lithium-sulfur battery, and reduce the capacity decay during the cycle of the lithium-sulfur battery. Finally, the present invention starts from the perspective of modification of electrostatic spinning membrane for lithium-sulfur battery, prepares a double-layer composite electrostatic spinning membrane, and carbonizes one layer of polymer / halloysite nanotube electrostatic spinning membrane, uses HNTs to adsorb and dissolve polysulfides in the electrolyte, and improves the "shuttle effect" of polysulfides; at the same time, a conductive polymer polypyrrole is grown on the surface of the carbonized halloysite nanotube carbonized membrane layer, and polypyrrole can convert soluble polysulfides into insoluble polysulfides, thereby improving the utilization rate of active substances. The lithium-sulfur battery separator of the present invention not only improves the utilization rate of positive electrode active substances, but also effectively inhibits the "shuttle effect" of polysulfides, and improves the electrochemical performance and cycle stability of lithium-sulfur batteries.

[0008] In some embodiments of the present invention, in the polymer / halloysite nanotube electrospinning membrane layer, the carbon atom content of the polymer is ≥35%.

[0009] In some embodiments of the present invention, the high molecular weight polymer includes a fluorocarbon polymer.

[0010] In some embodiments of the present invention, the high molecular weight polymer includes polyvinylidene fluoride (PVDF).

[0011] In some embodiments of the present invention, the polymer / halloysite nanotube electrospinning membrane layer is a polyvinylidene fluoride / halloysite nanotube (PVDF / HNTs) electrospinning membrane layer. Compared with commercial polyolefin membranes, the electrospinning membrane containing PVDF of the present invention has higher porosity, electrolyte absorption capacity, thermal stability and ionic conductivity.

[0012] In some embodiments of the present invention, the molecular formula of halloysite nanotubes (HNTs) is Al2Si2O5(OH)4·2H2O.

[0013] HNTs is a natural clay composed of aluminosilicate layers. It is a silicate mineral with spherical, lamellar and tubular structures, among which the tubular structure is the most common. The silicates in the molecules constitute the tubular layers of the halloysite nanotubes, which roll inward for more than twenty layers to form a tubular structure. The inner diameter of the tube is generally 15 to 100 nm, and the length of the tube is generally 500 to 1000 nm. HNTs have polar functional groups. The Si-O tetrahedron on the outer surface and the Al-O octahedron on the inner surface cause the HNTs to present an external negative charge and an internal positive charge. It has good ionic conductivity and good adsorption, can adsorb polysulfides, and weaken the "shuttle effect" of lithium-sulfur batteries. The present invention adds HNTS to the electrospinning membrane to adsorb and dissolve polysulfides in the electrolyte of lithium-sulfur batteries, reduce or even avoid the diffusion and migration of dissolved polysulfides to the negative electrode side of the battery to generate insulating and insoluble Li2S2 and Li2S, and then cover the negative electrode surface, thereby inhibiting the "shuttle effect" of lithium-sulfur batteries and achieving the effect of improving battery performance.

[0014] In some embodiments of the present invention, the functional layer includes a halloysite nanotube (HNTs) carbonized film layer, and the HNTs carbonized film layer is obtained by high-molecular polymer / halloysite nanotube electrospinning film layer through high-temperature carbonization treatment. After carbonization, the polymer becomes a carbon material and forms a HNTs carbonized film layer together with the halloysite nanotubes. Preferably, the HNTs carbonized film layer is obtained by high-temperature carbonization treatment of polyvinylidene fluoride / halloysite nanotube (PVDF / HNTs) electrospinning film layer. The present invention carbonizes the polymer / halloysite nanotube (such as PVDF / HNTs) electrospinning film at high temperature, and the carbonized film has good conductivity. At the same time, the HNTs in the carbonized fiber membrane can adsorb and dissolve polysulfides in the electrolyte, improving the shortcomings of the battery due to the "shuttle effect" of polysulfides, such as poor electrochemical reversibility and rapid capacity decay.

[0015] In some preferred embodiments of the present invention, the high temperature carbonization treatment is carried out under the following conditions: carbonization in a tube furnace at 800-1000°C for 8-12 hours under a protective gas atmosphere. Preferably, the protective gas is nitrogen. Preferably, carbonization in a tube furnace at 1000°C for 8 hours.

[0016] In some embodiments of the present invention, the functional layer further comprises a polypyrrole film layer in-situ grown on the surface of the HNTs carbonized film layer.

[0017] Polypyrrole (PPy) is a heterocyclic conjugated conductive polymer with good air stability and is a conductive polymer that is easy to electrochemically polymerize into a film. Polypyrrole has a conjugated chain oxidation and a corresponding anion doping structure, and its conductivity can reach 10 2 ~10 3S / cm, the tensile strength can reach 50-100Mpa, and it has good electrochemical redox reversibility. Conductive mechanism of polypyrrole: PPy has a conjugated structure composed of alternating carbon-carbon single bonds and carbon-carbon double bonds. The double bond is composed of σ electrons and π electrons. The σ electrons are fixed and cannot move freely, forming covalent bonds between carbon atoms. The two π electrons in the conjugated double bond are not fixed on a certain carbon atom. They can be transferred from one carbon atom to another carbon atom, and have a tendency to extend on the entire molecular chain. That is, the overlap of the π electron cloud within the molecule produces an energy band shared by the entire molecule, and the π electrons are similar to free electrons in metal conductors. When an electric field exists, the electrons that make up the π bond can move along the molecular chain. Polypyrrole has good electrical conductivity and electrochemical properties and the ability to adsorb and utilize polysulfides, which can inhibit the dissolution and shuttling of polysulfides. At the same time, polypyrrole and the highly conductive HNTs carbonized film work together to effectively inhibit the "shuttle effect" of polysulfides.

[0018] In the present invention, polypyrrole is in situ grown on the carbonized halloysite nanotube carbonized film fiber. Polypyrrole has good conductivity, electrochemical properties and the ability to adsorb and utilize polysulfides, and can inhibit the shuttling of polysulfides. The polypyrrole grows on the fiber and does not occupy additional space, and can be used as a separator to store Li + Moreover, due to the good ionic conductivity of HNTs, they can work synergistically with polypyrrole to further improve the cycle stability of lithium-sulfur batteries.

[0019] Meanwhile, compared with commercial polyolefin membranes, the electrospinning membrane containing PVDF of the present invention has higher porosity, electrolyte absorption capacity, thermal stability and ionic conductivity, etc.

[0020] In some embodiments of the present invention, in the high molecular polymer / halloysite nanotube electrospinning membrane layer, the mass fraction of halloysite nanotubes is 1 to 20%, preferably 1 to 5%.

[0021] In some embodiments of the present invention, in the carbonized halloysite nanotube film layer, the mass fraction of the halloysite nanotubes is 1 to 20%, preferably 1 to 5%.

[0022] In some embodiments of the present invention, in the polyvinylidene fluoride / halloysite nanotube (PVDF / HNTs) electrospinning membrane layer, the mass fraction of halloysite nanotubes is 1 to 20%, preferably 1 to 5%.

[0023] In some embodiments of the present invention, in the carbonized halloysite nanotube film layer, the mass fraction of the halloysite nanotubes is 1 to 20%, preferably 1 to 5%.

[0024] The mass fraction of HNTs in PVDF / HNTs electrospinning membrane affects its function. When the mass fraction of HNTs is greater than 5%, as the proportion of HNTs increases, the functional layer may become powdery and fall off during the cycle, losing its original function. When the mass fraction of HNTs is less than 1%, the effect of HNTs in adsorbing polysulfides will decrease.

[0025] In some embodiments of the present invention, the thickness of the base layer is 8-10 μm, for example, 8 μm, 9 μm, or 10 μm.

[0026] In some embodiments of the present invention, the thickness of the functional layer is 8-10 μm, for example, 8 μm, 9 μm, or 10 μm.

[0027] In a second aspect of the present invention, a method for preparing the above-mentioned lithium-sulfur battery separator is provided, comprising the steps of:

[0028] S10, preparing a polymer / halloysite nanotube solution;

[0029] S20, preparing a polymer / halloysite nanotube electrospinning membrane layer by an electrospinning process;

[0030] S30, subjecting the prepared high molecular polymer / halloysite nanotube electrospinning membrane layer to high temperature carbonization treatment to obtain a halloysite nanotube carbonized membrane layer;

[0031] S40, in-situ growing a polypyrrole film layer on the surface of the halloysite nanotube carbonized film layer to obtain a functional layer;

[0032] S50, preparing another layer of prepared high molecular polymer / halloysite nanotube electrospinning membrane layer as a base layer on the functional layer by an electrospinning process to obtain the lithium-sulfur battery separator.

[0033] The preparation method of the lithium-sulfur battery separator according to the embodiment of the present invention has at least the following beneficial effects: the preparation method of the present invention prepares a single-layer polymer / halloysite nanotube electrospun membrane by an electrospinning process, and then the polymer / halloysite nanotube electrospun membrane is carbonized at high temperature, and then polypyrrole with redox activity is grown in situ on the carbonized fiber, and then another layer of polymer / halloysite nanotube electrospun membrane is electrospun on the membrane as an insulating layer. Finally, the double-layer composite separator prepared by the present invention has high electrochemical performance and good ability to adsorb and utilize polysulfides, and the preparation process is simple, the reaction conditions are not harsh, and the time consumption is short. It is also compatible with common commercial battery preparation methods, providing a solution for the commercial use of lithium-sulfur batteries.

[0034] In some embodiments of the present invention, in the polymer / halloysite nanotube solution, the mass ratio of polymer:halloysite nanotube is (99:1) to (80:20); preferably, the mass ratio of polymer:halloysite nanotube is (99:1) to (95:5); more preferably, the mass ratio of polymer:halloysite nanotube is about 95:5.

[0035] The mass fraction of HNTs in the polymer / halloysite nanotube solution affects the mass fraction of HNTs in the formed electrospun membrane, and thus affects its function. When the mass fraction of HNTs is greater than 5%, as the proportion of HNTs increases, the functional layer may pulverize and fall off during the cycle and lose its original function; and when the mass fraction of HNTs is less than 1%, the effect of HNTs in adsorbing polysulfides will decrease. In some embodiments of the present invention, in steps S20 and S50, the thickness of the polymer / halloysite nanotube electrospinning membrane layer prepared by the electrospinning process is 8 to 10 μm, for example, 8 μm, 9 μm, or 10 μm.

[0036] In some embodiments of the present invention, in step S30, the conditions of the high temperature carbonization treatment are: carbonization in a tube furnace at 800-1000°C for 8-12 hours under a protective gas atmosphere. Preferably, the protective gas is nitrogen. Preferably, carbonization in a tube furnace at 1000°C for 8 hours. The halloysite nanotube carbonized film layer is obtained by high-molecular polymer / halloysite nanotube electrospinning film layer subjected to high-temperature carbonization treatment. After carbonization, the polymer becomes a carbon material and forms a HNTs carbonized film layer together with the halloysite nanotubes.

[0037] In some embodiments of the present invention, step S40 specifically includes:

[0038] S41, mixing appropriate amounts of pyrrole monomer solution, ammonium persulfate solution and ferric chloride solution to prepare a polypyrrole solution;

[0039] S42, placing the halloysite nanotube carbonized film layer in the polypyrrole solution, so that polypyrrole is in-situ grown on the surface of the halloysite nanotube carbonized film layer to form a polypyrrole film layer;

[0040] S43, after standing at room temperature for a predetermined time, the functional layer is obtained.

[0041] In some preferred embodiments of the present invention, in step S43, the reaction mixture is allowed to stand at room temperature for 12 to 48 hours; preferably, it is allowed to stand at room temperature for 18 to 30 hours; more preferably, it is allowed to stand at room temperature for 24 hours. Whether polypyrrole grows in situ on the surface of the halloysite nanotube carbonized film layer will affect the adsorption, conversion and utilization of polysulfide by the composite diaphragm. If the reaction time is too short, it is not conducive to the coating and generation of polypyrrole on the surface of the carbonized fiber; and when the reaction reaches the best, as time increases, it will cause the aggregation of polypyrrole and increase the thickness of the diaphragm, and its effect will be reduced.

[0042] In some preferred embodiments of the present invention, in step S43, after obtaining the functional layer, the excess polypyrrole and excess ions on the surface can be washed with deionized water and placed in a vacuum drying oven at 45°C for 12 hours.

[0043] In a specific embodiment of the present invention, the method for preparing the lithium-sulfur battery separator comprises the steps of:

[0044] S100, preparing a polyvinylidene fluoride / halloysite nanotube (PVDF / HNTs) solution;

[0045] S200, preparing a polyvinylidene fluoride / halloysite nanotube (PVDF / HNTs) electrospinning membrane layer by an electrospinning process;

[0046] S300, subjecting the polyvinylidene fluoride / halloysite nanotube (PVDF / HNTs) electrospinning membrane layer to high-temperature carbonization to obtain a halloysite nanotube (HNTs) carbonized membrane layer;

[0047] S400, in-situ growing a polypyrrole film layer on the surface of the halloysite nanotube (HNTs) carbonized film layer to obtain a functional layer;

[0048] S500, preparing another layer of polyvinylidene fluoride / halloysite nanotube (PVDF / HNTs) electrospinning membrane layer as a base layer on the functional layer by an electrospinning process to obtain the lithium-sulfur battery separator.

[0049] Figure 1The figure shows a schematic diagram of the preparation process of a specific embodiment of the double-layer composite diaphragm of a lithium-sulfur battery of the present invention. First, a PVDF / HNTs solution is prepared, and a single-layer PVDF / HNTs electrospinning membrane is prepared by an electrospinning process. The PVDF / HNTs electrospinning membrane is then carbonized at a high temperature above 800°C, and then a redox-active polypyrrole is grown in situ on the carbonized fiber to obtain a (PVDF / HNTS carbonized membrane)@polypyrrole single-layer membrane as a functional layer; finally, another layer of PVDF / HNTs electrospinning membrane is electrospun on the membrane as an insulating layer. Finally, the double-layer composite diaphragm prepared by the present invention has high electrochemical properties and good ability to adsorb and utilize polysulfides, providing a solution for the commercial use of lithium-sulfur batteries.

[0050] In some embodiments of the present invention, in the PVDF / HNTs solution, the mass ratio of PVDF:HNTS is (99:1) to (80:20); preferably, the mass ratio of PVDF:HNTS is (99:1) to (95:5); more preferably, the mass ratio of PVDF:HNTS is about 95:5.

[0051] The mass fraction of HNTs in the PVDF / HNTs solution affects the mass fraction of HNTs in the electrospun membrane, and thus affects its function. When the mass fraction of HNTs is greater than 5%, the increase in the mass fraction of HNTs may cause the functional layer to pulverize and fall off during the cycle, losing its original function; and when the mass fraction of HNTs is less than 1%, the effect of HNTs in adsorbing polysulfides will decrease.

[0052] In some embodiments of the present invention, in step S100, DMF is used as a solvent to prepare a PVDF / HNTs solution, and the mass fraction of the solution is 10-20%, preferably about 13%.

[0053] In some embodiments of the present invention, in steps S200 and S500, the thickness of the polyvinylidene fluoride / halloysite nanotube electrospinning membrane layer prepared by the electrospinning process is 8-10 μm, for example, 8 μm, 9 μm, or 10 μm.

[0054] In some embodiments of the present invention, in step S300, the high temperature carbonization treatment is carried out under the following conditions: carbonization in a tube furnace at 800-1000°C for 8-12 hours under a protective gas atmosphere. Preferably, the protective gas is nitrogen. Preferably, carbonization in a tube furnace at 1000°C for 8 hours.

[0055] In some embodiments of the present invention, step S400 specifically includes:

[0056] S401, mixing appropriate amounts of pyrrole monomer solution, ammonium persulfate solution and ferric chloride solution to prepare a polypyrrole solution;

[0057] S402, placing the halloysite nanotube carbonized film layer in the polypyrrole solution, so that polypyrrole grows in situ on the surface of the halloysite nanotube carbonized film layer to form a polypyrrole film layer;

[0058] S403, after standing at room temperature for a predetermined time, the functional layer is obtained.

[0059] In some preferred embodiments of the present invention, in step S403, the reaction mixture is allowed to stand at room temperature for 12 to 48 hours; preferably, it is allowed to stand at room temperature for 18 to 30 hours; and more preferably, it is allowed to stand at room temperature for 24 hours. Whether polypyrrole grows in situ on the surface of the PVDF / HNTs carbonized membrane will affect the adsorption, conversion and utilization of polysulfides by the composite membrane. If the reaction time is too short, it is not conducive to the coating and generation of polypyrrole on the surface of the carbonized fiber; and when the reaction reaches the optimum, as time increases, it will cause the aggregation of polypyrrole and increase the thickness of the membrane, and its effect will be reduced.

[0060] In some preferred embodiments of the present invention, in step S403, after obtaining the functional layer, the excess polypyrrole and excess ions on the surface can be washed off with deionized water and placed in a vacuum drying oven at 45°C for 12 hours.

[0061] In a third aspect of the present invention, a lithium-sulfur battery is provided, comprising the lithium-sulfur battery separator as described above or the lithium-sulfur battery separator prepared by the above preparation method.

[0062] The lithium-sulfur battery according to the embodiment of the present invention has at least the following beneficial effects: the lithium-sulfur battery proposed in the present invention adopts the above-mentioned composite diaphragm, so it has at least all the beneficial effects brought by the technical solution of the above-mentioned implementation mode, that is, the utilization rate of the obtained battery positive electrode active material is higher, the ability to adsorb polysulfides is better, and the "shuttle effect" of polysulfides can be effectively suppressed, the battery is more stable, the electrochemical performance is better, the specific capacity is higher, and the cycle capacity retention rate is better.

[0063] In the present invention, there are no restrictions on the positive electrode, negative electrode, electrolyte, etc. of the assembled battery, and materials commonly used in the art can be reasonably adopted, which will not be described in detail here.

[0064] In a fifth aspect of the present invention, a use of the above-mentioned lithium-sulfur battery separator or the lithium-sulfur battery separator prepared by the above-mentioned preparation method in the preparation of energy storage devices, power devices or electronic devices is proposed. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein:

[0066] Figure 1 Schematic diagram of the preparation process of a double-layer composite diaphragm for a lithium-sulfur battery in an embodiment of the present invention. DETAILED DESCRIPTION

[0067] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0068] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0069] In the description of the present invention, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, wherein a and b are real numbers. Unless otherwise specified, each reaction or operation step may be performed in sequence or not. Preferably, the reaction method of the present invention is performed in sequence.

[0070] If no specific techniques or conditions are specified in the following examples, the techniques or conditions described in the literature in the art or the product instructions are used. All reagents or instruments without manufacturer specified are conventional products that can be purchased commercially.

[0071] Example 1

[0072] 1. Preparation of diaphragm

[0073] (1) Using DMF as solvent, prepare a solution with a mass ratio of PVDF:HNTS of 95:5 and a mass fraction of 13%. Stir at 90°C for 5h to form a homogeneous precursor solution, transfer it to a 10mL syringe and let it stand until there are no bubbles, then fix it on a syringe pump with a moving speed of 20mm / min. Apply constant voltages of +26kV and -2kV, and spray the nanofibers onto a 600r / min drum at a distance of 20cm at a push speed of 0.4mL / h. Inject 1.5mL of spinning solution to spin the outer diaphragm, and sandwich tin foil in the same direction as the rotation of the drum to prepare a PVDF / HNTs single-layer electrospun membrane with a thickness of about 10μm.

[0074] (2) carbonizing the single-layer electrospun membrane prepared in step (1) in a tubular furnace at 1000° C. for 8 h under nitrogen protection to obtain a PVDF / HNTs carbonized membrane;

[0075] (3) Weigh 114 g of ammonium persulfate and place it in a 500 mL beaker to prepare a 1 mol / L ammonium persulfate solution A, stir evenly and let stand for use;

[0076] Weigh 81g of ferric chloride powder into a 500mL beaker to prepare a 1mol / L ferric chloride solution B, stir evenly and let stand for use;

[0077] Weigh 33.5 g of pyrrole monomer with a syringe and dissolve it in a 500 mL beaker to obtain pyrrole solution C. Wrap it in tin foil to avoid light, stir evenly, and let it stand for use;

[0078] Prepare 1 mol / L hydrochloric acid solution D and set aside;

[0079] Use a syringe to draw 20 mL of solution A, B, and C respectively, stir evenly, pour into a petri dish, and add dilute hydrochloric acid of solution D to adjust the pH to 3;

[0080] (4) placing the PVDF / HNTs carbonized film prepared in step (2) in the culture dish prepared in step (3), keeping the culture dish away from light, and leaving it at room temperature for 24 hours, a thin layer of polypyrrole will be obtained on the surface of the PVDF / HNTs carbonized film, and a PVDF / HNTs carbonized film @PPy will be obtained; after reacting for 24 hours, the film is taken out, and the excess polypyrrole and excess ions on the surface are washed off with deionized water, and placed in a vacuum drying oven at 45°C for 12 hours;

[0081] (5) Repeat step (1), fix the PVDF / HNTs carbonized membrane @PPy obtained in step (4) on tin foil to spin another layer of PVDF / HNTs electrospinning membrane; set the spinning environment temperature to 25°C, the relative humidity to 40%, and vacuum dry at 60°C for 12h.

[0082] Finally, a double-layer composite diaphragm is obtained, the thickness of which is about 20 μm, and it is cut into fiber diaphragms with a diameter of 19 mm for later use.

[0083] 2. Preparation of positive electrode

[0084] Elemental sulfur, conductive agent superconducting carbon (Super-P), and binder polyvinylidene fluoride (PVDF) are mixed evenly in a mass ratio of 8:1:1 to prepare a lithium-sulfur battery positive electrode slurry with a certain viscosity, the slurry is coated on the current collector aluminum foil, dried at 85°C and then cold pressed; then punching is carried out, and after punching, it is dried at 110°C for 4 hours under vacuum conditions to make a positive electrode sheet.

[0085] 3. Preparation of electrolyte

[0086] A mixed solvent of 1 M lithium bistrifluoromethanesulfonyl imide (LiTFSI) and 0.2 M lithium nitrate (LiNO3) in 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME) (1:1, v / v) was set aside.

[0087] 4. Preparation of lithium-ion batteries

[0088] The positive electrode sheet, composite separator, electrolyte and negative electrode sheet (metal lithium sheet) are assembled into a battery, with the composite separator located between the positive electrode sheet and the negative electrode sheet and the functional layer facing the positive electrode side.

[0089] Example 2

[0090] The only difference from Example 1 is that in step (1) of preparing the precursor solution in Example 2, the mass ratio of PVDF:HNTS is 80:20, and the rest is the same as Example 1.

[0091] Example 3

[0092] The only difference from Example 1 is that in step (1) of preparing the precursor solution in Example 3, the mass ratio of PVDF:HNTS is 90:10, and the rest is the same as Example 1.

[0093] Example 4

[0094] The only difference from Example 1 is that in step (1) of preparing the precursor solution in Example 4, the mass ratio of PVDF:HNTS is 99:1, and the rest is the same as Example 1.

[0095] Example 5

[0096] The only difference from Example 1 is that in step (4) of this Example 5, the reaction time of the PVDF / HNTs carbonized film in the pyrrole solution is 12 hours, and the rest is the same as Example 1.

[0097] Example 6

[0098] The only difference from Example 1 is that in step (4) of this Example 6, the reaction time of the PVDF / HNTs carbonized film in the pyrrole solution is 18 hours, and the rest is the same as Example 1.

[0099] Example 7

[0100] The only difference from Example 1 is that in step (4) of this Example 7, the reaction time of the PVDF / HNTs carbonized film in the pyrrole solution is 30 hours, and the rest is the same as Example 1.

[0101] Comparative Example 1

[0102] The difference from Example 1 is that the composite diaphragm is a base layer + a base layer, and has no functional layer. When preparing the diaphragm, a two-layer PVDF / HNTs single-layer electrospun membrane is directly prepared as the base layer. The rest is the same as Example 1 and will not be repeated.

[0103] Comparative Example 2

[0104] The difference from Example 1 is that the composite diaphragm is a functional layer + a functional layer, without a substrate layer. When preparing the diaphragm, a two-layer PVDF / HNTs carbonized film @PPy is directly prepared as the functional layer. The rest is the same as Example 1 and will not be repeated.

[0105] Comparative Example 3

[0106] The difference from Example 1 is that the functional layer and the base layer do not contain HNTs, when preparing the diaphragm, the precursor solution is a PVDF solution, the PVDF single-layer electrospun membrane is used as the base layer, and the PVDF carbonized membrane @ PPy is used as the functional layer. The rest is the same as Example 1 and will not be repeated.

[0107] Comparative Example 4

[0108] The difference from Example 1 is that PPy is directly grown in situ on the PVDF / HNTS membrane in the functional layer without carbonization, and the rest is the same as Example 1 and will not be described again.

[0109] Comparative Example 5

[0110] The difference from Example 1 is that PPy is not grown in situ on the functional layer, that is, the functional layer does not contain PPy. The rest is the same as Example 1 and will not be described again.

[0111] Lithium-sulfur battery performance test

[0112] Cycle test: Assemble (S / separator / Li) button cells, immerse for 24 hours, and charge and discharge 200 times at a constant current density of 1C using a battery test system from Newwell Electronics Co., Ltd. in a voltage range of 1.7 to 2.8 V. The test results are shown in Table 1.

[0113] Rate test: Assemble (S / diaphragm / Li) button cells, immerse for 24 hours, and use the battery test system of Newwell Electronics Co., Ltd. to perform charge and discharge tests for 5 weeks at rates of 0.2C, 0.5C, 1C, 2C, and 5C in the voltage range of 1.7 to 2.8V. The test results are shown in Table 2.

[0114] Table 1 Discharge capacity of button cell at 0.5C for 200 cycles

[0115]

[0116] Table 2 Specific capacity of button cell at different cycle rates (unit: mAh / g)

[0117]

[0118] It can be seen from Examples 1-4 and Comparative Examples 1 and 3 in Table 1 that after 200 cycles at a rate of 0.5C, Example 1 still has a specific capacity of 1283 mAh / g. This is mainly because the tubular structure of HNTs has polar functional groups. The Si-O tetrahedron on the outer surface and the Al-O octahedron on the inner surface cause the HNTS to present an external negative charge and an internal positive charge, and have good adsorption properties. It can adsorb polysulfides dissolved in the electrolyte, reduce or even avoid the diffusion and migration of dissolved polysulfides to the negative electrode side to undergo side reactions to generate insulating, insoluble Li2S2 and Li2S, which then cover the negative electrode surface, thereby inhibiting the "shuttle effect" of lithium-sulfur batteries.

[0119] By comparing the PVDF / HNTs mass fractions in Examples 1-4 in Table 1, it is found that when the mass fraction of HNTs is greater than 5%, as the mass fraction of HNTs increases, the functional layer will be powdered and fall off during the cycle and lose its original function; and when the mass fraction of HNTs is less than 1%, the effect of HNTs in adsorbing polysulfides decreases.

[0120] It can be seen from Example 1, Examples 5-7 and Comparative Examples 4-5 in Table 1 that whether polypyrrole grows in situ on the surface of the PVDF / HNTs carbonized film affects the adsorption, conversion and utilization of polysulfides by the composite membrane. If the reaction time is too short, it is not conducive to the coating and generation of polypyrrole on the surface of the carbonized fiber; and when the reaction reaches the best, as the reaction time of the PVDF / HNTs carbonized film in the pyrrole solution increases, it will cause the aggregation of polypyrrole and increase the thickness of the membrane, and its effect will be reduced.

[0121] It can be seen from comparative examples 4-5 in Table 1 that polypyrrole needs to cooperate with the highly conductive carbonized film to play an effective role.

[0122] It can be seen from Comparative Example 2 in Table 1 that the functional layer alone cannot be used as a separator, because the functional layer alone has electronic conductivity, which will cause a short circuit between the anode and cathode, making charging and discharging impossible.

[0123] It can be seen from Example 1 and Comparative Example 1 in Table 2 that at 0.2C, 0.5C, 1C, 2C, and 5C rates, the discharge specific capacities of Example 1 are 1586, 1389, 1056, 897, and 643 mAh / g, respectively. Compared with Comparative Example 1, at a rate of 2C, its specific capacity increases by ~660 mAh / g, showing good rate performance.

[0124] Polysulfide adsorption capacity test

[0125] The polysulfide solution was prepared by reacting elemental sulfur and lithium sulfide in a molar ratio of 1:1 in a solvent of 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME) (1:1, v / v). The ability of different membrane samples to adsorb polysulfides was tested (the method for obtaining the samples was referred to Example 1), as shown in Table 3.

[0126] Table 3 The ability of different samples to adsorb polysulfide

[0127]

[0128] As shown in Table 3, the pure PVDF membrane has no adsorption effect on polysulfides. The PVDF / HNTs membrane and PVDF / HNTs carbonized membrane changed from yellow to light yellow at 4h and 12h respectively. This is mainly because HNTs played an adsorption role. Compared with PVDF / HNTs membrane, the PVDF / HNTs carbonized membrane is loose and porous, which is more conducive to the penetration of solvents and can play a role faster. The (PVDF / HNTs carbonized membrane)@PPy gradually turned light yellow at 4h, and the solution color became clear at 12h. It has the best absorption of polysulfides, which further proves the adsorption effect of HNTs and PPy on polysulfides.

[0129] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A lithium-sulfur battery separator, It is characterized in that comprising a base layer and a functional layer disposed on the base layer; Wherein, the base layer comprises a high molecular polymer / halloysite nanotube electrospinning membrane layer; The functional layer includes a halloysite nanotube carbonized film layer and a polypyrrole film layer grown on the surface of the halloysite nanotube carbonized film layer.

2. The lithium-sulfur battery separator according to claim 1, It is characterized in that In the polymer / halloysite nanotube electrospinning membrane layer, the carbon atom content of the polymer is ≥35%; Preferably, the high molecular polymer comprises a fluorocarbon polymer; Preferably, the high molecular polymer includes polyvinylidene fluoride; Preferably, in the high molecular polymer / halloysite nanotube electrospinning membrane layer, the mass fraction of halloysite nanotubes is 1 to 20%, preferably 1 to 5%; Preferably, in the halloysite nanotube carbonized film layer, the mass fraction of the halloysite nanotubes is 1 to 20%, preferably 1 to 5%.

3. The lithium-sulfur battery separator according to claim 1, It is characterized in that The thickness of the base layer is 8 to 10 μm; And / or, the thickness of the functional layer is 8-10 μm.

4. A method for preparing a lithium-sulfur battery separator according to any one of claims 1 to 3, It is characterized in that The method comprises the following steps: preparing a high molecular polymer / halloysite nanotube solution; Preparation of high molecular polymer / halloysite nanotube electrospinning membrane layer by electrospinning process; The high molecular polymer / halloysite nanotube electrospinning membrane layer is subjected to high temperature carbonization treatment to obtain a halloysite nanotube carbonized membrane layer; In-situ growing a polypyrrole film layer on the surface of the halloysite nanotube carbonized film layer to obtain a functional layer; Another layer of high molecular polymer / halloysite nanotube electrospinning membrane is prepared on the functional layer by an electrospinning process as a base layer to obtain the lithium-sulfur battery separator.

5. The method for preparing the lithium-sulfur battery separator according to claim 4, It is characterized in that In the polymer / halloysite nanotube electrospinning membrane layer, the carbon atom content of the polymer is ≥35%; Preferably, the high molecular polymer comprises a fluorocarbon polymer; Preferably, the high molecular polymer includes polyvinylidene fluoride; Preferably, the thickness of the high molecular polymer / halloysite nanotube electrospinning membrane layer is 8-10 μm.

6. The method for preparing a lithium-sulfur battery separator according to claim 4, It is characterized in that In the polymer / halloysite nanotube solution, the mass ratio of polymer to halloysite nanotube is (99:1) to (80:20); Preferably, the mass ratio of high molecular weight polymer to halloysite nanotubes is (99:1) to (95:5).

7. The method for preparing a lithium-sulfur battery according to claim 4, It is characterized in that The specific steps of in-situ growing a polypyrrole film layer on the surface of the halloysite nanotube carbonized film layer to obtain a functional layer include: Mixing appropriate amounts of pyrrole monomer solution, ammonium persulfate solution and ferric chloride solution to prepare a polypyrrole solution; placing the halloysite nanotube carbonized film layer in the polypyrrole solution to allow polypyrrole to grow in situ on the surface of the halloysite nanotube carbonized film layer to form a polypyrrole film layer; After standing at room temperature for a predetermined time, the functional layer is obtained.

8. The method for preparing a lithium-sulfur battery according to claim 7, It is characterized in that Let stand at room temperature for 12 to 48 hours; Preferably, the mixture is allowed to stand at room temperature for 18 to 30 hours.

9. A lithium-sulfur battery, It is characterized in that It comprises the lithium-sulfur battery separator according to any one of claims 1 to 3 or the lithium-sulfur battery separator prepared by the preparation method according to any one of claims 4 to 8.

10. Use of the lithium-sulfur battery separator according to any one of claims 1 to 3 or the lithium-sulfur battery separator prepared by the preparation method according to any one of claims 4 to 8 in preparing energy storage devices, power devices or electronic devices.

Citation Information

Patent Citations

  • Method for preparing manganese dioxide / carbon composite nanotube

    CN106925220A

  • Preparation method of lithium sulfur battery cathode material

    CN109428079A

  • Preparation method of composite lithium-sulfur battery diaphragm material taking polyphenylene sulfide as substrate

    CN115911753A

  • Nanofibrous redox-active separator for lithium-ion battery

    WO2022232901A1