Silver nanowire transparent electromagnetic shielding film and preparation process

By using a double-layer shielding layer composed of silver nanowires and copper nanowire meshes in the electromagnetic shielding film, and adding TiO2 and UV adhesive layers, the problems of insufficient electromagnetic shielding effect and poor light resistance of the existing electromagnetic shielding films are solved. Achieving more efficient electromagnetic shielding and longer service life.

CN118765104APending Publication Date: 2024-10-11CHONGQING XIYU NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410933857.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The electromagnetic shielding effect of existing electromagnetic shielding films is limited, and the common nanometal wire mesh is prone to scattering and photolysis under light irradiation, resulting in high haze and low clarity. The contact area between metal wires is small, resulting in high resistance. , affecting the service life.

Method used

A double-layer electromagnetic shielding layer composed of silver nanowire and copper nanowire grids is used, and the surface is coated with a TiO2 anti-fogging layer and an anti-UV layer, and finally a high-hardness transparent UV glue protective layer is added to improve conductivity and light resistance. .

Benefits of technology

Significantly improves the electromagnetic shielding ability, reduces haze, extends service life, and enhances the stability of the metal shielding layer to avoid photolysis and oxidation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118765104A_ABST
    Figure CN118765104A_ABST
Patent Text Reader

Abstract

The invention discloses a silver nanowire transparent electromagnetic shielding film and a preparation process, and relates to the technical field of electromagnetic shielding films, in particular to a silver nanowire transparent electromagnetic shielding film which comprises a substrate layer, and the inner surface and the outer surface of the substrate layer are coated with a first battery shielding layer and a second battery shielding layer respectively. The first battery shielding layer is an AgNWs grid, the second battery shielding layer is a CuNWs grid, the surfaces of the first battery shielding layer and the second battery shielding layer are coated with fog reducing layers, and the fog reducing layers are TiO2 coatings. According to the silver nanowire transparent electromagnetic shielding film and the preparation process, the electromagnetic shielding capability of the electromagnetic shielding film can be improved by arranging the metal shielding layers composed of the AgNWs grids and the CuNWs grids on the inner surface and the outer surface of the substrate layer, and meanwhile the two metal shielding layers are protected by arranging the protection layers prepared from the UV glue on the inner surface and the outer surface, so that the electromagnetic shielding performance of the electromagnetic shielding film is improved. And the shielding performance of the electromagnetic shielding film is prevented from being degraded or lost due to oxidation of the metal shielding layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electromagnetic shielding films, in particular to a silver nanowire transparent electromagnetic shielding film and a preparation process thereof. Background Art

[0002] Electromagnetic compatibility means that an electronic device neither interferes with other devices nor is affected by other devices. Electromagnetic compatibility, like safety, is one of the most important indicators of product quality. Electromagnetic compatibility involves personal and environmental protection. The interference of electronic components to the outside world is called EMI. Electromagnetic waves will interact with electronic components and cause interference, which is called EMS. Electromagnetic shielding limits power lines or magnetic lines within a certain area in space, so that a certain area is not affected by external power lines and magnetic lines. In order to achieve electromagnetic shielding for a product or a specific area, it is usually achieved by attaching an electromagnetic shielding film to the product or a specific area.

[0003] Currently common battery shielding films usually set an electromagnetic shielding layer on a base material to achieve the electromagnetic shielding function, but this single-layer electromagnetic shielding layer has limited electromagnetic shielding effect, and the common electromagnetic shielding layer is usually composed of a conductive nanometal wire grid. When the incident light is irradiated on the nanometal wire, the light will be scattered, resulting in a larger haze and lower clarity of the electromagnetic shielding film. At the same time, the nanometal wires are overlapped with each other, resulting in a smaller contact area between the metal wires and a larger square resistance. In addition, when the metal wires are coated on the base material and are exposed to ultraviolet rays for a long time, photolysis is easily caused at the connection between the metal wires and the base material, which easily causes the electromagnetic shielding layer to fall off. For this reason, we propose a silver nanowire transparent electromagnetic shielding film and a preparation process to solve the above-mentioned problems. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a silver nanowire transparent electromagnetic shielding film and a preparation process, which solves the problems raised in the above background technology.

[0005] To achieve the above objectives, the present invention is implemented through the following technical scheme: a silver nanowire transparent electromagnetic shielding film, comprising a base layer, the inner and outer surfaces of the base layer are respectively coated with a first battery shielding layer and a second battery shielding layer, the first battery shielding layer is an AgNWs grid, and the second battery shielding layer is a CuNWs grid, the surfaces of the first battery shielding layer and the second battery shielding layer are both coated with a defogging layer, the defogging layer is a TiO2 coating, and the surfaces of the defogging layer are sequentially coated with an anti-ultraviolet layer and a protective layer.

[0006] Preferably, the thickness of the base layer is 5-500 μm, and the material of the base layer is any one of PET, CPI, PC, PDMS, PEN, and PVA.

[0007] Preferably, the first battery shielding layer is prepared by coating silver nanowire ink on the outer surface of the substrate layer, and the thickness of the first battery shielding layer is 10-250 nm.

[0008] Preferably, the second battery shielding layer is prepared by coating copper nanowire ink on the inner surface of the substrate layer, and the thickness of the second battery shielding layer is 10-250 nm.

[0009] Preferably, the anti-fogging layer is prepared by coating a TiO2 precursor solution, and TiO2 can be filled inside the AgNWs and CuNWs grids after coating.

[0010] Preferably, the protective layer is prepared by coating with high-hardness transparent UV glue, and the thickness of the protective layer is 1-100 μm.

[0011] A preparation process of a silver nanowire transparent electromagnetic shielding film comprises the following steps:

[0012] S1. Prepare TiO2 precursor solution: dissolve 0.3g isopropyl titanate in 47.5g deionized water, then add 2.5g hydrogen peroxide, stir magnetically for 30min / 1h at a speed of 400rpm and set aside;

[0013] S2. Coating silver nanowires: Spin-coating the silver nanowire ink evenly on one side of the PET base film, followed by drying in an oven at 120° for 2 min to obtain a PET / AgNWs film;

[0014] S3, coating nano copper wires: using a spin coating method to evenly coat the copper nanowire ink on the other side of the PET base film, and then drying it in an oven at 120° for 2 min to obtain an AgNWs / PET / CuNWs film;

[0015] S4, coating TiO2 precursor solution: drip the TiO2 precursor solution prepared in step 1 on both sides of the AgNWs / PET / CuNWs film, and operate the two sides independently in sequence. After the precursor solution is spread on the surface of the silver nanowire network and the copper nanowire network, spin coating is performed, and then drying is performed in an oven at 120° for 5 minutes to obtain a TiO2 / AgNWs / PET / CuNWs / TiO2 film;

[0016] S5. Coating an anti-ultraviolet layer: Spin-coating a transparent anti-ultraviolet coating on both sides of the TiO2 / AgNWs / PET / CuNWs / TiO2 film, and then drying in an oven at 120° for 5 min to obtain an anti-ultraviolet TiO2 and AgNWs / PET / CuNWs / TiO2 film;

[0017] S6. Coating protective layer: Use spin coating method to coat high hardness UV glue on both sides of anti-ultraviolet TiO2 and AgNWs / PET / CuNWs / TiO2 film, spin coating, and then take out through ultraviolet irradiation for 3 minutes to complete the preparation of the whole electromagnetic shielding film.

[0018] The present invention provides a silver nanowire transparent electromagnetic shielding film and a preparation process, which has the following beneficial effects:

[0019] 1. The silver nanowire transparent electromagnetic shielding film and its preparation process can improve the electromagnetic shielding capability of the electromagnetic shielding film by arranging metal shielding layers composed of AgNWs grids and CuNWs grids on the inner and outer surfaces of the base layer. At the same time, by arranging protective layers prepared by UV glue on the inner and outer surfaces, the two groups of metal shielding layers are protected to prevent the metal shielding layers from being oxidized and causing the shielding performance of the electromagnetic shielding film to be attenuated or lost.

[0020] 2. The silver nanowire transparent electromagnetic shielding film and preparation process, by coating the surface of two sets of metal shielding layers with TiO2 coating, can make the contact between the metal shielding layers closer, increase the area of ​​the metal wire overlap points, reduce the resistance of the overlap points, improve the conductivity of the metal shielding layers, and further improve the electromagnetic shielding capability. At the same time, the TiO2 coating can also increase the absorbance of the metal shielding layer and weaken the ability of the metal shielding layer to scatter light, thereby reducing the haze of the electromagnetic shielding film and improving clarity.

[0021] 3. The silver nanowire transparent electromagnetic shielding film and its preparation process, by coating an anti-ultraviolet layer on the surface of the two metal shielding layers, prevents ultraviolet rays from irradiating the metal shielding layers, avoids photolysis between the metal shielding layers and the base layer, reduces the impact of ultraviolet rays on the electromagnetic shielding film, and increases its service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic diagram of the structure after the overall combination of the present invention;

[0023] Figure 2 It is a schematic diagram of the overall explosion structure of the present invention.

[0024] In the figure: 1. base layer; 2. first battery shielding layer; 3. second battery shielding layer; 4. fog reduction layer; 5. anti-ultraviolet layer; 6. protective layer. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0026] See also Figure 1The present invention provides a technical solution: a silver nanowire transparent electromagnetic shielding film, comprising a substrate 1, the inner and outer surfaces of the substrate 1 are respectively coated with a first battery shielding layer 2 and a second battery shielding layer 3, the first battery shielding layer 2 is an AgNWs grid, and the second battery shielding layer 3 is a CuNWs grid, and by arranging a metal shielding layer composed of an AgNWs grid and a CuNWs grid on the inner and outer surfaces of the substrate 1, the electromagnetic shielding capability of the electromagnetic shielding film can be improved, the surfaces of the first battery shielding layer 2 and the second battery shielding layer 3 are both coated with a defogging layer 4, the defogging layer 4 is a TiO2 coating, and the surface of the defogging layer 4 is sequentially coated with an anti-ultraviolet layer 5 and a protective layer 6, and by arranging a protective layer 6 prepared by UV glue on the inner and outer surfaces, the two groups of metal shielding layers are protected to prevent the metal shielding layers from being oxidized, thereby preventing the shielding performance of the electromagnetic shielding film from being attenuated or lost.

[0027] See also Figure 2 The thickness of the substrate layer 1 is 5-500 μm μm, and the material of the substrate layer 1 is any one of PET, CPI, PC, PDMS, PEN, and PVA. The substrate material is set in the electromagnetic shielding film to ensure the overall strength of the electromagnetic shielding film. The substrate material can be freely selected according to the usage. The first battery shielding layer 2 is prepared by coating the outer surface of the substrate layer 1 with silver nanowire ink, and the thickness of the first battery shielding layer 2 is 10-250 nm. The second battery shielding layer 3 is prepared by coating the inner surface of the substrate layer 1 with copper nanowire ink, and the thickness of the second battery shielding layer 3 is 10-250 nm. By arranging a metal shielding layer composed of AgNWs mesh and CuNWs mesh on the inner and outer surfaces of the substrate layer 1, the electromagnetic shielding ability of the electromagnetic shielding film can be improved. The anti-fog layer 4 is prepared by coating with a TiO2 precursor solution. The TiO2 coating can make the contact between the metal shielding layers closer, increase the area of ​​the metal wire overlap points, reduce the resistance of the overlap points, improve the conductivity of the metal shielding layer, and further improve the electromagnetic shielding capability. After coating, TiO2 can be filled in the AgNWs and CuNWs grids. The TiO2 coating can also increase the absorbance of the metal shielding layer and weaken the ability of the metal shielding layer to scatter light, thereby reducing the haze of the electromagnetic shielding film and improving clarity. The protective layer 6 is prepared by coating with a high-hardness transparent UV glue. The thickness of the protective layer 6 is 1-100μm, which prevents ultraviolet rays from irradiating the metal shielding layer, avoids photolysis between the metal shielding layer and the base layer, reduces the influence of ultraviolet rays on the electromagnetic shielding film, and improves the service life.

[0028] A preparation process of a silver nanowire transparent electromagnetic shielding film comprises the following steps:

[0029] S1. Prepare TiO2 precursor solution: dissolve 0.3g isopropyl titanate in 47.5g deionized water, then add 2.5g hydrogen peroxide, stir magnetically for 30min / 1h at a speed of 400rpm and set aside;

[0030] S2. Coating silver nanowires: Spin coating the silver nanowire ink evenly on one side of the PET base film at 400r / 15s, and then dry it in an oven at 120° for 2min to obtain a PET / AgNWs film;

[0031] S3, coating nano copper wires: using a spin coating method of 400r / 15s to evenly coat the copper nanowire ink on the other side of the PET base film, and then drying it in an oven at 120° for 2min to obtain an AgNWs / PET / CuNWs film;

[0032] S4, coating TiO2 precursor solution: adding the TiO2 precursor solution prepared in step 1 to both sides of the AgNWs / PET / CuNWs film, and the two sides are operated independently in turn. After the precursor solution is spread on the surface of the silver nanowire network and the copper nanowire network, spin coating is performed for 400r / 15s, 800r / 15s, 1200r / 15s, and 1200r / 15s, and the precursor solution is diluted by half with DI, and then dried in an oven at 120° for 5min to obtain a TiO2 / AgNWs / PET / CuNWs / TiO2 film;

[0033] S5. Coating an anti-ultraviolet layer: Spin coating the TiO2 / AgNWs / PET / CuNWs / TiO2 film with a transparent anti-ultraviolet coating on both sides of the film, spin coating at 800r / 15s and 1200r / 15s, and then drying in an oven at 120° for 5min to obtain anti-ultraviolet TiO2 and AgNWs / PET / CuNWs / TiO2 films;

[0034] S6. Coating protective layer: Use the spin coating method to coat high-hardness UV glue on both sides of the anti-ultraviolet TiO2 and AgNWs / PET / CuNWs / TiO2 films. The spin coating process is 1200r / 30s, and then it is taken out through ultraviolet irradiation for 3 minutes to complete the preparation of the entire electromagnetic shielding film.

[0035] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific position, be constructed and operated in a specific position, and therefore cannot be understood as limiting the present invention; the terms "first", "second", and "third" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance. In addition, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be a connection between the two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances. Moreover, the terms "comprises," "comprising," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements but also other elements not expressly listed, or also includes elements inherent to such process, method, article, or apparatus.

[0036] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A silver nanowire transparent electromagnetic shielding film, comprising a base layer (1), characterized in that: The inner and outer surfaces of the base layer (1) are coated with a first battery shielding layer (2) and a second battery shielding layer (3), respectively; the first battery shielding layer (2) is an AgNWs grid, and the second battery shielding layer (3) is a CuNWs grid; the surfaces of the first battery shielding layer (2) and the second battery shielding layer (3) are both coated with a defogging layer (4), the defogging layer (4) is a TiO2 coating, and the surfaces of the defogging layer (4) are coated with an anti-ultraviolet layer (5) and a protective layer (6) in sequence.

2. The silver nanowire transparent electromagnetic shielding film according to claim 1, characterized in that: The thickness of the base layer (1) is 5-500 μm, and the material of the base layer (1) is any one of PET, CPI, PC, PDMS, PEN, and PVA.

3. The silver nanowire transparent electromagnetic shielding film according to claim 1, characterized in that: The first battery shielding layer (2) is prepared by coating silver nanowire ink on the outer surface of the substrate layer (1), and the thickness of the first battery shielding layer (2) is 10-250 nm.

4. The silver nanowire transparent electromagnetic shielding film according to claim 1, characterized in that: The second battery shielding layer (3) is prepared by coating copper nanowire ink on the inner surface of the substrate layer (1), and the thickness of the second battery shielding layer (3) is 10-250 nm.

5. The silver nanowire transparent electromagnetic shielding film according to claim 1, characterized in that: The defogging layer (4) is prepared by coating a TiO2 precursor solution, and after coating, the TiO2 can be filled inside the AgNWs and CuNWs grids.

6. The silver nanowire transparent electromagnetic shielding film according to claim 1, characterized in that: The protective layer (6) is prepared by coating with high-hardness transparent UV glue, and the thickness of the protective layer (6) is 1-100 μm.

7. A process for preparing a silver nanowire transparent electromagnetic shielding film according to any one of claims 1 to 6, characterized in that: The steps include: S1. Prepare TiO2 precursor solution: dissolve 0.3g isopropyl titanate in 47.5g deionized water, then add 2.5g hydrogen peroxide, stir magnetically for 30min / 1h at a speed of 400rpm and set aside; S2. Coating silver nanowires: Spin coating (400r / 15s) the silver nanowire ink evenly on one side of the PET base film, and then dry it in an oven at 120° for 2 min to obtain a PET / AgNWs film; S3, coating nano copper wires: using a spin coating method (400r / 15s) to evenly coat the copper nanowire ink on the other side of the PET base film, and then drying it in an oven at 120° for 2 min to obtain an AgNWs / PET / CuNWs film; S4, coating TiO2 precursor solution: adding the TiO2 precursor solution prepared in step 1 to both sides of the AgNWs / PET / CuNWs film, and the two sides are operated independently in turn. After the precursor solution is spread on the surface of the silver nanowire network and the copper nanowire network, spin coating is performed (400r / 15s, 800r / 15s, 1200r / 15s, 1200r / 15s, and the precursor solution is diluted by DI), and then dried in an oven at 120° for 5 min to obtain a TiO2 / AgNWs / PET / CuNWs / TiO2 film; S5. Coating an anti-ultraviolet layer: Spin coating the TiO2 / AgNWs / PET / CuNWs / TiO2 film with a transparent anti-ultraviolet coating on both sides thereof (800r / 15s, 1200r / 15s), and then drying the film in an oven at 120° for 5 min to obtain an anti-ultraviolet TiO2 and AgNWs / PET / CuNWs / TiO2 film; S6. Coating protective layer: Use the spin coating method to coat high-hardness UV glue on both sides of the anti-ultraviolet TiO2 and AgNWs / PET / CuNWs / TiO2 films, spin coating (1200r / 30s), and then remove it after ultraviolet irradiation for 3 minutes to complete the preparation of the entire electromagnetic shielding film.