Preparation method of positive electrode slurry, secondary battery, battery pack and electric device
Patent Information
- Application Number
- CN202280092933.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-11
- Publication Date
- 2024-10-11
AI Technical Summary
The cathode slurry preparation method in the prior art cannot be applied to binders with different weight average molecular weights, resulting in poor versatility of the slurry mixing process and difficulty in meeting the use needs of high molecular weight binders, and the slurry is prone to gelation, which affects Production efficiency and cost.
A step-by-step slurry mixing process is adopted, including the first stirring, the second stirring, the third stirring and the fourth stirring. By controlling the stirring parameters such as rotation speed, revolution speed and stirring time, the solvent mass ratio is adjusted to prepare a mixture suitable for different weight averages. The positive electrode slurry of molecular weight binder reduces the shipping viscosity and resting viscosity, and alleviates the gelation phenomenon.
It improves the coatability, processability and stability of the cathode slurry, broadens the process window, is suitable for low molecular weight and high molecular weight binders, reduces preparation costs, and is suitable for large-scale production.
Smart Images

Figure CN118765442A_ABST
Abstract
Description
Preparation method of positive electrode slurry, secondary battery, battery pack and electric device Technical Field
[0001] The present application relates to the technical field of secondary batteries, and in particular to a method for preparing a positive electrode slurry for a secondary battery, a secondary battery, a battery pack, and an electrical device. Background Art
[0002] In recent years, as the application scope of secondary batteries has become increasingly wider, secondary batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields.
[0003] Electrode slurry is the basis for forming electrodes and is also the first step in the production of secondary batteries. The characteristics of electrode slurry have a significant impact on subsequent electrode production and battery performance. The positive electrode slurry is mainly a solid-liquid phase mixed system formed by positive electrode active materials, conductive agents, binders and solvents. This system is in a metastable state. The slurrying process, that is, the preparation method of the slurry has a crucial impact on the dispersibility, uniformity, stability and other properties of the slurry. The slurrying process in the prior art is often a one-step method, in which the components in the positive electrode slurry are directly mixed and stirred. However, the one-step preparation method cannot meet the manufacturing requirements of binders with different weight-average molecular weights, and the slurrying process has poor versatility, which is not conducive to reducing manufacturing costs. Therefore, it is necessary to develop a new method for preparing slurry that is suitable for binders with different weight-average molecular weights.
[0004] Summary of the Invention
[0005] The present application is made in view of the above-mentioned problems, and its purpose is to provide a method for preparing a secondary battery positive electrode slurry, which is applicable to binders with different weight-average molecular weights and improves the coating and processability of the slurry.
[0006] In order to achieve the above-mentioned purpose, the present application provides a method for preparing a positive electrode slurry, including first stirring, second stirring, third stirring and fourth stirring; in the first stirring, the conductive agent and the binder are mixed and stirred to prepare a dry mixture; in the second stirring, the solvent and the dry mixture are mixed and stirred to prepare a primary slurry; in the third stirring, the positive electrode active material and the primary slurry are mixed and stirred to prepare a secondary slurry; in the fourth stirring, the solvent is mixed and stirred with the secondary slurry to prepare a positive electrode slurry; the solvent used in the second stirring is the same as the solvent used in the fourth stirring, and based on the total mass of the positive electrode active material, the mass ratio of the solvent used in the second stirring is 35% to 40%, and the mass ratio of the solvent used in the fourth stirring is 5% to 10%.
[0007] Therefore, the preparation method of the positive electrode slurry disclosed in the present application is more widely applicable than the existing preparation method of the positive electrode slurry, and is suitable for slurries containing binders with different weight-average molecular weights. Compared with the existing preparation method, the present application reduces the shipping viscosity of the positive electrode slurry by step-by-step slurry mixing, alleviates the gelation phenomenon of the positive electrode slurry, and improves the applicability of the preparation method for high-molecular-weight binders. The preparation method has wider universality, expands the process window for positive electrode slurry coating, and improves the processing performance of the positive electrode slurry.
[0008] In any embodiment, the binder comprises at least one polyvinylidene fluoride having a weight average molecular weight of 400,000 to 1.8 million.
[0009] The preparation method disclosed in this application is universally applicable to both low-molecular-weight and high-molecular-weight polyvinylidene fluoride binders, effectively alleviating the gelation phenomenon of different slurries, helping to improve production efficiency and broaden the slurry coating window. The preparation method disclosed in this application can be applied to binders with a weight-average molecular weight of up to 1.8 million, allowing slurries containing high-weight-average molecular weight binders to still have low shipping viscosity and anti-gel properties, meeting the use requirements of the new generation of binders.
[0010] In any embodiment, the binder comprises at least two polyvinylidene fluoride having a weight average molecular weight difference of no more than 1.8 million.
[0011] The applicant unexpectedly discovered that the preparation method disclosed in this application can effectively adapt to positive electrode slurries containing binders with various weight-average molecular weights. The positive electrode slurry prepared using the method of this application can effectively utilize the properties of polyvinylidene fluoride binders of different molecular weights. Through the interaction of large and small chain segments and steric hindrance, the slurry has a good gel state. At the same time, the slurry has a low shipping viscosity and a viscosity after standing for 24 hours.
[0012] In any embodiment, the rotation speed of the first stirring is 0.
[0013] Controlling the rotation speed of the first stirring to 0 reduces the shear force of the first stirring, reduces the possibility of excessive breakage of the conductive agent and the binder, ensures that the conductive agent and the binder have a certain particle size and specific surface area, helps to improve the dispersion effect of the conductive agent and the binder, reduces the viscosity of the slurry at delivery and the viscosity after standing for 24 hours, slows down the gelation phenomenon of the slurry, and improves the stability of the slurry.
[0014] In any embodiment, the stirring time of the first stirring is 15 minutes to 30 minutes. The stirring time of the first stirring is within a suitable range, so that the slurry has a low shipping viscosity and a viscosity after standing for 24 hours, so that the slurry has good coating performance, processing performance and stability. At the same time, controlling the stirring time of the first stirring within a suitable range can reduce the working time of slurry preparation, improve the working efficiency of slurry preparation, and reduce costs without significantly changing the shipping viscosity of the slurry, the viscosity of the slurry after standing for 24 hours, and the gelation phenomenon of the slurry.
[0015] In any embodiment, the revolution speed of the first stirring is 10 rpm to 20 rpm. The revolution speed of the first stirring in a suitable range makes the slurry have a low shipping viscosity and a viscosity after standing and storing for 24 hours, so that the slurry has good coating performance, processing performance and stability. At the same time, the revolution speed of the first stirring is controlled within a suitable range. The revolution speed of the first stirring can be controlled to be 10 rpm to 20 rpm without significantly changing the shipping viscosity of the slurry, the viscosity of the slurry after standing for 24 hours, and the gelation phenomenon of the slurry, thereby reducing the power of the agitator, saving energy, and taking into account both the quality and cost of the slurry.
[0016] In any embodiment, the stirring time of the second stirring is 50 to 80 minutes. The stirring time of the second stirring in the appropriate range makes the slurry have a low shipping viscosity and a viscosity after standing for 24 hours, so that the slurry has good coating performance, processing performance and stability. At the same time, controlling the stirring time of the second stirring in the appropriate range can reduce the working time of slurry preparation, improve the working efficiency of slurry preparation, and reduce costs without significantly changing the shipping viscosity of the slurry, the viscosity of the slurry after standing for 24 hours, or the gelation phenomenon of the slurry.
[0017] In any embodiment, the revolution speed of the second stirring is 15 rpm to 30 rpm. The revolution speed of the second stirring in the appropriate range can slow down the gelation of the slurry, improve the stability of the slurry, broaden the process window, and at the same time make the slurry have a low shipping viscosity and a viscosity after standing for 24 hours, so that the slurry has good coating performance and processing performance.
[0018] In any embodiment, the second stirring rotation speed is 800 rpm to 1300 rpm. The second stirring rotation speed in the appropriate range can reduce the viscosity of the slurry before shipment and the viscosity after standing for 24 hours, thereby improving the coating and processability of the slurry.
[0019] In any embodiment, the stirring time of the third stirring is 100 minutes to 130 minutes. The stirring time of the third stirring in a suitable range makes the slurry have a low shipping viscosity and a viscosity after standing for 24 hours, so that the slurry has good coating performance, processing performance and stability. At the same time, controlling the stirring time of the third stirring in a suitable range can reduce the working time of slurry preparation, improve the working efficiency of slurry preparation, and reduce costs without significantly changing the shipping viscosity of the slurry, the viscosity of the slurry after standing for 24 hours, and the gelation phenomenon of the slurry.
[0020] In any embodiment, the revolution speed of the third stirring is 20 rpm to 40 rpm. The revolution speed of the third stirring in the appropriate range can reduce the viscosity of the slurry before shipment and the viscosity after standing for 24 hours, thereby improving the coating and processability of the slurry.
[0021] In any embodiment, the rotation speed of the third stirring is 1000 rpm to 1300 rpm. The rotation speed of the third stirring in the appropriate range can reduce the viscosity of the slurry before shipment and the viscosity after standing for 24 hours, thereby improving the coating and processability of the slurry.
[0022] In any embodiment, the stirring time of the fourth stirring is 30 minutes to 50 minutes. A suitable stirring time of the fourth stirring helps to reduce the viscosity of the slurry before shipment and the viscosity after standing for 24 hours, improves the coating and processability of the slurry, slows down the gelation of the slurry, improves the stability of the slurry, and broadens the process window.
[0023] In any embodiment, the revolution speed of the fourth stirring is 20 rpm to 40 rpm. The revolution speed of the fourth stirring in the appropriate range helps to reduce the viscosity of the slurry when shipped and the viscosity after standing for 24 hours, improves the coating and processability of the slurry, and makes the slurry have good anti-gel properties.
[0024] In any embodiment, the rotation speed of the fourth stirring is 1000 rpm to 1300 rpm. The rotation speed of the fourth stirring in the appropriate range helps to reduce the viscosity of the slurry before shipment and the viscosity after standing for 24 hours, improves the coating and processability of the slurry, and makes the slurry have good anti-gel properties.
[0025] In any embodiment, the mass of the positive electrode active material is 900kg to 1300kg. This preparation method is suitable for industrial mass production of slurry, effectively overcoming the problems of poor raw material batch stability and poor precision encountered in the transition from laboratory production to industrial mass production, and is conducive to improving production efficiency.
[0026] In any embodiment, the mass ratio of the positive electrode active material, the binder, and the conductive agent in the positive electrode slurry is (95-98.5): (1-3): (0.5-1). The positive electrode slurry within the above range has good processing performance and enables the formed positive electrode sheet to have excellent electrochemical performance.
[0027] In any embodiment, the positive electrode active material is one or more of lithium iron phosphate, lithium cobalt oxide, lithium titanate, and lithium nickel cobalt manganese oxide. The above positive electrode active materials give the battery a high energy density, which is beneficial to improving the battery's cycle performance.
[0028] The second aspect of the present application also provides a positive electrode slurry, the solid content of the positive electrode slurry is 65% to 70%, the initial viscosity of the positive electrode slurry is 1000 to 35000 mPa·s, and after the positive electrode slurry is allowed to stand for 24 hours, the viscosity of the positive electrode slurry does not exceed 50000 mPa·s.
[0029] The positive electrode slurry has good processing and storage properties, and can improve production efficiency and broaden the coating process window.
[0030] In any embodiment, the positive electrode slurry is prepared by the preparation method described in the first aspect.
[0031] The third aspect of the present application provides a secondary battery comprising a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte, wherein the positive electrode sheet is prepared from the positive electrode slurry prepared by the preparation method described in the first aspect. The positive electrode sheet has high quality and production efficiency.
[0032] In any embodiment, the secondary battery is any one of a lithium ion battery, a sodium ion battery, a magnesium ion battery, and a potassium ion battery.
[0033] The fourth aspect of the present application further provides a battery module, comprising the secondary battery described in the third aspect of the present application.
[0034] The fifth aspect of the present application provides a battery pack, comprising the secondary battery described in the third aspect of the present application or the battery module described in the fourth aspect of the present application.
[0035] The sixth aspect of the present application provides an electrical device comprising at least one selected from the secondary battery of the third aspect of the present application, the battery module of the fourth aspect of the present application, or the battery pack of the fifth aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] FIG1 is a schematic diagram of a secondary battery according to an embodiment of the present application;
[0037] FIG2 is an exploded view of the secondary battery according to one embodiment of the present application shown in FIG1 ;
[0038] FIG3 is a schematic diagram of a battery module according to an embodiment of the present application;
[0039] FIG4 is a schematic diagram of a battery pack according to an embodiment of the present application;
[0040] FIG5 is an exploded view of the battery pack according to an embodiment of the present application shown in FIG4 ;
[0041] FIG6 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.
[0042] Description of reference numerals:
[0043] 1 battery pack; 2 upper box; 3 lower box; 4 battery module; 5 secondary battery; 51 shell; 52 electrode assembly; 53 cover plate. DETAILED DESCRIPTION
[0044] Below, the embodiments of the positive electrode active material and its manufacturing method, positive electrode sheet, secondary battery, battery module, battery pack and electrical device of the present application are specifically disclosed in detail with appropriate reference to the drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0045] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0046] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0047] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0048] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0049] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0050] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0051] The positive electrode slurry is mainly a solid-liquid phase mixed system formed by the positive electrode active material, conductive agent, binder and solvent. In order to improve the uniformity of the distribution of different components in the system, slurry is often mixed through stirring, ball milling, ultrasound and other processes. However, the slurry mixing process in the prior art is usually only applicable to slurry systems with fixed components, and has poor versatility. After the physical properties of the components in the slurry change, the slurry mixing process often needs to be adjusted. For example, the slurry mixing process in the prior art cannot be applied to high molecular weight binders. The performance of slurries using binders of different molecular weights prepared using the same slurry mixing process in the prior art is greatly different, and the slurry shipment viscosity is high, which makes it difficult to meet the production needs of subsequent electrodes.
[0052] [Preparation of positive electrode slurry]
[0053] Based on this, the present application proposes a method for preparing a positive electrode slurry, including first stirring, second stirring, third stirring and fourth stirring; in the first stirring, the conductive agent and the binder are mixed and stirred to prepare a dry mixture; in the second stirring, the solvent and the dry mixture are mixed and stirred to prepare a primary slurry; in the third stirring, the positive electrode active material and the primary slurry are mixed and stirred to prepare a secondary slurry; in the fourth stirring, the solvent and the secondary slurry are mixed and stirred to prepare a positive electrode slurry; the solvent used in the second stirring is the same as the solvent used in the fourth stirring, and based on the total mass of the positive electrode active material, the mass ratio of the solvent used in the second stirring is 35% to 40%, and the mass ratio of the solvent used in the fourth stirring is 5% to 10%.
[0054] In some embodiments, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0055] In this preparation method, the conductive agent and the binder are first stirred to obtain a dry mix. The first stirring mechanically rivets the two together to form a tight entanglement. The dry mix is then mixed with a solvent and stirred for a second time to obtain a primary slurry. The second stirring helps evenly disperse the binder and the conductive agent in the solvent. In a third stirring process, the positive electrode active material is mixed with the primary slurry to obtain a secondary slurry. The third stirring process helps evenly disperse the positive electrode active material in the primary slurry system and evenly coat and entangle the conductive agent and the binder. In a fourth stirring process, the secondary slurry is mixed with the solvent to obtain a uniform and stable positive electrode slurry that meets both processability and electrical properties. The mass ratio of the solvent used in the second stirring process is 35% to 40%, and the mass ratio of the solvent used in the fourth stirring process is 5% to 10%. Based on the total mass of the positive electrode active material used in the third stirring process, this can effectively reduce the shipping viscosity of the slurry and further adjust the viscosity of the shipping slurry to prevent the shipping viscosity and the viscosity after standing for 24 hours from being too high, which would affect the subsequent coating process.
[0056] If too much or too little solvent is added during the second stirring or the fourth stirring, the viscosity of the slurry after standing for 24 hours cannot be effectively reduced, and the purpose of slowing down the gelation of the slurry cannot be achieved.
[0057] The preparation method of the positive electrode slurry in the prior art has poor compatibility and cannot adapt to the difference in the weight average molecular weight of the binder in the slurry. Therefore, a very high precision requirement is put forward for the material. The present application reduces the shipping viscosity and the viscosity of the positive electrode slurry after standing for 24 hours by adjusting the step-by-step slurry mixing and stirring parameters, alleviates the gelation phenomenon of the positive electrode slurry, and makes the slurry with a high weight average molecular weight binder still have a low shipping viscosity and viscosity and anti-coagulation after standing for 24 hours, thereby improving the universality of the preparation method. The preparation method of the present application is not only applicable to binders with low weight average molecular weight, but also to binders with high weight average molecular weight. It can effectively alleviate the gelation phenomenon of different slurries, help to improve production efficiency, and broaden the process window of slurry coating.
[0058] In some embodiments, the binder comprises at least one polyvinylidene fluoride having a weight average molecular weight of 400,000 to 1.8 million. In some embodiments, the weight average molecular weight of the polyvinylidene fluoride can be any one of 400,000, 450,000, 500,000, 550,000, 600,000, 650,000, 700,000, 750,000, 800,000, 850,000, 900,000, 950,000, 1,000,000, 1,050,000, 1,100,000, 1,150,000, 1,200,000, 1,250,000, 1,300,000, 1,350,000, 1,400,000, 1,450,000, 1,500,000, 1,550,000, 1,600,000, 1,650,000, 1,700,000, 1,750,000, and 1,800,000.
[0059] As used herein, the term "weight average molecular weight" refers to the statistical average molecular weight of a polymer by mass, the molecular weight averaged over a unit weight.
[0060] The existing slurry mixing process is difficult to apply to high-weight-average molecular weight binders. The prepared slurry has a high shipping viscosity, which makes it difficult to meet coating requirements, and the slurry will experience severe gelation. However, the preparation method disclosed in this application can be applied to binders with a weight-average molecular weight of up to 1.8 million, ensuring that the slurry still has a low shipping viscosity and viscosity after standing for 24 hours. The slurry also has good anti-gel properties, which can meet the application requirements of the new generation of high-molecular-weight binders.
[0061] In some embodiments, the binder comprises at least two polyvinylidene fluorides having a weight average molecular weight difference of no more than 1.8 million. In some embodiments, the weight average molecular weight difference of the two or more polyvinylidene fluorides can be any one of 100,000, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,100,000, 1,200,000, 1,300,000, 1,400,000, 1,500,000, 1,600,000, 1,700,000, and 1,800,000.
[0062] The applicant unexpectedly discovered that the preparation method disclosed in this application can effectively adapt to positive electrode slurries containing binders with various weight-average molecular weights. The positive electrode slurry prepared using the method of this application can effectively utilize the properties of polyvinylidene fluoride binders of different molecular weights. Through the mutual coordination of large and small chain segments and steric hindrance, the slurry has a good gel state. At the same time, the slurry has a low shipping viscosity and a viscosity after standing for 24 hours. This preparation method has a wider range of universality.
[0063] In some embodiments, the rotation speed of the first stirring is 0.
[0064] As used herein, the term "rotational speed" refers to the speed at which the agitator rotates about its own axis.
[0065] In some embodiments, the stirring device is a planetary mixer. The operating principle of a planetary mixer is that after the mixer is started, the planetary carrier rotates, driving the stirring shaft inside the box to rotate. The stirring shaft revolves around the axis of the barrel and rotates at high speed, thereby subjecting the material to strong shearing and kneading effects. It is understood that the preparation method provided in this application is applicable to any type of planetary mixer.
[0066] Controlling the rotation speed of the first stirring to 0 reduces the shear force of the first stirring, reduces the risk of excessive crushing of the conductive agent and the binder, ensures that the conductive agent and the binder have a certain particle size and specific surface area, improves the dispersion effect of the conductive agent and the binder, helps to reduce the viscosity of the slurry at delivery and the viscosity after standing for 24 hours, slows down the gelation phenomenon of the slurry, and improves the stability of the slurry.
[0067] In some embodiments, the stirring time of the first stirring is 15 minutes to 30 minutes. In some embodiments, the stirring time of the first stirring can be any one of 15 minutes, 20 minutes, 25 minutes, and 30 minutes.
[0068] If the stirring time of the first stirring is too short, the conductive agent and the binder cannot be effectively mixed, and the viscosity of the slurry when shipped and the viscosity after standing for 24 hours are too large, which cannot meet the production needs; if the stirring time of the first stirring is too long, without significantly improving the viscosity of the slurry when shipped, the viscosity of the slurry after standing for 24 hours, and the gelation phenomenon of the slurry, the long stirring time will lead to energy waste and reduce production efficiency.
[0069] The stirring time of the first stirring is within a suitable range, so that the slurry has a low shipping viscosity and a low viscosity after standing for 24 hours, so that the slurry has good coating performance, processing performance and stability. At the same time, controlling the stirring time of the first stirring within a suitable range can reduce the working time of slurry preparation, improve the working efficiency of slurry preparation, and reduce costs without significantly changing the shipping viscosity of the slurry, the viscosity of the slurry after standing for 24 hours, or the gel phenomenon of the slurry.
[0070] In some embodiments, the revolution speed of the first stirring is 10 rpm to 20 rpm. In some embodiments, the revolution speed of the first stirring is any one of 10 rpm, 15 rpm, and 20 rpm.
[0071] As used herein, the term "revolution speed" refers to the speed at which the agitator rotates around the vessel containing the material.
[0072] If the rotational speed of the first stirring is too low, the conductive agent and the binder cannot be effectively mixed, and the viscosity of the slurry when shipped and the viscosity after standing for 24 hours are too high, which cannot meet the production needs; if the rotational speed of the first stirring is too high, while the viscosity of the slurry when shipped, the viscosity of the slurry after standing for 24 hours, and the gel phenomenon of the slurry cannot be significantly improved, the excessive stirring speed will lead to an increase in the power of the stirrer, resulting in energy waste.
[0073] The revolution speed of the first stirring device within a suitable range enables the slurry to have a low shipping viscosity and a low viscosity after standing for 24 hours, and thus enables the slurry to have good coating performance, processing performance, and stability. At the same time, by controlling the revolution speed of the first stirring device within a suitable range, the revolution speed of the first stirring device can be controlled to be 10 rpm to 20 rpm without significantly changing the shipping viscosity of the slurry, the viscosity of the slurry after standing for 24 hours, or the gelation phenomenon of the slurry, thereby reducing the power of the stirrer, saving energy, and taking into account both the quality and cost of the slurry.
[0074] In some embodiments, the stirring time of the second stirring is 50 minutes to 80 minutes. In some embodiments, the stirring time of the second stirring can be any one of 50 minutes, 60 minutes, 70 minutes, and 80 minutes.
[0075] If the stirring time of the second stirring is too short, the conductive agent and the binder cannot be effectively dispersed in the solvent, and the viscosity of the slurry when shipped and the viscosity after standing for 24 hours are too large, which is not conducive to the stability of the slurry; if the stirring time of the second stirring is too long, without significantly improving the viscosity of the slurry when shipped, the viscosity of the slurry after standing for 24 hours, and the gel phenomenon of the slurry, the long stirring time will lead to energy waste and reduced production efficiency.
[0076] The stirring time of the second stirring within an appropriate range makes the slurry have a low shipping viscosity and a viscosity after standing for 24 hours, so that the slurry has good coating performance, processing performance and stability. At the same time, controlling the stirring time of the second stirring within an appropriate range can reduce the working time of slurry preparation, improve the working efficiency of slurry preparation and reduce costs without significantly changing the shipping viscosity of the slurry, the viscosity of the slurry after standing for 24 hours and the gel state of the slurry.
[0077] In some embodiments, the revolution speed of the second stirring is 15 rpm to 30 rpm. In some embodiments, the revolution speed of the second stirring can be any one of 15 rpm, 20 rpm, 25 rpm, and 30 rpm.
[0078] If the rotational speed of the second stirring is too low, the conductive agent and the binder cannot be effectively dispersed in the solvent, the viscosity of the positive electrode slurry at delivery and after standing for 24 hours are too high, and cannot meet actual needs. In addition, the slurry is prone to gelation. If the rotational speed of the second stirring is too high, the slurry is prone to gelation.
[0079] The revolution speed of the second stirring in the appropriate range can slow down the gelation of the slurry, improve the stability of the slurry, and widen the process window. At the same time, the slurry has a low shipping viscosity and a viscosity after standing for 24 hours, so that the slurry has good coating performance and processing performance.
[0080] In some embodiments, the second stirring rotation speed is 800 rpm to 1300 rpm. In some embodiments, the second stirring rotation speed can be selected from any one of 800 rpm, 900 rpm, 1000 rpm, 1100 rpm, 1200 rpm, and 1300 rpm.
[0081] If the rotation speed of the second stirring is too low or too high, the conductive agent and the binder cannot be effectively dispersed in the solvent, making the viscosity of the slurry too high to meet production needs.
[0082] The rotation speed of the second stirring in the appropriate range can reduce the viscosity of the slurry when it is shipped and the viscosity after standing for 24 hours, thereby improving the coating and processability of the slurry.
[0083] In some embodiments, the stirring time of the third stirring is 100 minutes to 130 minutes. In some embodiments, the stirring time of the third stirring can be any one of 100 minutes, 110 minutes, 120 minutes, and 130 minutes.
[0084] If the stirring time of the third stirring is too short, the positive electrode active material cannot be effectively dispersed in the primary slurry, and the viscosity of the slurry when shipped and the viscosity after standing for 24 hours are too large to meet production needs; if the stirring time of the third stirring is too long, without significantly improving the viscosity of the slurry when shipped, the viscosity of the slurry after standing for 24 hours, and the gel phenomenon of the slurry, the long stirring time will lead to energy waste and reduce production efficiency.
[0085] The stirring time of the third stirring within an appropriate range makes the slurry have low shipping viscosity and viscosity after standing for 24 hours, so that the slurry has good coating performance, processing performance and stability. At the same time, controlling the stirring time of the third stirring within an appropriate range can reduce the working time of slurry preparation, improve the working efficiency of slurry preparation and reduce costs without significantly changing the shipping viscosity of the slurry, the viscosity of the slurry after standing for 24 hours, and the gel phenomenon of the slurry.
[0086] In some embodiments, the revolution speed of the third stirring is 20 rpm to 40 rpm. In some embodiments, the revolution speed of the third stirring can be any one of 20 rpm, 30 rpm, and 40 rpm.
[0087] If the rotational speed of the third stirring is too low, the positive electrode active material cannot be effectively dispersed in the primary slurry, and the viscosity of the slurry when shipped and after standing for 24 hours is too high to meet production needs; if the rotational speed of the third stirring is too high, the positive electrode active material will be easily broken, causing the slurry to easily settle.
[0088] The revolution speed of the third stirring device within a suitable range can reduce the viscosity of the slurry when it is shipped and the viscosity after standing for 24 hours, thereby improving the coating and processability of the slurry.
[0089] In some embodiments, the third stirring rotation speed is 1000 rpm to 1300 rpm. In some embodiments, the third stirring rotation speed can be selected from any one of 1000 rpm, 1100 rpm, 1200 rpm, and 1300 rpm.
[0090] If the rotation speed of the third stirring is too low, the positive electrode active material cannot be effectively dispersed in the primary slurry, and the viscosity of the slurry when shipped and after standing for 24 hours is too high to meet production needs; if the rotation speed of the third stirring is too high, the positive electrode active material will be easily broken, causing the slurry to easily settle.
[0091] The rotation speed of the third stirring device within a suitable range can reduce the viscosity of the slurry when it is shipped and the viscosity after standing for 24 hours, thereby improving the coating and processability of the slurry.
[0092] In some embodiments, the stirring time of the fourth stirring is 30 minutes to 50 minutes. In some embodiments, the stirring time of the fourth stirring can be any one of 30 minutes, 40 minutes, and 50 minutes.
[0093] If the stirring time of the fourth stirring is too short, the solvent cannot be effectively dispersed in the secondary slurry, and the solvent cannot effectively adjust the shipping viscosity of the slurry. The shipping viscosity of the slurry and the viscosity after standing for 24 hours are too large to meet production needs. The slurry is prone to gelation, which is not conducive to the stability of the slurry. If the stirring time of the fourth stirring is too long, it will lead to waste of energy and reduce production efficiency.
[0094] The stirring time of the fourth stirring in the appropriate range helps to reduce the viscosity of the slurry when it is shipped and the viscosity after standing for 24 hours, improve the coating and processability of the slurry, slow down the gelation phenomenon of the slurry, improve the stability of the slurry, and widen the process window.
[0095] In some embodiments, the revolution speed of the fourth stirring is 20 rpm to 40 rpm. In some embodiments, the revolution speed of the fourth stirring is any one of 20 rpm, 30 rpm, and 40 rpm.
[0096] If the rotational speed of the fourth stirring is too low, the solvent cannot be effectively dispersed in the secondary slurry, and the solvent cannot effectively adjust the shipping viscosity of the slurry. The shipping viscosity of the slurry and the viscosity after standing for 24 hours are too large to meet production needs; if the rotational speed of the fourth stirring is too high, the positive electrode active material and conductive agent in the slurry are excessively stirred and easily broken, causing the slurry to easily settle.
[0097] The revolution speed of the fourth stirring device within a suitable range helps to reduce the viscosity of the slurry when it is shipped and the viscosity after standing for 24 hours, improves the coating and processability of the slurry, and makes the slurry have good anti-gel properties.
[0098] In some embodiments, the fourth stirring rotation speed is 1000 rpm to 1300 rpm. In some embodiments, the fourth stirring rotation speed can be any one of 1000 rpm, 1100 rpm, 1200 rpm, and 1300 rpm.
[0099] If the rotation speed of the fourth stirring is too low, the solvent cannot be effectively dispersed in the secondary slurry, and the solvent cannot effectively adjust the shipping viscosity of the slurry. The shipping viscosity and the viscosity after standing for 24 hours of the slurry are too large to meet production needs; if the rotation speed of the fourth stirring is too high, the positive electrode active material and conductive agent in the slurry are excessively stirred and easily broken, causing the slurry to easily settle.
[0100] The rotation speed of the fourth stirring in a suitable range helps to reduce the viscosity of the slurry when it is shipped and the viscosity after standing for 24 hours, improves the coating and processability of the slurry, and makes the slurry have good anti-gel properties.
[0101] In some embodiments, the mass of the positive electrode active material is 900 kg to 1300 kg. In some embodiments, the mass of the positive electrode active material can be selected from any one of 900 kg, 1000 kg, 1100 kg, 1200 kg, and 1300 kg.
[0102] The preparation method is suitable for mass production of slurry, can meet the needs of large-scale production of slurry, and improve production efficiency.
[0103] In some embodiments, the mass ratio of the positive electrode active material, the binder, and the conductive agent in the positive electrode slurry is (95-98.5):(1-3):(0.5-1). In some embodiments, the mass ratio of the positive electrode active material, the binder, and the conductive agent in the positive electrode slurry can be any one of 96.3:3:0.7, 96:3:1, 97:2:1, and 98:1:1.
[0104] The positive electrode slurry within the above range has good processing performance and also enables the formed positive electrode sheet to have excellent electrochemical performance.
[0105] In some embodiments, the solvent used in the second stirring and the solvent used in the fourth stirring can be selected from one or more of N-methyl-2-pyrrolidone, N,N-dimethylpropionamide, N,N-diethylpropionamide, N,N-dipropylpropionamide, N,N-dibutylpropionamide, N,N-dimethylethylpropionamide and 3-butoxy-N-methylpropionamide.
[0106] The above solvents have good solubility for various binders and can effectively disperse various materials such as binders, positive electrode active materials, and conductive agents, which helps to improve the coating quality of the slurry.
[0107] In some embodiments, the positive electrode active material is one or more of lithium iron phosphate, lithium cobaltate, lithium titanate, and lithium nickel cobalt manganese oxide.
[0108] The positive electrode active material enables the battery to have a high energy density, which is beneficial to improving the cycle performance of the battery.
[0109] [Cathode slurry]
[0110] The present application provides a positive electrode slurry, wherein the solid content of the positive electrode slurry is 65% to 70%, the initial viscosity of the positive electrode slurry is 1000 to 35000 mPa·s, and after the positive electrode slurry is allowed to stand for 24 hours, the viscosity of the positive electrode slurry does not exceed 50000 mPa·s.
[0111] The positive electrode slurry has good processing and storage properties, and can improve production efficiency and broaden the coating process window.
[0112] In some embodiments, the positive electrode slurry is prepared by the preparation method in any embodiment of the present application.
[0113] [Positive electrode]
[0114] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector. The positive electrode film layer is prepared from the slurry prepared by the preparation method in any embodiment of the present application.
[0115] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.
[0116] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0117] In some embodiments, the positive electrode active material may adopt the positive electrode active material for batteries known in the art. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.
[0118] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.
[0119] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0120] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and the solvent (such as N-methyl-2-pyrrolidone), are used to prepare the positive electrode slurry using the positive electrode slurry preparation method in any embodiment of the present application, and the positive electrode slurry is coated on the positive electrode current collector. After drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0121] [Negative electrode]
[0122] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0123] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0124] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0125] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0126] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0127] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0128] In some embodiments, the negative electrode film layer may optionally further include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0129] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0130] [Electrolytes]
[0131] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.
[0132] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.
[0133] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0134] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0135] In some embodiments, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0136] [Isolation film]
[0137] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0138] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0139] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.
[0140] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0141] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0142] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG1 shows a secondary battery 5 with a square structure as an example.
[0143] In some embodiments, referring to Figure 2, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0144] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.
[0145] Figure 3 shows an example battery module 4. Referring to Figure 3 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.
[0146] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.
[0147] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.
[0148] Figures 4 and 5 illustrate an example battery pack 1. Referring to Figures 4 and 5 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be placed over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0149] In addition, the present application also provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.
[0150] As the electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.
[0151] Figure 6 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.
[0152] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.
[0153] Example
[0154] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.
[0155] 1. Preparation method
[0156] Example 1
[0157] 1) Preparation of positive electrode slurry
[0158] Weighing raw materials: weighing raw materials according to the positive electrode slurry ratio, the mass ratio of positive electrode active material: binder: conductive agent is 96.3:3:0.7, wherein the positive electrode active material is lithium iron phosphate, the mass of lithium iron phosphate weighed is 900 kg, the binder is polyvinylidene fluoride with a weight average molecular weight of 1.2 million, and the conductive agent is conductive carbon black;
[0159] First stirring: the conductive agent and the binder are mixed and stirred for 20 minutes at a revolution speed of 20 rpm and a rotation speed of 0 to obtain a dry mix;
[0160] Second stirring: adding the above dry mix to N-methyl-2-pyrrolidone solution (NMP) and stirring thoroughly, wherein the mass of the NMP solution is 35% of the mass of the positive electrode active material, the revolution speed is 25 rpm, the rotation speed is 800 rpm, and the stirring time is 60 minutes to obtain a primary slurry;
[0161] Third stirring: adding the positive electrode active material to the primary slurry and stirring thoroughly, wherein the revolution speed is 30 rpm, the rotation speed is 1200 rpm, and the stirring time is 110 minutes to obtain the secondary slurry.
[0162] Fourth stirring: add NMP solution with a mass of 10% of the mass of the positive electrode active material and continue stirring to adjust the viscosity, wherein the revolution speed is 25 rpm, the rotation speed is 1200 rpm, and the stirring time is 30 minutes to obtain the positive electrode slurry.
[0163] Examples 2-3
[0164] The process is basically the same as Example 1, except that the mass fraction of the solvent in the second stirring and the fourth stirring is adjusted. For specific parameters, see Table 1.
[0165] Examples 4 to 6
[0166] The method is basically the same as Example 1, except that the weight average molecular weight of the polyvinylidene fluoride binder is adjusted. For specific parameters, see Table 1.
[0167] Examples 7 to 10
[0168] The results are basically the same as those in Example 1, except that a plurality of binders with different weight-average molecular weights are added. For specific parameters, see Table 1. In Examples 7 to 9, the mass ratio of the first polyvinylidene fluoride to the second polyvinylidene fluoride is 2:1. In Example 10, the mass ratio of the first polyvinylidene fluoride to the second polyvinylidene fluoride to the third polyvinylidene fluoride is 3:2:1.
[0169] Examples 11 to 50
[0170] The process is basically the same as Example 1, except that the stirring parameters are adjusted. For specific parameters, see Table 1.
[0171] Comparative Example 1
[0172] Weighing raw materials: weighing raw materials according to the positive electrode slurry ratio, the mass ratio of positive electrode active material: binder: conductive agent is 96.3:3:0.7, wherein the positive electrode active material is lithium iron phosphate, the mass of lithium iron phosphate weighed is 900 kg, the binder is polyvinylidene fluoride with a weight average molecular weight of 1.2 million, and the conductive agent is conductive carbon black;
[0173] Add the binder to N-methyl-2-pyrrolidone (NMP) solvent and stir thoroughly. The mass of the NMP solution is 35% of the mass of the positive electrode active material. The revolution speed is 25 rpm, the rotation speed is 800 rpm, and the stirring time is 20 minutes to obtain a glue solution.
[0174] Add the conductive agent to the glue solution and stir thoroughly at a revolution speed of 25 rpm and a rotation speed of 1200 rpm for 40 minutes to obtain a primary slurry;
[0175] The positive electrode active material was added to the primary slurry and stirred thoroughly at an orbital speed of 30 rpm, an autorotational speed of 1200 rpm, and a stirring time of 110 minutes to obtain a secondary slurry.
[0176] Add 10% of the mass of the positive electrode active material to the NMP solution and continue stirring to adjust the viscosity at a revolution speed of 25 rpm and a rotation speed of 1200 rpm for 30 minutes to obtain a positive electrode slurry;
[0177] Comparative Examples 2-3
[0178] It is basically the same as Comparative Example 1, except that the weight average molecular weight of polyvinylidene fluoride is 400,000 and 800,000 respectively. For specific parameters, see Table 1.
[0179] Comparative Examples 4-5
[0180] The process is basically the same as Example 1, except that the mass fraction of the solvent in the second stirring and the fourth stirring is adjusted. For specific parameters, see Table 1.
[0181] 2. Slurry property test
[0182] 1. Viscosity test of slurry shipment
[0183] The prepared positive electrode slurry was allowed to stand for 10 minutes before being shipped. The viscosity value initially measured using a Brookfield Dveslvtjo rotary viscometer was recorded as the shipping viscosity. The test conditions were: 25°C, 12 rpm, a 64-spindle for measuring slurry viscosities of 2000 mPa·s or higher, and a 62-spindle for measuring slurry viscosities of less than 2000 mPa·s. Three replicate measurements were performed, and the average value was taken.
[0184] 2. Viscosity test of the slurry after standing for 24 hours
[0185] After standing for 24 hours, the slurry was retested for viscosity. The viscosity value measured using a Brookfield Dveslvtjo rotary viscometer was recorded as the 24-hour viscosity. The test conditions were: 25°C, 12 rpm, a 64-spindle for measuring slurry viscosities of 2000 mPa·s or higher, and a 62-spindle for measuring slurry viscosities of less than 2000 mPa·s. Three replicate measurements were performed, and the average value was calculated.
[0186] 3. Gel state test after the slurry has been allowed to stand for 24 hours
[0187] After the slurry has been allowed to stand for 24 hours, use a steel ruler to pick up the slurry in the beaker and judge whether the slurry is non-gel, slightly gelled, moderately gelled, or severely gelled based on the flow state of the slurry.
[0188] Non-gel state: the slurry flows naturally and continuously, and the slurry flows flat on the surface of the steel ruler without agglomeration;
[0189] Slight gel state: The slurry flows naturally and continuously, but the fluid is thin and the slurry is basically spread evenly on the surface of the steel ruler with slight small lumps;
[0190] Moderate gel state: The slurry drips naturally and intermittently; it does not flow continuously, and the slurry cannot be spread evenly on the surface of the steel ruler, with obvious block agglomerations;
[0191] Severe gel state: The slurry cannot flow down in a stream, falls into lumps or remains directly on the steel ruler and cannot flow down.
[0192] Table 1 Preparation parameters and performance tests in Examples and Comparative Examples
[0193]
[0194]
[0195]
[0196] 3. Analysis of test results of various embodiments and comparative examples
[0197] The positive electrode slurries of the embodiments and comparative examples were prepared according to the above method, and various parameters were measured. The results are shown in Table 1 below.
[0198] According to the results in Table 1, the positive electrode slurries in Examples 1 to 50 are all prepared by the slurry preparation method disclosed in the present application, including first stirring, second stirring, third stirring and fourth stirring; in the first stirring, the conductive agent and the binder are mixed and stirred to prepare a dry mixture; in the second stirring, the solvent and the dry mixture are mixed and stirred to prepare a primary slurry; in the third stirring, the positive electrode active material and the primary slurry are mixed and stirred to prepare a secondary slurry; in the fourth stirring, the solvent and the secondary slurry are mixed and stirred to prepare a positive electrode slurry; the solvent used in the second stirring is the same as the solvent used in the fourth stirring, and based on the total mass of the positive electrode active material, the mass ratio of the solvent used in the second stirring is 35% to 40%, and the mass ratio of the solvent used in the fourth stirring is 5% to 10%.
[0199] From the comparison of Examples 1 to 10 with Comparative Examples 1 to 3, it can be seen that the preparation method disclosed in the present application has wide versatility and is applicable to slurries of one or more polyvinylidene fluoride binders with a weight average molecular weight of 400,000 to 1.8 million. The preparation method is universal for low weight average molecular weight polyvinylidene fluoride binders and high weight average molecular weight polyvinylidene fluoride binders, which helps to reduce preparation costs and improve production efficiency.
[0200] As can be seen from Comparative Example 1, the prior art preparation process is unable to reduce the shipping viscosity of the slurry for a binder with a weight-average molecular weight of 1.2 million. The viscosity of the slurry even exceeds the measuring range after standing for 24 hours, and the slurry will experience severe gelation. As can be seen from Example 6, the preparation method disclosed in this application enables a slurry containing a binder with a weight-average molecular weight of up to 1.8 million to still have low shipping viscosity and viscosity after standing for 24 hours. The slurry also has good anti-gel properties, which can meet the use requirements of the new generation of high molecular weight binders.
[0201] As shown in Examples 7-10, this application is also applicable to slurries containing at least two polyvinylidene fluoride binders with a weight-average molecular weight difference of no more than 1.8 million. The slurries prepared using the method of this application have low shipping viscosity and viscosity after standing for 24 hours, as well as good anti-gel properties. Compared to existing preparation methods, this method has wider applicability.
[0202] From the comparison of Examples 1 to 3 with Comparative Examples 4 to 5, it can be seen that controlling the mass ratio of the solvent used in the second stirring to be 35% to 40%, and the mass ratio of the solvent used in the fourth stirring to be 5% to 10%, based on the total mass of the positive electrode active material, helps to reduce the viscosity of the slurry after standing for 24 hours, can effectively alleviate the gelation of the slurry, improve the storage performance of the slurry, and broaden the process window of the slurry coating.
[0203] From the comparison between Example 1 and Examples 11 to 12, it can be seen that controlling the rotation speed of the first stirring to 0 helps to reduce the viscosity of the positive electrode slurry at delivery and the viscosity after standing for 24 hours, slows down the gelation phenomenon of the slurry, improves the stability of the slurry, and widens the process window.
[0204] From the comparison of Example 1, Examples 14-15 and Example 13, it can be seen that controlling the stirring time of the first stirring to 15 minutes to 30 minutes can reduce the shipping viscosity of the slurry and the viscosity after standing for 24 hours, improve the coating and processability of the slurry, and make the slurry have good anti-gel properties. From the comparison of Example 1, Examples 14-15 and Example 16, it can be seen that controlling the stirring time of the first stirring to 15 minutes to 30 minutes without significantly changing the shipping viscosity of the slurry, the viscosity of the slurry after standing for 24 hours, and the gel phenomenon of the slurry can reduce the working time of slurry preparation, improve the working efficiency of slurry preparation, reduce costs, and can take into account both the quality and efficiency of the slurry.
[0205] From the comparison between Example 1, Examples 18 to 19 and Example 17, it can be seen that controlling the revolution speed of the first stirring to 10 rpm to 20 rpm can reduce the shipping viscosity of the slurry and the viscosity after standing for 24 hours, and improve the coating and processability of the slurry. From the comparison between Example 1, Examples 18 to 19 and Example 20, it can be seen that without significantly changing the shipping viscosity of the slurry, the viscosity of the slurry after standing for 24 hours, and the gelation phenomenon of the slurry, controlling the revolution speed of the first stirring to 10 rpm to 20 rpm can reduce the power of the agitator, save energy, and take into account both the quality and cost of the slurry.
[0206] Comparison of Example 1, Examples 22-23, and Example 21 shows that controlling the second stirring time to 50-80 minutes helps reduce the slurry's shipping viscosity and viscosity after standing for 24 hours, improves the slurry's coating and processability, and imparts good anti-gel properties to the slurry. Comparison of Example 1, Examples 22-23, and Example 24 shows that controlling the second stirring time to 50-80 minutes, without significantly changing the slurry's shipping viscosity, viscosity after standing for 24 hours, or gelation, can reduce slurry preparation time, improve slurry preparation efficiency, and reduce costs.
[0207] From the comparison between Example 1, Examples 26 to 27 and Examples 25 and 28, it can be seen that controlling the revolution speed of the second stirring to 15 rpm to 30 rpm helps to reduce the shipping viscosity of the positive electrode slurry and the viscosity after standing for 24 hours, improves the coating and processability of the slurry, and can also slow down the gelation phenomenon of the slurry, improve the stability of the slurry, and widen the process window.
[0208] From the comparison between Example 1, Examples 30-31 and Example 29, it can be seen that controlling the rotation speed of the second stirring to 800 rpm-1300 rpm can reduce the shipping viscosity of the slurry and the viscosity after standing for 24 hours, and improve the coating and processability of the slurry.
[0209] From the comparison of Example 1, Examples 33-34, and Example 32, it can be seen that controlling the stirring time of the third stirring to 100 minutes to 130 minutes can reduce the shipping viscosity of the slurry and the viscosity after standing for 24 hours, thereby improving the coating and processability of the slurry. From the comparison of Example 1, Examples 33-34, and Example 35, it can be seen that controlling the stirring time of the third stirring to 100 minutes to 130 minutes without significantly changing the shipping viscosity of the slurry, the viscosity of the slurry after standing for 24 hours, or the gelation phenomenon of the slurry can reduce the working time of slurry preparation, improve the working efficiency of slurry preparation, and reduce costs.
[0210] From the comparison between Example 1, Examples 37 to 38 and Example 36, it can be seen that controlling the revolution speed of the third stirring to 20 rpm to 40 rpm can reduce the shipping viscosity of the slurry and the viscosity after standing for 24 hours, thereby improving the coating and processability of the slurry.
[0211] From the comparison between Example 1, Examples 40 to 41 and Example 39, it can be seen that controlling the rotation speed of the third stirring to 1000 rpm to 1300 rpm can reduce the shipping viscosity of the slurry and the viscosity after standing for 24 hours, thereby improving the coating and processability of the slurry.
[0212] From the comparison between Example 1, Examples 43 to 44 and Example 42, it can be seen that controlling the stirring time of the fourth stirring to 30 minutes to 50 minutes helps to reduce the shipping viscosity of the slurry and the viscosity after standing for 24 hours, improves the coating and processability of the slurry, slows down the gelation phenomenon of the slurry, improves the stability of the slurry, and widens the process window.
[0213] From the comparison between Example 1, Examples 46 to 47 and Example 45, it can be seen that controlling the revolution speed of the fourth stirring to 20 rpm to 40 rpm helps to reduce the shipping viscosity of the slurry and the viscosity after standing for 24 hours, improves the coating and processability of the slurry, and makes the slurry have good anti-gel properties.
[0214] From the comparison between Example 1, Examples 49 to 50 and Example 48, it can be seen that controlling the rotation speed of the third stirring to 1000 rpm to 1300 rpm helps to reduce the shipping viscosity of the slurry and the viscosity after standing for 24 hours, improves the coating and processability of the slurry, and makes the slurry have good anti-gel properties.
[0215] The slurries of Examples 1 to 50 contained 900 kg to 1300 kg of positive electrode active material, demonstrating that the preparation method is suitable for large-scale slurry production. Currently available preparation methods incorporate low amounts of material, making them suitable only for laboratory preparation and difficult to adapt to industrial production. The method disclosed in this application overcomes the challenges of multiple raw material batches, poor dispersion, and low precision associated with transitioning from laboratory preparation to large-scale production, thereby improving the production efficiency of positive electrode slurries.
[0216] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A method for preparing a positive electrode slurry, characterized in that: including first stirring, second stirring, third stirring and fourth stirring; In the first stirring, the conductive agent and the binder are mixed and stirred to prepare a dry mix; In the second stirring, the solvent and the dry mix are mixed and stirred to prepare a primary slurry; In the third stirring, the positive electrode active material is mixed and stirred with the primary slurry to prepare a secondary slurry; In the fourth stirring, the solvent is mixed and stirred with the secondary slurry to prepare a positive electrode slurry; The solvent used in the second stirring is the same as the solvent used in the fourth stirring. Based on the mass of the positive electrode active material, the mass ratio of the solvent used in the second stirring is 35% to 40%, and the mass ratio of the solvent used in the fourth stirring is 5% to 10%.
2. The method for preparing the positive electrode slurry according to claim 1, wherein: The binder comprises at least one polyvinylidene fluoride having a weight average molecular weight of 400,000 to 1.8 million.
3. The method for preparing the positive electrode slurry according to claim 1 or 2, characterized in that: The binder comprises at least two polyvinylidene fluoride having a weight average molecular weight difference of no more than 1.8 million.
4. The method for preparing a positive electrode slurry according to any one of claims 1 to 3, characterized in that: The rotation speed of the first stirring is 0.
5. The method for preparing a positive electrode slurry according to any one of claims 1 to 4, characterized in that: The stirring time of the first stirring is 15 minutes to 30 minutes.
6. The method for preparing a positive electrode slurry according to any one of claims 1 to 5, characterized in that: The revolution speed of the first stirring is 10 rpm to 20 rpm.
7. The method for preparing a positive electrode slurry according to any one of claims 1 to 6, characterized in that: The second stirring time is 50 to 80 minutes.
8. The method for preparing a positive electrode slurry according to any one of claims 1 to 7, characterized in that: The revolution speed of the second stirring is 15 rpm to 30 rpm.
9. The method for preparing a positive electrode slurry according to any one of claims 1 to 8, characterized in that: The second stirring rotation speed is 800 rpm to 1300 rpm.
10. The preparation method according to any one of claims 1 to 9, characterized in that The stirring time of the third stirring is 100 minutes to 130 minutes.
11. The preparation method according to any one of claims 1 to 10, characterized in that The revolution speed of the third stirring is 20 rpm to 40 rpm.
12. The preparation method according to any one of claims 1 to 11, characterized in that The rotation speed of the third stirring is 1000 rpm to 1300 rpm.
13. The preparation method according to any one of claims 1 to 12, characterized in that The stirring time of the fourth stirring is 30 minutes to 50 minutes.
14. The preparation method according to any one of claims 1 to 13, characterized in that The revolution speed of the fourth stirring is 20 rpm to 40 rpm.
15. The preparation method according to any one of claims 1 to 14, characterized in that The rotation speed of the fourth stirring is 1000 rpm to 1300 rpm.
16. The preparation method according to any one of claims 1 to 15, characterized in that The mass of the positive electrode active material is 900kg to 1300kg; 17. The preparation method according to any one of claims 1 to 16, characterized in that In the positive electrode slurry, the mass ratio of the positive electrode active material, the binder, and the conductive agent is (95-98.5):(1-3):(0.5-1). 18 . The preparation method according to claim 1 , wherein the positive electrode active material is one or more of lithium iron phosphate, lithium cobaltate, lithium titanate, and lithium nickel cobalt manganese oxide.
19. A positive electrode slurry, characterized in that: The positive electrode slurry has a solid content of 65% to 70%, an initial viscosity of the positive electrode slurry is 1000 to 35000 mPa·s, and after the positive electrode slurry is left to stand for 24 hours, the viscosity of the positive electrode slurry does not exceed 50000 mPa·s.
20. The positive electrode slurry according to claim 19, characterized in that The positive electrode slurry is prepared by the positive electrode slurry preparation method according to any one of claims 1 to 18.
21. A secondary battery, characterized in that: The invention comprises a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte, wherein the positive electrode sheet is prepared by the positive electrode slurry prepared by the positive electrode slurry preparation method according to any one of claims 1 to 18.
22. The secondary battery according to claim 21, wherein The secondary battery is any one of a lithium ion battery, a sodium ion battery, a magnesium ion battery, and a potassium ion battery.
23. A battery module, characterized in that: Includes the secondary battery according to claim 21 or 22.
24. A battery pack, characterized in that: The invention comprises at least one of the secondary battery according to claim 21 or 22 and the battery module according to claim 23.
25. An electrical device, characterized in that: The battery comprises at least one selected from the secondary battery according to claim 21 or 22, the battery module according to claim 23, or the battery pack according to claim 24.