Filter element for simulating tianshan characteristic mineral water, preparation method of filter element and water purifier
By combining materials such as modified granite, dolomite, basalt and tuff, combined with pickled coconut shell activated carbon and polyethylene, a mineral water filter element simulating Tianshan characteristics is prepared, which solves the problem of mineral loss in traditional water purification technology and achieves rich The production of mineral-containing drinking water meets the needs of high-quality life.
Patent Information
- Application Number
- CN202310349203.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-15
AI Technical Summary
When existing water purification technology removes impurities from water, it leads to the loss of minerals in the water, which cannot meet the human body's demand for minerals. Moreover, the water quality that simulates the characteristic mineral water of Tianshan is difficult to achieve through traditional methods.
Modified granite, modified dolomite, modified basalt and modified tuff are used as filter element materials. Through specific modification treatments and combinations, combined with pickled coconut shell activated carbon and polyethylene, a filter element that simulates the characteristic mineral water of Tianshan Mountains is prepared. It can process municipal tap water into mineral-rich drinking water in a water purifier, and the water quality is close to Tianshan mineral water.
It is possible to produce drinking water consistent with Tianshan characteristic mineral water in a small water quality processor to meet the needs of high-quality life. The water tastes good and is rich in minerals, which can meet the human body's demand for minerals.
Smart Images

Figure CN118767541A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of drinking water, and in particular to a filter element simulating the characteristic mineral water of Tianshan Mountain, a preparation method thereof, and a water purifier. Background Art
[0002] With the improvement of living standards, people's requirements for drinking water are getting higher and higher. Since municipal tap water and some centralized water supply cannot meet the needs of users, many urban communities have installed commercial water stations to provide direct drinking water, and some families choose to install household water purifiers to solve the drinking water problem. However, both commercial water stations and household water purifiers use filtration technology to remove impurities in water to achieve the purpose of safe drinking water. Although this technology can ensure the safety of water quality, it also removes the minerals necessary for the human body in the water while removing impurities, and cannot meet the normal human body's needs for minerals.
[0003] Natural mineral water is the only way to better meet the demand. For example, the Tianshan Mountains have excellent water sources. Most of the natural mineral water they have not only tastes good but is also rich in minerals. However, due to its special geographical environment, it is not only extremely difficult to mine, but also has extremely high mining and transportation costs. At present, although there are a small amount of mined water sources, due to long-term storage and transportation, the transported water has lost many of its original excellent factors, which greatly affects the user experience.
[0004] Therefore, simulating the water quality evolution process of Tianshan characteristic mineral water and producing drinking water with the same quality as Tianshan characteristic mineral water through a small household water quality processor is of great significance for people's high-quality life requirements. Summary of the invention
[0005] In view of this, the present application provides a filter element and a preparation method and a water purifier that simulates Tianshan characteristic mineral water, aiming to produce drinking water with the same quality as Tianshan characteristic mineral water through a small water quality processor.
[0006] The embodiment of the present application is implemented as follows:
[0007] In a first aspect, the present application provides a filter element for simulating Tianshan characteristic mineral water, comprising modified granite, modified dolomite, modified basalt and modified tuff.
[0008] Optionally, in some embodiments of the present application, the filter element comprises, by weight, 10 to 20 parts of modified granite, 10 to 30 parts of modified dolomite, 10 to 20 parts of modified basalt and 5 to 10 parts of modified tuff; and / or,
[0009] The modified dolomite comprises hydrated carbonate compounds, and the cations in the hydrated carbonate compounds comprise calcium ions and magnesium ions; and / or,
[0010] The modified granite is immersed in pure water of equal mass at 20 to 30° C. for 23 to 25 hours to precipitate sodium ions, potassium ions and metasilicate ions, and in the immersion water corresponding to 20 g of the modified granite, the concentration of the sodium ions is 16 to 28 mg / L, the concentration of the potassium ions is 2.2 to 3.9 mg / L, and the concentration of the metasilicate ions is 2.5 to 8 mg / L; and / or,
[0011] The pure water filtered by the modified dolomite contains calcium ions and magnesium ions. Under the condition that the flow rate of the water is 1.9 to 2.1 L / min, the concentration of the calcium ions in the filtered water corresponding to 10 g of the modified dolomite is 3 to 18 mg / L, and the concentration of the magnesium ions is 2 to 10 mg / L; and / or,
[0012] The modified basalt is immersed in pure water at 20 to 30° C. for 23 to 25 hours to precipitate metasilicate ions, and the concentration of the metasilicate ions in the immersed water corresponding to 5 g of the modified basalt is 13.5 to 33.5 mg / L; and / or,
[0013] The modified tuff contains strontium element, and the mass percentage of the strontium element is 42% to 50.5%.
[0014] Optionally, in some embodiments of the present application, the particle size of the modified granite is less than or equal to 35 mesh and greater than 200 mesh; and / or,
[0015] The particle size of the modified dolomite is less than or equal to 80 mesh and greater than 325 mesh; and / or,
[0016] The particle size of the modified basalt is less than or equal to 325 mesh and greater than 1000 mesh; and / or,
[0017] The particle size of the modified tuff is less than or equal to 35 meshes and greater than 200 meshes.
[0018] Optionally, in some embodiments of the present application, the filter element further comprises 30 to 60 parts of acid-washed coconut shell activated carbon and 30 to 60 parts of polyethylene, calculated by weight.
[0019] Optionally, in some embodiments of the present application, the particle size of the acid-washed coconut shell activated carbon is 35 to 1000 mesh; and / or,
[0020] The molecular weight of the polyethylene is greater than or equal to 5 million.
[0021] Optionally, in some embodiments of the present application, the water filtered by the filter element meets the following standards: strontium content is 0.2-1.2 mg / L, calcium content is 10.0-48.0 mg / L, potassium content is 0.5-1.5 mg / L, magnesium content is 4.0-18.0 mg / L, sodium content is 6.0-35.0 mg / L, TDS value is 50.0-280.0 mg / L, orthosilicic acid content is greater than or equal to 25 mg / L, and pH is 7.3-8.3.
[0022] In a second aspect, the present application also proposes a method for preparing a filter element simulating Tianshan characteristic mineral water, comprising the following steps:
[0023] After heating natural granite at 400-600°C, it is placed in a sodium salt solution and cooled to obtain modified granite;
[0024] The natural dolomite is heated in a mixed gas of carbon dioxide and water vapor to form hydrated carbonate compounds, thereby obtaining modified dolomite;
[0025] The natural basalt is soaked in acid and ultrasonicated, and then heated at 800°C to 900°C to obtain modified basalt;
[0026] The natural tuff is heated at 400-500°C and then modified with sulfuric acid to obtain modified tuff;
[0027] Mix various raw materials and shape them into filter elements;
[0028] The plurality of raw materials include the modified granite, the modified dolomite, the modified basalt and the modified tuff.
[0029] Optionally, in some embodiments of the present application, the molar concentration of sodium ions in the sodium salt solution is 2 to 5 mol / L; and / or,
[0030] In the step of heating the natural dolomite in a mixed gas of carbon dioxide and water vapor to form hydrated carbonate compounds, the heating temperature is 400-650° C.; and / or,
[0031] In the mixed gas of carbon dioxide and water vapor, the volume ratio of the carbon dioxide to the water vapor is (1.5-2.5):1; and / or,
[0032] The acid comprises a hydrochloric acid solution with a concentration of 1 to 4 mol / L; and / or,
[0033] The concentration of the sulfuric acid is 1 to 3 mol / L; and / or,
[0034] Calculated by weight, the plurality of raw materials include 10 to 20 parts of the modified granite, 10 to 30 parts of the modified dolomite, 10 to 20 parts of the modified basalt and 5 to 10 parts of the modified tuff.
[0035] Optionally, in some embodiments of the present application, the filter element further comprises 30 to 60 parts of acid-washed coconut shell activated carbon and 30 to 60 parts of polyethylene, calculated by weight.
[0036] In a third aspect, the present application further proposes a water purifier, comprising a filter element, wherein the filter element comprises the filter element described above, or the filter element is prepared by the preparation method described above.
[0037] The technical solution provided in the present application comprises a filter element including modified granite, modified dolomite, modified basalt and modified tuff. The filter element can provide rich minerals and adjust the pH value of raw water, and mineralize the RO pure water passing through the filter element into drinking water rich in strontium, calcium, potassium, magnesium, sodium and orthosilicic acid. The water quality of the drinking water is similar to that of the characteristic mineral water of Tianshan Mountain. It not only tastes good, but is also rich in minerals, and can meet people's high-quality life requirements. By applying it to a water purifier, ordinary municipal tap water or centralized water supply can be processed into drinking water with the same water quality as the characteristic mineral water of Tianshan Mountain. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0039] Figure 1 It is a schematic flow chart of a method for preparing a filter element proposed in an embodiment of the present application;
[0040] Figure 2 This is an electron microscope image of natural granite;
[0041] Figure 3 This is an electron microscope image of modified granite;
[0042] Figure 4 It is a schematic diagram of the structure of the water purifier proposed in the embodiment of the present application;
[0043] Figure numbers: 100-purification module; 200-mineralization module; 1-water inlet; 2-PP cotton filter element; 3-low-pressure switch; 4-water inlet solenoid valve; 5-granular activated carbon filter element; 6-scale-inhibiting carbon rod filter element; 7-boosting pump; 8-RO reverse osmosis filter element; 9-high-pressure switch; 10-wastewater ratio solenoid valve; 11-filter element simulating Tianshan characteristic mineral water; 12-sterilization taste filter element; 13-water outlet; 14-control panel. DETAILED DESCRIPTION
[0044] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.
[0045] In this application, unless otherwise specified, the directional words used, such as "upper" and "lower", refer specifically to the directions of the drawings in the accompanying drawings. In addition, in the description of the specification of this application, the term "including" means "including but not limited to".
[0046] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0047] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.
[0048] In the present application, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0049] The technical solution of this application is implemented as follows:
[0050] In a first aspect, the present application provides a filter element for simulating Tianshan characteristic mineral water, comprising modified granite, modified dolomite, modified basalt and modified tuff.
[0051] The technical solution provided in the present application comprises a filter element including modified granite, modified dolomite, modified basalt and modified tuff. The filter element can provide rich minerals and adjust the pH value of raw water, and mineralize the RO pure water passing through the filter element into drinking water rich in strontium, calcium, potassium, magnesium, sodium and orthosilicic acid. The water quality of the drinking water is similar to that of the characteristic mineral water of Tianshan Mountain. It not only tastes good, but is also rich in minerals, and can meet people's high-quality life requirements. By applying it to a water purifier, ordinary municipal tap water or centralized water supply can be processed into drinking water with the same water quality as the characteristic mineral water of Tianshan Mountain.
[0052] In some embodiments of the present application, the filter element includes 10-20 parts of modified granite, 10-30 parts of modified dolomite, 10-20 parts of modified basalt and 5-10 parts of modified tuff, measured by weight. It can be understood that the filter element can adopt any combination of modified granite, modified dolomite, modified basalt and modified tuff within the above range. For example, the filter element may include 10-12 parts of modified granite, 20-30 parts of modified dolomite, 10-15 parts of modified basalt and 8-10 parts of modified tuff; it may also include 11-15 parts of modified granite, 10-20 parts of modified dolomite, 15-20 parts of modified basalt and 5-8 parts of modified tuff; it may also include 15-20 parts of modified granite, 15-25 parts of modified dolomite, 12-18 parts of modified basalt and 7-9 parts of modified tuff. Limiting the combination of modified granite, modified dolomite, modified basalt and modified tuff in the above-mentioned proportions can, on the one hand, allow the pure water to reach the water quality characteristics of Tianshan mineral water after filtration through the filter element, and on the other hand, can also control the sanitary safety indicators such as heavy metals in the effluent water to be within a reasonable range.
[0053] The modified granite refers to a product formed after natural granite is modified, and the purpose of the modification treatment includes increasing the sodium content in the ore and increasing the precipitation amount of potassium and metasilicate. In some embodiments, the modified granite (20g) obtained after the modification treatment is placed in pure water (obtained by RO membrane treatment) of room temperature (20-30°C) equal to its mass and soaked for 23-25h, then the modified granite is taken out, and the ion types and concentrations in the soaking water are detected. The soaking water contains at least sodium ions, potassium ions and metasilicate ions, and the contents of these three ions meet the following standards: the concentration of the sodium ions is 16-28mg / L, the concentration of the potassium ions is 2.2-3.9mg / L, and the concentration of the metasilicate ions is 2.5-8mg / L. For example, the concentration of sodium ions in the immersion water can be 16 mg / L, 17 mg / L, 18 mg / L, 19 mg / L, 20 mg / L, 21 mg / L, 22 mg / L, 23 mg / L, 24 mg / L, 25 mg / L, 26 mg / L, 27 mg / L, 28 mg / L and a concentration between any two of the above values; the concentration of potassium ions in the immersion water can be 2.2 mg / L, 2.3 mg / L, 2.4 mg / L, 2.5 mg / L, 2.6 mg / L, 2.7 mg / L, 2.8 mg / L, 2.9 mg / L, 3 mg / L, 3.1 mg / L, 3.2 mg / L, 3.3 The concentration of metasilicate ions in the immersion water can be 2.5 mg / L, 3 mg / L, 3.2 mg / L, 3.5 mg / L, 3.8 mg / L, 4 mg / L, 4.5 mg / L, 5 mg / L, 5.8 mg / L, 6 mg / L, 6.1 mg / L, 6.2 mg / L, 6.3 mg / L, 6.5 mg / L, 6.8 mg / L, 7 mg / L, 7.5 mg / L, 8 mg / L and the concentration between any two of the above values.
[0054] The modified dolomite refers to a product formed after natural dolomite is modified. After the natural dolomite is modified, the calcium compound and magnesium compound contained therein are at least partially converted into hydrated carbonate compounds, so that calcium and magnesium ions can be released more stably and the pH value of water can be adjusted at the same time. In some embodiments of the present application, the modified dolomite includes hydrated carbonate compounds, and the cations in the hydrated carbonate compounds include calcium ions and magnesium ions.
[0055] In other embodiments, the water filtered by the modified dolomite contains calcium ions and magnesium ions. Specifically, the modified dolomite (10 g) and acid-washed coconut shell activated carbon and 5 million molecular weight polyethylene are mixed in a weight ratio of 1:6:6 and then compression molded into a filter material. The filter material is then used to filter pure water. Under the condition that the pure water flow rate is 1.9 to 2.1 L / min, the water sample after filtering through the filter material contains calcium ions and magnesium ions, and the contents of the two ions meet the following standards: the concentration of the calcium ions is 3 to 18 mg / L, and the concentration of the magnesium ions is 2 to 10 mg / L. For example, the concentration of the precipitated calcium ions can be 3mg / L, 4mg / L, 5mg / L, 6mg / L, 7mg / L, 8mg / L, 9mg / L, 10mg / L, 10.5mg / L, 11mg / L, 11.5mg / L, 12mg / L, 13mg / L, 15mg / L, 18mg / L and the concentration between any two of the above values; the concentration of the precipitated magnesium ions can be 2mg / L, 2.5mg / L, 3mg / L, 3.5mg / L, 4mg / L, 4.5mg / L, 4.8mg / L, 4.9mg / L, 5mg / L, 5.5mg / L, 6mg / L, 7mg / L, 8mg / L, 9mg / L, 10mg / L and the concentration between any two of the above values.
[0056] The modified basalt refers to a product obtained by modifying natural basalt, which can better precipitate metasilicic acid; in some embodiments, 5g of the modified basalt is placed in pure water (obtained by RO membrane treatment) of room temperature (20-30°C) with an equal mass and soaked for 23-25h, the modified basalt is taken out, and the type and concentration of ions in the soaking water are detected. The soaking water contains at least metasilicate ions, and the content of the metasilicate ions meets the following standards: the concentration of the metasilicate ions is 13.5-33.5mg / L; for example, the metasilicate The concentration of silicate ions can be 13.5 mg / L, 13.6 mg / L, 14 mg / L, 15 mg / L, 16 mg / L, 17 mg / L, 18 mg / L, 20 mg / L, 21 mg / L, 22 mg / L, 23 mg / L, 24 mg / L, 25 mg / L, 28 mg / L, 29 mg / L, 30 mg / L, 31 mg / L, 32 mg / L, 33 mg / L, 33.1 mg / L, 33.2 mg / L, 33.5 mg / L and concentrations between any two of the above values.
[0057] The modified tuff refers to a product obtained by modifying natural tuff, and the purpose of the modification is to increase the strontium content; in some embodiments, the modified tuff contains strontium, and the mass percentage of the strontium element is 42% to 50.5%. For example, the mass percentage of the strontium element can be 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 50.2%, 50.5%, 50.5% and concentrations between any two of the above values.
[0058] In some embodiments, the particle size of the modified granite is less than or equal to 35 mesh and greater than 200 mesh; it is understood that the modified granite can pass through a 35 mesh sieve but cannot pass through a 200 mesh sieve when passing through a sieve. For example, the modified granite can pass through a 35 mesh sieve, a 40 mesh sieve, a 45 mesh sieve, a 50 mesh sieve, a 60 mesh sieve, a 70 mesh sieve, a 80 mesh sieve, a 90 mesh sieve, a 100 mesh sieve, a 120 mesh sieve, a 150 mesh sieve, a 180 mesh sieve, a 190 mesh sieve, etc. The sieve involved in the present application can be selected from any sieve on the market that meets the basic size of the national standard GBT6005-2008 test sieve metal wire woven mesh, perforated plate and electroformed thin plate sieve hole.
[0059] In some embodiments, the particle size of the modified dolomite is less than or equal to 80 mesh and greater than 325 mesh. It can be understood that the modified dolomite can pass through an 80 mesh sieve but cannot pass through a 325 mesh sieve. For example, the modified dolomite can pass through an 80 mesh sieve, a 90 mesh sieve, a 100 mesh sieve, a 150 mesh sieve, a 200 mesh sieve, a 250 mesh sieve, a 300 mesh sieve, a 320 mesh sieve, and the like.
[0060] In some embodiments, the particle size of the modified basalt is less than 325 mesh and greater than 1000 mesh; it can be understood that the modified basalt can pass through a 325 mesh sieve but cannot pass through a 1000 mesh sieve. For example, the modified basalt can pass through a 325 mesh sieve, a 330 mesh sieve, a 350 mesh sieve, a 400 mesh sieve, a 500 mesh sieve, a 600 mesh sieve, a 700 mesh sieve, an 800 mesh sieve, a 900 mesh sieve, a 950 mesh sieve, a 990 mesh sieve, and the like.
[0061] In some embodiments, the particle size of the modified tuff is less than or equal to 35 mesh and greater than 200 mesh; for example, the modified tuff can pass through a 35 mesh sieve, but cannot pass through a 200 mesh sieve, for example, it can pass through a 35 mesh sieve, a 40 mesh sieve, a 45 mesh sieve, a 50 mesh sieve, a 60 mesh sieve, a 70 mesh sieve, an 80 mesh sieve, a 90 mesh sieve, a 100 mesh sieve, a 120 mesh sieve, a 150 mesh sieve, a 180 mesh sieve, a 190 mesh sieve, and the like.
[0062] In some embodiments, the particle size of the modified granite is less than or equal to 35 mesh and greater than 200 mesh, the particle size of the modified dolomite is less than or equal to 80 mesh and greater than 325 mesh, the particle size of the modified basalt is less than 325 mesh and greater than 1000 mesh, and the particle size of the modified tuff is 35-200 mesh. In this way, the particle size distribution is within the range of 35-1000 mesh, which, on the one hand, helps the dissolution of various elements, and on the other hand, when several materials are mixed, the particle sizes of the several materials match each other, which not only better compresses to form filter materials, but also ensures that the materials are evenly distributed, so that they can fully play their role.
[0063] In addition to the above-mentioned ores, the filter element may also include auxiliary materials. In some embodiments, the filter element further includes activated carbon and polyethylene, the activated carbon is preferably acid-washed coconut shell activated carbon, and the polyethylene is preferably ultra-high molecular weight polyethylene. By adding activated carbon, impurities can be adsorbed and water quality can be purified. By adding polyethylene, it can play a bonding role. Further, by weight, the filter element includes 30 to 60 parts of acid-washed coconut shell activated carbon and 30 to 60 parts of polyethylene; for example, by weight, the filter element includes 10 to 20 parts of modified granite, 10 to 30 parts of modified dolomite, 10 to 20 parts of modified basalt, 5 to 10 parts of modified tuff, 30 to 60 parts of acid-washed coconut shell activated carbon and 30 to 60 parts of polyethylene.
[0064] In some embodiments, the particle size of the acid-washed coconut shell activated carbon is 35 to 1000 mesh; for example, the acid-washed coconut shell activated carbon can pass through a 35 mesh sieve, a 40 mesh sieve, a 60 mesh sieve, an 80 mesh sieve, a 100 mesh sieve, a 200 mesh sieve, a 500 mesh sieve, a 600 mesh sieve, an 800 mesh sieve, a 1000 mesh sieve, and the like.
[0065] In some embodiments, the molecular weight of the polyethylene is greater than or equal to 5 million, for example, it can be 5 million, 6 million, 8 million, 10 million, and so on.
[0066] In some embodiments of the present application, the water filtered by the filter element meets the following standards: strontium content is 0.2-1.2 mg / L, calcium content is 10.0-48.0 mg / L, potassium content is 0.5-1.5 mg / L, magnesium content is 4.0-18.0 mg / L, sodium content is 6.0-35.0 mg / L, TDS value is 50.0-280.0 mg / L, metasilicic acid content is greater than or equal to 30 ppm, pH is 7.3-8.3. The water that meets the above standards has the characteristics of Tianshan water quality, not only has a good taste, but also is rich in minerals. The content of strontium, calcium, potassium, magnesium, sodium, metasilicic acid, etc. is similar to that of Tianshan water quality, and can meet the requirements of high-quality drinking water.
[0067] In the second aspect, the present application also proposes a method for preparing a filter element simulating the characteristic mineral water of Tianshan Mountain, please refer to Figure 1 , the preparation method comprises the following steps:
[0068] S10, heating the natural granite at 400-600° C., and then putting it into a sodium salt solution and cooling it to obtain modified granite;
[0069] S20, heating natural dolomite in a mixed gas of carbon dioxide and water vapor to form hydrated carbonate compounds to obtain modified dolomite;
[0070] S30, soaking the natural basalt with acid and ultrasonicating, and then heating at 800°C to 900°C to obtain modified basalt;
[0071] S40, heating the natural tuff at 400-500° C. and modifying it with sulfuric acid to obtain modified tuff;
[0072] S50, mixing a plurality of raw materials and molding them to obtain a filter element; wherein the plurality of raw materials include the modified granite, the modified dolomite, the modified basalt and the modified tuff.
[0073] Among them, the natural granite can be selected from any common granite, including but not limited to the granite in Beijing Zhoukoudian area, the granite in Shandong Mengyin area, the granite in Sichuan Leshan area, etc.; preferably, the granite in Beijing Zhoukoudian area can not only dissolve more calcium, potassium, magnesium, sodium, metasilicic acid ions, but also contain less impurities such as heavy metals, and have better safety. It is understandable that other granites with less heavy metal impurities and more dissolved calcium, potassium, magnesium, sodium, and metasilicic acid can also be selected.
[0074] The natural dolomite can be any common dolomite, including but not limited to the dolomite in Bama, Guangxi, the dolomite in Chenzhou, Hunan, the dolomite in Qichun, Hubei, and the dolomite in Tongling, Anhui; preferably, the dolomite in Bama, Guangxi can not only dissolve more calcium and magnesium, but also contains less silicon, which has less effect on the precipitation of calcium and magnesium. It is understandable that other dolomites with less silicon content and more dissolved calcium and magnesium can also be selected.
[0075] Natural basalt can be selected from any common basalt, including but not limited to basalt in Luoyang, Henan, basalt in Tengchong, Yunnan, and basalt in Mingguang, Anhui, etc.; preferably, basalt in Tengchong, Yunnan, which can not only dissolve more metasilicic acid, but also contains less impurities such as heavy metals, and is safer. It is understandable that other basalts with less heavy metal impurities and more metasilicic acid dissolution can also be selected.
[0076] The natural tuff can be selected from any common tuff, including but not limited to the tuff in Shangrao, Jiangxi, the tuff in Fuzhou, Fujian, and the tuff in Altay, Xinjiang, etc.; preferably, the tuff in Altay, Xinjiang, which can not only dissolve more strontium, but also contains less impurities such as heavy metals, and is safer. It is understandable that other basalts with less heavy metal impurities and more strontium dissolution can also be selected.
[0077] Furthermore, unweathered ores may be preferred, for example, granite buried at a depth of 15 to 20 meters, basalt buried at a depth of 25 to 40 meters, etc. Unweathered ores have a hard structure and are not easy to break, which is convenient for subsequent cleaning, crushing and particle size control. Moreover, they contain mineral components of sufficient abundance. Using them as raw materials makes it easier to control the properties of the modified ore, the quality of the filter element, and the content of various mineral components precipitated therefrom.
[0078] In step S10:
[0079] The purpose of the heating is to destroy part of the structure of the granite by temperature change modification, which can promote the precipitation of potassium therein, and at the same time promote the precipitation of part of the silicon therein in the form of metasilicic acid. The heating temperature is 400-600°C, for example, it can be 400°C, 420°C, 450°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 550°C, 580°C, 600°C and temperatures between any two values listed above. In some embodiments, the heating temperature is preferably 450-550°C, further preferably 480-520°C, and more preferably 500°C. Within this range, the precipitation amount of sodium, potassium, and metasilicic acid is high, and the energy consumption is low, and the economic benefit is higher.
[0080] In some embodiments, the heating time is 1 to 3 hours, for example, 1 hour, 1.5 hours, 1.8 hours, 2 hours, 2.2 hours, 2.5 hours, 3 hours and values between any two of the values listed above, so as to ensure that the granite is fully modified.
[0081] The effect of cooling in a sodium salt solution is that the sodium content in the ore can be increased by exchange adsorption, and the sodium can be slowly released in the filter element. In some embodiments, the molar concentration of sodium ions in the sodium salt solution is 2 to 5 mol / L, for example, it can be 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L and any two values listed above. Within this range, the amount of sodium precipitation can be effectively increased while maintaining the content of potassium and metasilicic acid. Further, the molar concentration of sodium ions in the sodium salt solution is preferably 2 to 4 mol / L, more preferably 3 mol / L, so that not only the amount of sodium precipitation can be greatly increased, and the precipitation of each other component in the leachate can be balanced, but also the amount of sodium salt can be saved and the material can be saved. The sodium salt can be selected from any common sodium salt, such as sodium chloride.
[0082] In some embodiments, before heating, the natural granite may be pre-treated by crushing, cleaning, etc. Specifically, the pre-treatment includes crushing the natural granite into small particles with an average particle size of 2 to 3 mm, washing the surface debris with pure water, and then drying at 100 to 110° C. The pure water may be primary reverse osmosis pure water, and the drying time may be 2 to 4 hours.
[0083] In some embodiments, after treating with the sodium salt solution, the method further comprises: washing with pure water.
[0084] In some embodiments, step S10 further comprises repeating the steps of drying-heating-cooling with sodium salt solution-washing at least once, for example, repeating twice, three times, four times, five times or more times.
[0085] In addition, in some embodiments, the step S10 further includes the following steps: ultrasonically cleaning with deionized water for 15 to 45 minutes, and fully drying at 110 to 130° C. in a ventilated environment; then, fully grinding the cooled granite and passing it through a 35 to 200 mesh sieve to obtain modified granite.
[0086] In step S20:
[0087] The purpose of the step of heating the natural dolomite in a mixed gas of carbon dioxide and water vapor is to convert calcium and magnesium therein into hydrated carbonate compounds by heating in an atmosphere of carbon dioxide and water vapor, so that calcium and magnesium ions can be released more stably and the pH value can be adjusted at the same time. The mixed gas is a mixture of carbon dioxide and water vapor, and the mixing ratio of carbon dioxide and water vapor is a volume ratio of (1.5 to 2.5):1, for example, 1.5:1, 1.8:1, 1.9:1, 2:1, 2.1:1, 2.2:1, 2.5:1, and the like.
[0088] In some embodiments, the heating temperature is 400-650° C., for example, 400° C., 420° C., 450° C., 480° C., 490° C., 500° C., 510° C., 520° C., 530° C., 550° C., 580° C., 600° C., 650° C., and any two values thereof. Within this range, the precipitation amount of calcium and magnesium ions can be effectively increased, and the pH of the leachate can be maintained.
[0089] In some embodiments, the step of heating natural dolomite in a mixture of carbon dioxide and water vapor may specifically include: placing the natural dolomite in a tubular furnace, passing a mixture of carbon dioxide and water vapor into the furnace, and then controlling the temperature to rise by 45 to 55° C. every 10 minutes, raising the temperature to 400 to 650° C., heating at a constant temperature for 3 to 5 hours, stopping heating, and continuing to pass the mixture of carbon dioxide and water vapor until it is completely cooled.
[0090] In some embodiments, before heating, the natural dolomite may be pre-treated by crushing, cleaning, etc. Specifically, the pre-treatment includes: crushing the natural dolomite into small particles of 0.5 to 1 mm, repeatedly washing with tap water until there are no impurities, and then repeatedly washing with deionized water for several times, and drying. The drying temperature may be 100 to 110°C.
[0091] In addition, in some embodiments, the step S20 further includes the steps of crushing and screening the modified dolomite, and the sieve used during the screening is 80-325 mesh.
[0092] In step S30:
[0093] In this embodiment, natural basalt is soaked in acid to dissolve some soluble minerals therein, and then ultrasonic cleaning is performed to open up the blind pores therein, and then high-temperature treatment is performed to allow silicon to precipitate better to form metasilicic acid, thereby increasing the precipitation amount of metasilicic acid.
[0094] In some embodiments, the acid includes a hydrochloric acid solution with a concentration of 1 to 4 mol / L, for example, the acid concentration may be 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, and any two values between the above. Within this range, the amount of metasilicic acid precipitation can be effectively increased; further, for the comprehensive consideration of increasing the amount of metasilicic acid precipitation, saving materials, and environmental protection, the concentration may preferably be 3 mol / L.
[0095] In some embodiments, the acid immersion and ultrasonication time is 0.5 to 1.5 h, for example, 0.5 h, 0.8 h, 1 h, 1.2 h, 1.5 h, and values between any two of the values listed above.
[0096] In some embodiments, the acid soaking and ultrasonic step further includes: washing the basalt with deionized water until the concentration of chloride ions in the eluent is less than 0.001 mg / L, and then drying it at 100-110° C. with ventilation.
[0097] In some embodiments, the heating temperature is 800°C to 900°C, for example, 800°C, 810°C, 820°C, 830°C, 840°C, 845°C, 850°C, 855°C, 860°C, 870°C, 880°C, 900°C, and values between any two of the above values. Further, the heating temperature is preferably 845 to 855°C, more preferably 850°C. The heating time is 3 to 5 hours, for example, specifically 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, and values between any two of the above values.
[0098] In some embodiments, before acid immersion, the natural basalt may be pre-treated by crushing, cleaning, etc.; specifically, the pre-treatment includes: crushing the natural basalt into small particles of 1 to 2 mm, and repeatedly washing with tap water until there are no impurities.
[0099] In addition, in some embodiments, the step S30 further includes the steps of crushing and screening the modified basalt, and the sieve used during the screening is a 325-1000 mesh sieve.
[0100] In step S40:
[0101] In this embodiment, the percentage of strontium in the tuff is increased by first heating the natural tuff and then modifying it with sulfuric acid, while the percentage of barium is reduced to a certain extent. The heating temperature is 400-500°C, for example, it can be 400°C, 420°C, 450°C, 480°C, 490°C, 500°C and any value between the above two values; the heating time can be 4-5h, for example, 4h, 4.5h, 5h and any value between the above two values.
[0102] The sulfuric acid modification step includes: mixing tuff and sulfuric acid solution, soaking, then washing with deionized water and drying. The concentration of the sulfuric acid solution is 1-3 mol / L; for example, it can be 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L and any concentration between two values listed above. Within this range, not only can the strontium precipitation amount be greatly increased, but also the barium content can be controlled within a certain range. Furthermore, the concentration is preferably 1.5-2.2 mol / L, more preferably 2 mol / L, so that the barium content can be greatly reduced.
[0103] In some embodiments, the soaking time may be 15 to 45 minutes, for example, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, 45 minutes, and values between any two of the values listed above.
[0104] In some embodiments, the drying temperature is 140-160° C., and the drying time is 2-5 hours.
[0105] In some embodiments, the natural tuff may be pre-treated by crushing, cleaning, etc. before heating; specifically, the pre-treatment includes: crushing the natural tuff into small particles of 3 to 5 mm, repeatedly washing with tap water until there are no impurities, and drying. The drying temperature may be 100 to 110° C., and the drying time may be 3 to 5 hours.
[0106] In addition, in some embodiments, in the step S40, after heating and before the modification with sulfuric acid, the step of crushing and screening the tuff is also included, and the sieve used for screening is 35-200 mesh.
[0107] In step S50:
[0108] In some embodiments, the multiple raw materials include, by weight, 10 to 20 parts of the modified granite, 10 to 30 parts of the modified dolomite, 10 to 20 parts of the modified basalt, and 5 to 10 parts of the modified tuff. In other embodiments, the multiple raw materials include, by weight, 10 to 20 parts of the modified granite, 10 to 30 parts of the modified dolomite, 10 to 20 parts of the modified basalt, 5 to 10 parts of the modified tuff, 30 to 60 parts of acid-washed coconut shell activated carbon, and 30 to 60 parts of polyethylene; wherein the particle size of the acid-washed coconut shell activated carbon is 35 to 1000 mesh; and the molecular weight of the polyethylene is greater than or equal to 5 million.
[0109] Specifically, step S50 may include: mixing a variety of raw materials, loading them into a prepared mold, setting the hydraulic press pressure to 8-12 MPa, pressing and molding, then placing them in an oven, setting the temperature to 180-220°C, baking for 1-2 hours, taking out the mold while hot, cutting them into a preset length after natural cooling, adding a shell, and obtaining the filter element.
[0110] The filter element is installed at the pure water outlet of the water purifier to mineralize the pure water. The mineralized water has the characteristics of Tianshan water quality, including: strontium content of 0.2-1.2 mg / L, calcium content of 10.0-48.0 mg / L, potassium content of 0.5-1.5 mg / L, magnesium content of 4.0-18.0 mg / L, sodium content of 6.0-35.0 mg / L, TDS value of 50.0-280.0 mg / L, orthosilicic acid content of greater than or equal to 25 mg / L, and pH of 7.3-8.3.
[0111] In a third aspect, the present application further proposes a water purifier, comprising a filter element, wherein the filter element comprises the filter element described above, or the filter element is prepared by the preparation method described above.
[0112] Figure 4 An embodiment of the water purifier described in the present application is provided. Figure 4 The water purifier includes a PP cotton filter element 2, a granular activated carbon filter element 5, a scale-inhibiting carbon rod filter element 6, an RO reverse osmosis filter element 8, a filter element 11 for simulating the characteristic mineral water of Tianshan Mountain mentioned above, and a sterilizing taste filter element 12, which are sequentially connected along the water flow direction from the water inlet 1 to the water outlet 13. In addition, a low-pressure switch 3 and a water inlet electromagnetic valve 4 are provided between the PP cotton filter element 2 and the granular activated carbon filter element 5, a booster pump 7 is provided between the scale-inhibiting carbon rod filter element 6 and the RO reverse osmosis filter element 8, a high-pressure switch 9 is provided between the RO reverse osmosis filter element 8 and the filter element 11 for simulating the characteristic mineral water of Tianshan Mountain, and a wastewater ratio electromagnetic valve 10 is provided at the sewage outlet of the RO reverse osmosis filter element 8; the water purifier also includes a control panel 14, which is electrically connected to the low-pressure switch 3, the water inlet electromagnetic valve 4, the booster pump 7, the high-pressure switch 9, and the wastewater ratio electromagnetic valve 10 respectively. Among them, the PP cotton filter element 2, the granular activated carbon filter element 5, the scale-inhibiting carbon rod filter element 6, and the RO reverse osmosis filter element 8 together constitute the purification module 100, the filter element 11 simulating the characteristic mineral water of Tianshan Mountain and the sterilization taste filter element 12 constitute the mineralization module 200, and ordinary municipal tap water or centralized water supply is treated by the purification module 100 to remove impurities such as inorganic salts, heavy metals, organic matter, bacteria, etc. to form pure water; then it is treated by the mineralization module 200 to make sterile, mineralized and good-tasting drinking water.
[0113] The water purifier proposed in the present application is equipped with the above-mentioned filter element, and the pure water treated by the purification module 100 is mineralized to make it have the characteristics of Tianshan water quality, wherein: the strontium content is 0.2-1.2 mg / L, the calcium content is 10.0-48.0 mg / L, the potassium content is 0.5-1.5 mg / L, the magnesium content is 4.0-18.0 mg / L, the sodium content is 6.0-35.0 mg / L, the TDS value is 50.0-280.0 mg / L, the orthosilicic acid content is greater than or equal to 25 mg / L, and the pH is 7.3-8.3.
[0114] The technical scheme and technical effects of the present application are described in detail below through specific embodiments and comparative examples. The following embodiments are only some embodiments of the present application and do not specifically limit the present application.
[0115] Example 1 Screening of natural ore
[0116] Take unweathered natural ore, clean the surface impurities, dry and crush into 18-35 mesh samples, take 100g sample and place it in a clean beaker, add 400ml of grade 1 deionized water, stir with a glass rod for 30s and pour it out, repeat the cleaning 5 times, and then rinse with grade 3 deionized water 3 times. Finally, add 100ml of grade 3 deionized water, soak in 25±5℃ environment for 24h, and take the supernatant for testing. Note: This method is only used for the screening of granite, basalt and tuff, and dolomite is screened by component analysis.
[0117] (I) The sources of natural ore are: granite in Leshan, Sichuan, granite in Mengyin, Shandong, and granite in Zhoukoudian, Beijing. The test results are shown in Table 1.
[0118] Table 1 Natural granite
[0119] Leshan, Sichuan Mengyin, Shandong Beijing Zhoukoudian standard unit pH 7.0 8.6 7.2 8.5 / Potassium 1.7 1.2 1.8 / mg / L calcium 0.8 6.3 1.1 / mg / L sodium 10.6 8.8 14.3 / mg / L magnesium 0.8 1.9 0.5 / mg / L strontium ND ND ND / mg / L Metasilicic acid 2.1 1.9 2.2 / mg / L arsenic ND ND ND 0.001 mg / L cadmium 0.0009 0.0001 0.0001 0.0005 mg / L chromium 0.0013 0.0001 0.0001 0.005 mg / L lead 0.0006 0.0022 0.0001 0.001 mg / L aluminum 0.0882 0.1362 0.0225 0.02 mg / L iron 0.0030 0.0236 0.0021 0.06 mg / L manganese 0.0033 0.0095 0.0030 0.02 mg / L copper ND ND ND 0.2 mg / L Zinc ND ND ND 0.2 mg / L silver ND ND ND 0.005 mg / L
[0120] Among them, ND means that the corresponding heavy metals were not detected.
[0121] As can be seen from Table 1, the immersion water corresponding to the granite in Zhoukoudian, Beijing, has the lowest heavy metal content, the highest safety, and a pH value that is closer to the standard. Therefore, the granite in Zhoukoudian, Beijing can be selected as the mineralization material.
[0122] (II) The sources of natural ore are: basalt in Luoyang, Henan, basalt in Tengchong, Yunnan, and basalt in Mingguang, Anhui. The test results are shown in Table 2.
[0123] Table 2 Natural basalt
[0124] Luoyang, Henan Tengchong, Yunnan Anhui Mingguang standard unit Metasilicic acid 10.5 11.3 9.2 / mg / L arsenic ND ND ND 0.001 mg / L cadmium 0.0006 0.0001 0.0004 0.0005 mg / L chromium 0.0013 0.0011 0.0026 0.005 mg / L lead 0.0015 0.0003 0.0006 0.001 mg / L aluminum 1.9682 1.2035 1.1362 0.02 mg / L iron 0.3362 0.2659 0.3125 0.06 mg / L manganese 0.0325 0.0226 0.0293 0.02 mg / L copper 0.0338 0.0265 0.0299 0.2 mg / L Zinc ND 0.0002 0.0002 0.2 mg / L silver ND ND ND 0.005 mg / L
[0125] Among them, ND means that the corresponding heavy metals were not detected.
[0126] It can be seen from Table 2 that the basalt in Tengchong, Yunnan can not only dissolve more metasilicic acid, but also contains less impurities such as heavy metals and has better safety. Therefore, the basalt in Tengchong, Yunnan can be selected as mineralization material.
[0127] (III) The sources of natural ore are: tuff in Shangrao, Jiangxi, tuff in Fuzhou, Fujian, and tuff in Altay, Xinjiang. The test results are shown in Table III.
[0128] Table 3 Natural Tuff
[0129] Shangrao, Jiangxi Fuzhou, Fujian Altay, Xinjiang standard unit strontium 10.3 5.6 16.5 / mg / L arsenic 0.0016 0.0005 0.0008 0.001 mg / L cadmium ND ND ND 0.0005 mg / L chromium 0.0006 0.0009 0.0003 0.005 mg / L lead 0.0029 0.0011 0.0009 0.001 mg / L aluminum 0.0036 0.0028 0.0029 0.02 mg / L iron 0.0065 0.0255 0.0433 0.06 mg / L manganese 0.0065 0.0038 0.0046 0.02 mg / L copper ND ND ND 0.2 mg / L Zinc ND 0.0002 0.0002 0.2 mg / L silver ND ND ND 0.005 mg / L
[0130] It can be seen from Table 3 that the tuff in the Altay region of Xinjiang can not only dissolve more strontium, but also contains less impurities such as heavy metals and has better safety. The tuff in the Altay region of Xinjiang can be selected as mineralized material.
[0131] (IV) The sources of natural ore are: dolomite in Bama, Guangxi, dolomite in Chenzhou, Hunan, dolomite in Qichun, Hubei, and dolomite in Tongling, Anhui. Take unweathered natural ore, clean the surface impurities, and do component analysis. The test results are shown in Table 4.
[0132] Table 4 Natural dolomite (mass percentage)
[0133] Chenzhou, Hunan Bama, Guangxi Qichun, Hubei Anhui Tongling calcium 71.05 60.39 58.27 67.41 magnesium 20.26 33.91 27.24 19.73 silicon 5.34 4.22 13.36 10.56
[0134] It can be seen from Table 4 that the silicon content of dolomite in Qichun, Hubei and Tongling, Anhui is too high, which has a great impact on the later precipitation of calcium and magnesium. The calcium-magnesium ratio in Chenzhou, Hunan is quite different. Combined with the water quality data of Karez natural mineral water, its calcium-magnesium ratio is close to 2:1. Comprehensive analysis shows that the dolomite in Bama, Guangxi can be used as a more ideal mineralization material.
[0135] Example 2 Parameter adjustment of modified granite
[0136] Natural granite buried at a depth of 15 to 20 m in Zhoukoudian, Beijing, was taken and crushed into small particles of 2 to 3 mm. The surface debris was washed with primary reverse osmosis pure water, and the pretreated granite was obtained after ventilation and drying at 105°C for 3 hours for later use.
[0137] (I) The pretreated granite was placed in a muffle furnace and quickly heated to different temperatures (400℃, 450℃, 500℃, 550℃, 600℃), kept at a constant temperature for 2h, taken out and quickly put into a 3mol / L sodium chloride solution to cool, taken out and washed with pure water after complete cooling, and ventilated and dried at 105℃ for 3h. Repeat the above steps of heating-constant temperature-salt washing cooling-washing-drying 5 times, then ultrasonically cleaned with deionized water for 20min, and fully dried in a ventilated environment at 120℃. After cooling, the granite particles were fully ground and passed through 35 mesh and 200 mesh sieves. Modified granite with a particle size between 35 mesh and 200 mesh was obtained.
[0138] 20g of granite sample (20g of modified granite with muffle furnace heating temperature of 400℃, 450℃, 500℃, 550℃, 600℃ and other treatment conditions, and 20g of natural granite with particle size between 35 mesh and 200 mesh) was put into a beaker, 20g of pure water was added, and it was soaked in a 25℃ environment for 24h. The supernatant was taken for detection. The detection results are shown in Table 5.
[0139] Table 5
[0140]
[0141] As can be seen from Table 5, the modified granite treated at 400-600°C has sodium ions, potassium ions and metasilicate ions precipitated, all within the range: the concentration of sodium ions is 16-28 mg / L, the concentration of potassium ions is 2.2-3.9 mg / L, and the concentration of metasilicate ions is 2.5-8 mg / L; and the pH is also in the range of 7.3-8.3, which can be used to prepare filter elements simulating the characteristic mineral water of Tianshan Mountain.
[0142] Furthermore, based on a comprehensive evaluation from multiple aspects such as energy saving and gain maximization, the temperature is preferably 450-550°C, more preferably 500°C.
[0143] (ii) Place the pretreated granite in a muffle furnace and heat it rapidly to 500°C, keep the temperature constant for 2 hours, take it out and quickly put it into sodium chloride solution of different concentrations (2mol / L, 3mol / L, 4mol / L, 5mol / L) to cool it, take it out after complete cooling, wash it with pure water, and dry it at 105°C for 3 hours. Repeat the above steps of heating-constant temperature-salt washing cooling-washing-drying for 5 times, then ultrasonically clean it with deionized water for 20 minutes, and fully dry it in a ventilated environment at 120°C. After cooling, grind the granite particles thoroughly and pass them through 35 mesh and 200 mesh sieves. Modified granite with a particle size between 35 mesh and 200 mesh is obtained.
[0144] 20g of granite sample (20g of each of modified granite with the same treatment conditions and 20g of natural granite with a particle size between 35 mesh and 200 mesh) was put into a beaker, 20g of pure water was added, and the sample was immersed in a 25℃ environment for 24h. The supernatant was taken for detection. The detection results are shown in Table VI.
[0145] Table 6
[0146]
[0147] As can be seen from Table 6, the modified granite treated with a sodium chloride solution with a concentration of 2-5 mol / L has sodium ions, potassium ions and metasilicate ions precipitated that are within the range: the concentration of sodium ions is 16-28 mg / L, the concentration of potassium ions is 2.2-3.9 mg / L, and the concentration of metasilicate ions is 2.5-8 mg / L; and the pH is also in the range of 7.3-8.3, which can be used to prepare filter elements simulating the characteristic mineral water of Tianshan Mountain.
[0148] Furthermore, based on a comprehensive evaluation from multiple aspects such as material saving and maximization of the gain of each component, the molar concentration of sodium ions in the sodium salt solution is preferably 2 to 4 mol / L, more preferably 3 mol / L.
[0149] (III) Take the modified granite and natural granite with the muffle furnace heating temperature of 500℃, the sodium chloride solution concentration of 3mol / L and the other treatment conditions being the same, and observe them under electron microscope. The results are as follows Figure 2 and 3 shown.
[0150] contrast Figure 2 and Figure 3 It can be seen that after modification, the granite has a more developed pore structure and its pore development degree has been greatly improved. It can be seen that the modified granite is easier to precipitate mineral components.
[0151] Example 3 Parameter adjustment of modified dolomite
[0152] Take natural dolomite from Bama, Guangxi, crush it into small particles of 0.5-1 mm, rinse it repeatedly with tap water until there are no impurities, rinse it repeatedly with deionized water for several times, dry it in a drying oven at 105°C, and obtain pre-treated dolomite for later use.
[0153] The pretreated dolomite was placed in a tubular furnace, and a mixed gas of carbon dioxide and water vapor (mixing ratio of 2:1 by volume) was introduced into the tubular furnace. The temperature was raised by 50°C every 10 minutes to different temperatures (400°C, 500°C, 600°C, 700°C, 800°C), and the temperature was kept constant for 4 hours. The heating was stopped, and the mixed gas of carbon dioxide and water vapor was continued to be introduced until it was completely cooled. After cooling, it was crushed with a pulverizer, and sieved with 80-mesh and 325-mesh sieves to obtain modified dolomite with a particle size between 80 mesh and 325 mesh.
[0154] Randomly take 10g of dolomite sample (take 10g of each of modified dolomite with the same treatment conditions and the same tubular furnace heating temperature of 400℃, 500℃, 600℃, 700℃, 800℃, and other treatment conditions, and 10g of natural dolomite with a particle size between 80 mesh and 325 mesh), add 60g of acid-washed coconut shell activated carbon and 60g of ultra-high molecular weight polyethylene with a molecular weight of 5 million, mix well and put into a small T mold, hydraulically mold at a pressure of 10MPa, put into an oven, set the temperature to 200℃, bake for 1.5h, take out the demoulding, cut, add the shell, make a small T filter element, connect it to the pure water machine, set the water outlet flow rate to 2L / min, take water samples for testing, and the test results are shown in Table VII.
[0155] Table 7
[0156]
[0157] It can be seen from Table 7 that the modified dolomite obtained by heating at 400-650°C has calcium and magnesium ions precipitated in a range of 3-18 mg / L and 2-10 mg / L respectively; it can be used to prepare a filter element simulating the characteristic mineral water of Tianshan Mountain.
[0158] Furthermore, considering energy consumption, pH change and maximization of gains of each component, the temperature is preferably 500-600°C, more preferably 600°C.
[0159] Example 4 Parameter adjustment of modified basalt
[0160] Take natural basalt with a burial depth of 25-40m in Tengchong, Yunnan, break it into 1-2mm particles, and repeatedly rinse it with tap water until there are no impurities to obtain pre-treated basalt for use. Soak the pre-treated basalt in hydrochloric acid solutions of different concentrations (1mol / L, 2mol / L, 3mol / L, 4mol / L) and put it in an ultrasonic cleaning machine for ultrasonic treatment for 1h. After completion, wash it in deionized water until the Cl in the eluent is -The concentration is less than 0.0001 mg / L, and then dried in a ventilated environment at 105°C. Then put it in a muffle furnace, heat it to 850°C, keep it at a constant temperature for 4 hours, and cool it naturally. The cooled basalt is put into a ball mill for grinding, and after grinding, it is passed through 325 mesh and 1000 mesh sieves to obtain modified basalt with a particle size between 325 mesh and 1000 mesh.
[0161] Randomly take 5g of basalt sample (5g each of modified basalt with hydrochloric acid concentration of 1mol / L, 2mol / L, 3mol / L, 4mol / L, other modified basalt with the same treatment conditions, and natural basalt with a particle size between 325 mesh and 1000 mesh), put it in a beaker, add 5g of pure water, soak it in a 25℃ environment for 24h, take the supernatant for detection, and the detection results are shown in Table 8.
[0162] Table 8
[0163]
[0164] As shown in Table 8, the concentration of metasilicate ions precipitated from the modified basalt treated with 1-4 mol / L hydrochloric acid solution is in the range of 13.5-33.5 mg / L; it can be used to prepare filter elements for simulating Tianshan characteristic mineral water.
[0165] Furthermore, taking into account aspects such as material saving, environmental protection, and maximizing component gain, the concentration may preferably be 3 mol / L.
[0166] Example 5 Parameter adjustment of modified tuff
[0167] The natural tuff from the Altay region of Xinjiang was taken and crushed into 3-5 mm particles, the surface debris was washed off with tap water, and the pretreated tuff was obtained for later use at 105°C.
[0168] The pretreated tuff was placed in a muffle furnace and heated to 450°C, kept at a constant temperature for 4 hours, and then naturally cooled and ground into 35-200 mesh powder. Sulfuric acid solutions of different concentrations (1 mol / L, 2 mol / L, 3 mol / L) were added, stirred and soaked for 30 minutes, washed with deionized water, and dried at 150°C in a ventilated environment for 3 hours.
[0169] 2 g of tuff samples were randomly taken (2 g each of modified tuffs and natural tuffs with sulfuric acid concentrations of 1 mol / L, 2 mol / L, and 3 mol / L, and other treatment conditions were the same) for component analysis. The analysis results are shown in Table 9.
[0170] Table 9
[0171]
[0172] It can be seen from Table 9 that the modified tuff obtained by treatment with 1-3 mol / L sulfuric acid solution contains a strontium element mass percentage in the range of 42% to 50.5%; it can be used to prepare a filter element for simulating the characteristic mineral water of Tianshan Mountain.
[0173] Example 6
[0174] Take the natural granite buried at a depth of 15 to 20m in Zhoukoudian, Beijing, and crush it into small particles of 2 to 3mm. Wash the surface debris with primary reverse osmosis pure water, and then ventilate and dry it at 105℃ for 3h to obtain pretreated granite for standby use. Put the pretreated granite into a muffle furnace and quickly heat it to 500℃, keep it at a constant temperature for 2h, take it out and quickly put it into a 3mol / L sodium chloride solution to cool it. After it is completely cooled, take it out and wash it with pure water, and ventilate and dry it at 105℃ for 3h. Repeat the above heating-constant temperature-salt washing cooling-washing-drying steps 5 times, then ultrasonically clean it with deionized water for 20min, and fully dry it in a ventilated environment at 120℃. After cooling, grind the granite particles fully, pass through 35 mesh and 200 mesh sieves, and obtain modified granite with a particle size between 35 mesh and 200 mesh.
[0175] Take natural dolomite from Bama, Guangxi, crush it into small particles of 0.5-1mm, and rinse it repeatedly with tap water until there are no impurities. Rinse it repeatedly with deionized water several times, dry it in a drying oven at 105℃, and obtain pretreated dolomite for standby use. Put the pretreated dolomite into a tubular furnace, pass a mixed gas of carbon dioxide and water vapor (mixing ratio is 2:1 by volume) into the tubular furnace, control the temperature to rise by 50℃ every 10min, raise the temperature to 600℃, keep the temperature constant for 4h, stop heating, continue to pass the mixed gas of carbon dioxide and water vapor until it is completely cooled, and crush it with a pulverizer after cooling, select a sieve of 80-325 mesh to sieve, and obtain modified dolomite with a particle size between 80 mesh and 325 mesh.
[0176] Take natural basalt from Tengchong, Yunnan, buried at a depth of 25-40m, break it into 1-2mm particles, and repeatedly rinse it with tap water until there are no impurities, to obtain pre-treated basalt for later use. Soak the pre-treated basalt in 3mol / L hydrochloric acid solution, and put it in an ultrasonic cleaning machine for ultrasonic treatment for 1h. After completion, wash it in deionized water until the Cl in the eluent is - The concentration is less than 0.0001 mg / L, and then dried in a ventilated environment at 105°C. Then put it in a muffle furnace, heat it to 850°C, keep it at a constant temperature for 4 hours, and cool it naturally. The cooled basalt is put into a ball mill for grinding, and after grinding, it is passed through 325 mesh and 1000 mesh sieves to obtain modified basalt with a particle size between 325 mesh and 1000 mesh.
[0177] Take the natural tuff from the Altay area of Xinjiang, break it into 3-5mm particles, rinse the surface debris with tap water, dry it at 105℃ for 4h, and get the pretreated tuff for use. Put the pretreated tuff into a muffle furnace and heat it to 450℃, keep the temperature constant for 4h, and grind it into powder with a particle size between 35 mesh and 200 mesh after natural cooling. Add sulfuric acid solution of different concentrations of 2mol / L, stir and soak for 30min, wash it with deionized water, and dry it in a ventilated environment at 150℃ for 3h.
[0178] Modified granite, modified dolomite, modified basalt, modified tuff, acid-washed coconut shell activated carbon (particle size 35-1000 mesh) and polyethylene with a molecular weight of 5 million are mixed evenly according to the proportions of formula 1 to 3 in Table 10 below, then put into a large T mold, hydraulically molded at a pressure of 10 MPa, put into an oven, set the temperature to 200°C, bake for 1.5 hours, then take out the mold, cut, add a shell, and make a large T filter element.
[0179] Comparative Example
[0180] This comparative example is basically the same as Example 6, except that the ratio of each component of the filter element is adjusted, as shown in Table 10. Other parameters and steps remain unchanged.
[0181] Table 10 (Unit: copies)
[0182]
[0183] (I) Perform a functional water flow test on the filter element of Formula 1.
[0184] The test method is: take the filter element of Formula 1, install its water inlet on the water outlet (RO reverse osmosis filter element) of the purification module of the water purifier, and conduct a water flow test, wherein pure water refers to the water flowing out of the water outlet of the purification module, and the water with a water flow rate of 0L refers to the water sampled immediately after filtration by the filter element of Formula 1. Since the flow rate is close to 0, it is defined as a water flow rate of 0L.
[0185] The results are recorded in Table XI.
[0186] Table 11
[0187]
[0188] (II) Referring to the test method of "Functional water flow test on filter element of formula 1" above, water flow test was conducted on filter elements of formulas 1 to 3 and control formulas 1 to 5, and the water after filtration by the filter element was tested at the same water flow rate (2000L). The results are shown in Table 12.
[0189] Table 12
[0190]
[0191]
[0192] It can be seen from Table 12 that under the same water flow conditions, the indicators of the effluent corresponding to control formulas 1, 2, 4 and 5 are different from those of Karez mineral water. Although the effluent water quality corresponding to control formula 3 is close to that of Karez mineral water, its orthosilicic acid content is too low. The effluents corresponding to formulas 1 to 3 not only show the same water quality as Karez mineral water, but also contain orthosilicic acid greater than or equal to 25 mg / L, which not only tastes good, but also has better benefit effects on the body. This shows that the filter element proposed in this application can simulate mineral water with Tianshan characteristics and a high orthosilicic acid content.
[0193] (II) Taste evaluation
[0194] The test method is: take the filter element of formula 1, install the water inlet on the water outlet (RO reverse osmosis filter element) of the purification module of the water purifier, and after passing 2000L of water, take the water flowing out of the filter element outlet (defined as filter element outlet water), the water out of the purification module outlet (defined as pure water), Karez mineral water and Nongfu Spring mineral water for taste evaluation.
[0195] Evaluation method: Before the evaluation, the water sample was placed in a thermostat to keep the water temperature close to 10°C. 40 mL of water was poured into a disposable cup, and 5 test subjects aged 20 to 40 were selected. They were required not to smoke, drink, or have rhinitis. Before the experiment, the test subjects were required to rinse their mouths with Yibao pure water. Before tasting each water sample, they tasted Yibao water first, and all water samples were compared with Yibao water. The test subjects first held the water in their mouths for about 5 seconds (forward taste), then swallowed it, and the post-stimulation was delayed by 10 seconds (aftertaste). After tasting one water sample, they waited 1 minute before tasting the next water sample. Each water sample was evaluated for top taste, mellowness, earthy taste, strange taste, bitterness, sweetness, aftertaste and overall impression on a 10-point scale, with 0-2 points representing an extremely bad taste that is difficult to accept and cannot be swallowed; 3-5 points representing a poor taste with average acceptance and can be swallowed but not used for daily drinking; 6 points representing a passing taste that is acceptable and can be used for daily drinking with no obvious odor; 7-8 points representing a good taste and the consumer is willing to drink it often or for daily drinking; 9-10 points representing a very good taste, sweet and crisp.
[0196] The results are recorded in Table XIII.
[0197] Table 13
[0198]
[0199] It can be found from Table 13 that compared with the taste of pure water, the taste of the water out of the filter element has been greatly improved, and is close to the taste of the characteristic Karez mineral water of Tianshan Mountain, and the taste improvement effect is obvious.
[0200] The filter element and its preparation method and water purifier for simulating Tianshan characteristic mineral water provided in the embodiments of the present application are introduced in detail above. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for technical personnel in this field, according to the ideas of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A filter element simulating Tianshan characteristic mineral water, characterized in that: Includes modified granite, modified dolomite, modified basalt and modified tuff.
2. The filter element according to claim 1, characterized in that: The filter element comprises, by weight, 10 to 20 parts of modified granite, 10 to 30 parts of modified dolomite, 10 to 20 parts of modified basalt and 5 to 10 parts of modified tuff; and / or, The modified dolomite comprises hydrated carbonate compounds, and the cations in the hydrated carbonate compounds comprise calcium ions and magnesium ions; and / or, The modified granite is immersed in pure water of equal mass at 20 to 30° C. for 23 to 25 hours to precipitate sodium ions, potassium ions and metasilicate ions, and in the immersion water corresponding to 20 g of the modified granite, the concentration of the sodium ions is 16 to 28 mg / L, the concentration of the potassium ions is 2.2 to 3.9 mg / L, and the concentration of the metasilicate ions is 2.5 to 8 mg / L; and / or, The pure water filtered by the modified dolomite contains calcium ions and magnesium ions. Under the condition that the flow rate of the water is 1.9 to 2.1 L / min, the concentration of the calcium ions in the filtered water corresponding to 10 g of the modified dolomite is 3 to 18 mg / L, and the concentration of the magnesium ions is 2 to 10 mg / L; and / or, The modified basalt is immersed in pure water at 20 to 30° C. for 23 to 25 hours to precipitate metasilicate ions, and the concentration of the metasilicate ions in the immersed water corresponding to 5 g of the modified basalt is 13.5 to 33.5 mg / L; and / or, The modified tuff contains strontium element, and the mass percentage of the strontium element is 42% to 50.5%.
3. The filter element according to claim 1, characterized in that: The particle size of the modified granite is less than or equal to 35 mesh and greater than 200 mesh; and / or, The particle size of the modified dolomite is less than or equal to 80 mesh and greater than 325 mesh; and / or, The particle size of the modified basalt is less than or equal to 325 mesh and greater than 1000 mesh; and / or, The particle size of the modified tuff is less than or equal to 35 meshes and greater than 200 meshes.
4. The filter element according to claim 2, characterized in that: Calculated by weight, the filter element also includes 30 to 60 parts of acid-washed coconut shell activated carbon and 30 to 60 parts of polyethylene.
5. The filter element according to claim 4, characterized in that: The particle size of the acid-washed coconut shell activated carbon is 35 to 1000 mesh; and / or, The molecular weight of the polyethylene is greater than or equal to 5 million.
6. The filter element according to claim 1, characterized in that: The water filtered by the filter element meets the following standards: strontium content is 0.2-1.2 mg / L, calcium content is 10.0-48.0 mg / L, potassium content is 0.5-1.5 mg / L, magnesium content is 4.0-18.0 mg / L, sodium content is 6.0-35.0 mg / L, TDS value is 50.0-280.0 mg / L, orthosilicic acid content is greater than or equal to 25 mg / L, and pH is 7.3-8.
3.
7. A method for preparing a filter element simulating Tianshan characteristic mineral water, characterized in that: The following steps are involved: After heating natural granite at 400-600°C, it is placed in a sodium salt solution and cooled to obtain modified granite; The natural dolomite is heated in a mixed gas of carbon dioxide and water vapor to form hydrated carbonate compounds, thereby obtaining modified dolomite; The natural basalt is soaked in acid and ultrasonicated, and then heated at 800°C to 900°C to obtain modified basalt; The natural tuff is heated at 400-500°C and then modified with sulfuric acid to obtain modified tuff; Mix various raw materials and shape them into filter elements; The plurality of raw materials include the modified granite, the modified dolomite, the modified basalt and the modified tuff.
8. The preparation method according to claim 7, characterized in that: The molar concentration of sodium ions in the sodium salt solution is 2 to 5 mol / L; and / or, In the step of heating the natural dolomite in a mixed gas of carbon dioxide and water vapor to form hydrated carbonate compounds, the heating temperature is 400-650° C.; and / or, In the mixed gas of carbon dioxide and water vapor, the volume ratio of the carbon dioxide to the water vapor is (1.5-2.5):1; and / or, The acid comprises a hydrochloric acid solution with a concentration of 1 to 4 mol / L; and / or, The concentration of the sulfuric acid is 1 to 3 mol / L; and / or, Calculated by weight, the plurality of raw materials include 10 to 20 parts of the modified granite, 10 to 30 parts of the modified dolomite, 10 to 20 parts of the modified basalt and 5 to 10 parts of the modified tuff.
9. The preparation method according to claim 7, characterized in that: Calculated by weight, the filter element also includes 30 to 60 parts of acid-washed coconut shell activated carbon and 30 to 60 parts of polyethylene.
10. A water purifier, characterized in that: Comprising a filter element, the filter element comprises the filter element according to any one of claims 1 to 6, or the filter element is prepared by the preparation method according to any one of claims 7 to 9.
Citation Information
Cited By
Slow-release metasilicic acid mineralization material, filter element and preparation method