Film for battery bag and preparation method thereof
The barrier layer, adhesive layer and functional fabric layer are formed through one pass and three coating lines, which solves the problems of running loss and process defects in the preparation of battery bag films, and achieves a battery bag film with excellent mechanical strength uniformity and formability.
Patent Information
- Application Number
- CN202410403410.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-06
- Filing Date
- 2024-04-03
- Publication Date
- 2024-10-15
AI Technical Summary
The existing battery bag film preparation process involves risks of operational losses and process defects. The film is subject to increased stress, resulting in uneven mechanical strength and difficulty in achieving high bonding strength and formability.
Adopting the one-pass three-coating (1P3C) line method, the barrier layer, adhesive layer and functional fabric layer are formed through more than three coating processes, which reduces the driving roller tension, reduces the number of windings, increases the process speed, and ensures the longitudinal and transverse mechanical strength. Uniformity.
A battery bag film with excellent mechanical strength, low film stress, low mechanical strength deviation, and excellent formability has been realized, reducing operating losses and the probability of process defects, and improving formability and durability.
Smart Images

Figure CN118769635A_ABST
Abstract
Description
Technical Field
[0001] This specification discloses a film for a battery bag and a method for preparing the same.
[0002] [Korean R&D project supporting this invention]
[0003]
Project unique number
[0004]
Project number
[0005]
Department name
[0006] [Name of project management (specialized) organization] Korea Industrial Technology Evaluation and Management Institute
[0007]
Research Project Name
[0008] [Research Topic Name] Development of a next-generation secondary battery bag that can achieve more than twice the bonding strength (60°C)
[0009]
Contribution rate
[0010]
Project execution organization name
[0011] [Study period] January 1, 2023 to December 31, 2023 Background Art
[0012] Generally, compared with cylindrical or prismatic batteries, pouch-type batteries for electric vehicles have the advantages of being easy to change shape and having high energy density. Generally, such a battery pouch is prepared by sequentially performing a first process of surface treating one side of a metal layer, a second process of surface treating the other side of the metal layer, a third process of attaching an outer layer to one side, and a fourth process of attaching a sealing layer to the other side.
[0013] The above process is disclosed in the Korean Patent Gazette No. 10-2016-0070468. However, according to this existing process, it is necessary to repeatedly perform each process in the order of coating, drying and winding. In this case, when the fabric is transferred, there is a risk of increased operating loss (Loss) and process defects. In addition, the existing process has the problem of increased stress on the film due to its slow speed and repeated winding. In addition, the tensile force of the driving roller used to transfer the film is high, which causes the tensile curve of the film to change, resulting in changes in the longitudinal (MD) mechanical strength and transverse (TD) mechanical strength of the film.
[0014] Prior art literature
[0015] Patent Literature
[0016] Patent Document 1: Korean Patent Publication No. 10-2016-0070468
[0017] Patent Document 2: Korean Patent Publication No. 10-2022-0031820 Summary of the invention
[0018] Technical issues
[0019] According to one embodiment of the present invention, an object of the present invention is to provide a battery bag film having excellent mechanical strength, small film stress, low mechanical strength deviation, and excellent formability, and a method for preparing the same.
[0020] Technical Solution
[0021] According to one embodiment of the present invention, the battery bag film provided by the present invention includes: a barrier layer made of metal and surface-treated on both sides; an adhesive layer formed on both sides of the barrier layer; and a functional fabric layer formed on both sides of the adhesive layer, and the difference between the longitudinal (MD) breaking strength and the transverse (TD) breaking strength is less than 40N / 15mm.
[0022] According to still another embodiment, a battery bag provided by the present invention includes the above-mentioned film for a battery bag.
[0023] According to another embodiment, the method for preparing a battery bag film provided by the present invention includes: a two-side surface treatment step, in which both sides of the metal fabric used to form a barrier layer are surface treated; a one-side coating step, in which an adhesive is applied to one side of the surface-treated metal fabric to form an adhesive layer; and a bonding step, in which a functional fabric is bonded to one side of the adhesive layer to form a functional fabric layer.
[0024] Effects of the Invention
[0025] The battery bag film and the preparation method thereof according to an embodiment of the present invention provide the effects of excellent mechanical strength, small stress on the film, low deviation in mechanical strength, and excellent formability. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a diagram schematically showing a cross section of a film according to an embodiment of the present invention.
[0027] Figure 2 Schematic diagram of a battery bag film preparation device according to an embodiment of the present invention.
[0028] Figure 3 FIG. 1 is a stress-strain curve of a battery bag film according to an embodiment of the present invention.
[0029] Description of Reference Numerals
[0030] 1: Fabric supply unit 2: Foreign matter removal device
[0031] 3: First coater 4: Second coater
[0032] 5: Physical property stabilization drying section 6: Cooling section
[0033] 7: The third coating machine 8: Adhesive drying section
[0034] 9: Laminating section 10: Final winding section
[0035] 100: Outer layer 200: Outer surface bonding layer
[0036] 300: Barrier layer 310: Surface treatment layer
[0037] 320: Metal layer 330: Surface treatment layer
[0038] 400: Inner surface bonding layer 500: Sealing layer DETAILED DESCRIPTION
[0039] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0040] The embodiments of the present invention disclosed herein are only for illustrative purposes, and the embodiments of the present invention may exist in a variety of implementations and should not be construed as being limited to the embodiments described herein. The present invention may be subjected to a variety of changes and may have a variety of implementations. The embodiments do not limit the present invention to a specific disclosed implementation, and should be understood to include all changes, equivalent technical solutions, and alternative technical solutions within the scope of the present invention.
[0041] In the present specification, when a certain part “includes” another structural element, unless there is a special description to the contrary, it means that the other structural elements are also included, rather than excluding the other structural elements.
[0042] Throughout the specification, similar parts are given the same reference numerals. Throughout the specification, when a layer, film, region, plate, or other part is located "on" or "above" another part, this not only means the case where it is directly located on the other part, but also includes the case where there are other parts between them. Throughout the specification, terms such as "first" and "second" are used to describe various structural elements, but such terms do not limit the structural elements. Such terms are only used to distinguish one structural element from other structural elements.
[0043] In this specification, the term "battery (cell)" refers to a battery in its broadest sense, including various batteries such as secondary batteries such as lithium ion batteries and lithium polymer batteries, and portable storage batteries.
[0044] In this specification, "cell pouch" refers to a component used to immerse battery structural elements such as anode, cathode and separator in electrolyte and house them, and includes the broadest meaning of processing a laminated structure film into a bag shape or box shape, etc., taking into account gas barrier properties, flexibility, electrolyte resistance and thermal adhesion in order to house the above-mentioned battery structural elements.
[0045] In this specification, "barrier property" refers to the ability to block water vapor from the outside of the battery.
[0046] In this specification, "flexibility" refers to the degree of bending of a battery and / or a battery bag. The better the flexibility, the easier it is for the battery and / or the flexible battery bag to bend.
[0047] Battery bag film
[0048] Figure 1 This is a diagram schematically showing a cross section of a film according to an embodiment of the present invention.
[0049] The battery bag film provided by the exemplary implementation example of the present invention includes: a barrier layer 300, which is made of metal and has surface-treated sides; adhesive layers 200, 400, which are formed on both sides of the above-mentioned barrier layer; and functional fabric layers 100, 500, which are formed on both sides of the above-mentioned adhesive layers 200, 400, and the difference between the longitudinal direction (MD, Machine direction) breaking strength and the transverse direction (TD, Transverse direction) breaking strength is less than 40N / 15mm.
[0050] A battery bag film provided in one embodiment of the present disclosure includes: a sealing layer 500; an inner surface adhesive layer 400, laminated on the sealing layer 500; a barrier layer 300, laminated on the inner surface adhesive layer 400; an outer surface adhesive layer 200, laminated on the barrier layer 300; and an outer layer 100, formed on the outer surface adhesive layer 200, wherein the barrier layer 300 includes: a metal layer 320; and surface treatment layers 310 and 330, respectively and evenly coated on both sides of the metal layer 320.
[0051] In one implementation example, an extruded resin layer may be further formed between the adhesive layer and the functional fabric layer. The extruded resin layer may improve the bendability, adhesiveness, insulation, etc. of the bag. The extruded resin layer comprises an olefin resin such as a polypropylene resin. The extruded resin layer may have a thickness of about 5 μm to 80 μm. Alternatively, the extruded resin layer and the sealing layer may constitute the inner layer of the battery bag film without the inner surface adhesive layer. As described above, in the absence of an inner surface adhesive layer, the extruded resin layer may also serve as an inner surface adhesive layer.
[0052] In one implementation example, the barrier layer can block the entry and exit of external moisture or air and internally generated gas. The barrier layer can be made of metal with gas barrier properties without any particular limitation. The barrier layer can include one or more selected from metal films and metal vapor-deposited layers. In this case, metal foil can be used as the metal film, and the metal vapor-deposited layer can be made by vacuum evaporation on a separate plastic film, for example, polyethylene terephthalate (PET), polyethylene (PE) or polypropylene (PP) films.
[0053] In one implementation example, the difference between the longitudinal (MD, Machine direction) breaking strength and the transverse (TD, Transverse direction) breaking strength of the above-mentioned film is 40N / 15mm or less. More specifically, the difference between the longitudinal (MD) breaking strength and the transverse (TD) breaking strength of the above-mentioned film can be 5N / 15mm or more, 10N / 15mm or more, 15N / 15mm or more, 20N / 15mm or more, 23N / 15mm or more; 40N / 15mm or less, 35N / 15mm or less, 30N / 15mm or less, 25N / 15mm or less, 22N / 15mm or less, but it is not limited thereto.
[0054] The preparation method of the present invention is different from the existing method of repeatedly performing each process in the order of coating, drying and winding. According to the preparation method of the present invention, the present invention adopts a 1P3C (1Pass 3Coating) line method that uses one device to perform more than three coating processes. As a result, when the fabric is transferred, the operating loss (Loss) and the probability of process defects can be reduced. In addition, the method of the present invention can increase the process speed, reduce the number of windings, and reduce the stress on the film. Therefore, the tensile curve of the film can be prevented from changing by reducing the pulling force of the driving roller used to transfer the film, thereby preventing the longitudinal (MD) mechanical strength and transverse (TD) mechanical strength of the film from changing.
[0055] In one implementation example, the functional fabric layer formed on one side of the bonding layer is an outer layer made of synthetic resin fabric, and the functional fabric layer formed on the other side of the bonding layer is a sealing layer made of sealing fabric.
[0056] In one implementation example, the sealing layer is provided with sealing properties by thermal bonding after the battery is built into the inner layer, and may include a sealing resin for thermal bonding.
[0057] In one implementation example, the transverse direction (TD) rupture strength of the above-mentioned film is 250N / 15mm or less. More specifically, the transverse direction (TD) rupture strength of the above-mentioned film can be 150N / 15mm or more, 160N / 15mm or more, 170N / 15mm or more, 180N / 15mm or more, 190N / 15mm or more, 200N / 15mm or more, 210N / 15mm or more, 220N / 15mm or more, 221N / 15mm or more; 250N / 15mm or less, 240N / 15mm or less, 230N / 15mm or less, 221N / 15mm or less, but is not limited thereto.
[0058] In one implementation example, the difference between the longitudinal (MD) elongation and the transverse (TD) elongation of the film is 6% or less. More specifically, the difference between the longitudinal (MD) elongation and the transverse (TD) elongation of the film can be 0% or more, 1% or more, 2% or more, 3% or more; 6% or less, 5% or less, 4% or less, 3% or less, but is not limited thereto.
[0059] In one implementation example, the product of the difference (N / 15 mm) between the longitudinal (MD) breaking strength and the transverse (TD) breaking strength of the above-mentioned film and the difference (%) between the longitudinal (MD) elongation and the transverse (TD) elongation of the above-mentioned film is 240 or less. More specifically, the product of the difference (N / 15 mm) in breaking strength and the difference (%) in elongation can be 5 or more, 10 or more, 15 or more, 20 or more, 25 or more, 30 or more, 35 or more, 40 or more, 45 or more, 50 or more, 55 or more, 60 or more, 65 or more, 70 or more, 75 or more, 80 or more, 85 or more, 90 or more, 95 or more, 99 or more; 200 or less, 190 or less, 180 or less, 170 or less, 160 or less, 150 or less, 140 or less, 130 or less, 120 or less, 110 or less, 100 or less, 99 or less, but is not limited thereto. If the product of the difference in breaking strength (N / 15mm) and the difference in elongation (%) is within the above range, the battery bag film has uniform physical properties in the longitudinal direction (MD) and the transverse direction (TD), and the stress borne by the film can be uniformly dispersed during the molding and processing steps of the battery bag film. As a result, the phenomenon of accelerated cracking due to stress concentration in one direction is delayed, and the moldability and durability can be improved.
[0060] In one implementation example, the longitudinal (MD) formability and transverse (TD) formability of the above-mentioned film are both above 16.5 mm. When measuring the depth of the test piece cut from the battery bag film after forming, if 10 out of 10 are not broken at their depth, a deeper depth is applied. In this case, as long as one breaks, the depth before the break is taken as the maximum depth, which is called formability. More specifically, the longitudinal (MD) formability and transverse (TD) formability of the above-mentioned film can be above 16.5 mm, but are not limited to this. When the battery bag film is formed, the formed shape is a rectangle (for example, a transverse length of 190 mm and a longitudinal length of 90 mm) rather than a square. For example, the longitudinal (MD) formability of the film means that the formed rectangular shape has a transverse length of 190 mm (TD direction) and a longitudinal length of 90 mm (MD direction). Transverse (TD) formability means that the formed rectangular shape has a transverse length of 190 mm (MD direction) and a longitudinal length of 90 mm (TD direction).
[0061] In one implementation example, for example, the metal constituting the barrier layer, specifically, the metal constituting the metal film or the vapor-deposited layer may be one or more selected from the group consisting of aluminum (Al), iron (Fe), copper (Cu), nickel (Ni), tin (Sn), zinc (Zn), indium (In), and tungsten (W) (single metal or a mixture of single metals) or an alloy (alloy) of two or more selected therefrom. In one implementation example, the metal of the barrier layer is aluminum or an aluminum alloy. In addition to the barrier property against water vapor or other gases, the barrier layer also requires properties such as formability. Moreover, in order to obtain corrosion resistance, the barrier layer may be surface treated with phosphoric acid, chromium, etc.
[0062] In one implementation example, the outer layer comprises one or more resins selected from the group consisting of polyethylene terephthalate (PET) resin and polyamide resin. The outer layer requires properties such as heat resistance, pinhole resistance, chemical resistance, wear resistance, formability and insulation. The outer layer may be composed of multiple layers. In one implementation example, the outer layer is made of polyethylene terephthalate (PET) resin and polyamide resin.
[0063] In one implementation example, the sealing layer comprises one or more polyolefin resins selected from the group consisting of polypropylene, low-density polyethylene, linear low-density polyethylene, very low-density polyethylene, medium-density polyethylene, high-density polyethylene, polybutene, and ethylene / propylene copolymer. Considering that the sealing layer is in contact with the electrolyte, in addition to heat resistance, cold resistance, hot adhesiveness, and formability, the sealing layer requires properties such as electrolytic resistance and insulation resistance. The sealing layer may be composed of multiple layers.
[0064] In one implementation example, in order to improve the corrosion resistance of the metal, the surface treatment layer may be surface treated with phosphoric acid, chromium, zirconium, cerium, lanthanum, etc.
[0065] In one implementation example, the adhesive layer may include one or more of epoxy adhesive, polyurethane adhesive, phenol resin adhesive, polyester adhesive, and polyolefin adhesive. As an embodiment, the inner surface adhesive layer and the outer surface adhesive layer may have a thickness of 0.5 μm to 10 μm respectively.
[0066] In one implementation example, the barrier layer may have a thickness of 5 μm to 100 μm. When the thickness of the barrier layer is less than 5 μm, it will be difficult to realize a battery bag of a secondary battery. When the thickness of the barrier layer is greater than 100 μm, the battery capacity may be sharply reduced in a bendability test of the battery bag.
[0067] In one implementation example, the outer layer may have a thickness of 5 μm to 50 μm.
[0068] In one implementation example, the sealing layer may have a thickness of 5 μm to 100 μm.
[0069] In one embodiment, an extruded resin layer may be further formed between the inner surface adhesive layer and the sealing layer. The extruded resin layer may improve the flexibility, adhesiveness, insulation, etc. of the bag. As one embodiment, the extruded resin layer may include an olefin resin such as a polypropylene resin. As another embodiment, the inner layer of the battery bag film may be formed by the extruded resin layer and the sealing layer without the inner surface adhesive layer. As described above, in the absence of an inner surface adhesive layer, the extruded resin layer may also serve as an inner surface adhesive layer. In one implementation example, the extruded resin layer may have a thickness of 5 μm to 80 μm.
[0070] Battery Bag
[0071] The battery bag film according to one embodiment of the present invention has excellent gas barrier properties, flexibility, electrolytic resistance, and thermal adhesion, and is therefore suitable for battery bag applications.
[0072] A battery bag provided by yet another exemplary implementation of the present invention includes the film for a battery bag according to an embodiment of the present invention.
[0073] Preparation method of film for battery bag
[0074] Another exemplary implementation example of the present invention provides a method for preparing a battery bag film, which includes: a two-side surface treatment step, in which both sides of a metal fabric used to form a barrier layer are surface treated; a one-side coating step, in which an adhesive is applied to one side of the surface-treated metal fabric to form an adhesive layer; and a bonding step, in which a functional fabric is bonded to one side of the adhesive layer to form a functional fabric layer.
[0075] The preparation method of the present invention is different from the existing method of repeatedly performing each process in the order of coating, drying and winding. According to the preparation method of the present invention, the present invention adopts a 1P3C (1Pass 3Coating) line method that uses one device to perform more than three coating processes. As a result, when the fabric is transferred, the operating loss (Loss) and the probability of process defects can be reduced. In addition, the method of the present invention can increase the process speed, reduce the number of windings, and reduce the stress on the film. Therefore, the tensile curve of the film can be prevented from changing by reducing the pulling force of the driving roller used to transfer the film, thereby preventing the longitudinal (MD) mechanical strength and transverse (TD) mechanical strength of the film from changing.
[0076] The above-mentioned two-sided surface treatment step refers to a surface treatment process of performing a first coating and a second coating on the two sides of the metal fabric used to form the metal layer. The above-mentioned two-sided surface treatment step is performed by a two-sided double coating device including a first coater and a second coater.
[0077] The above-mentioned two-sided surface treatment steps may include: a fabric supply process, unwinding and supplying the wound metal fabric; a foreign matter removal process, removing foreign matter on the surface of the supplied metal fabric; a tension adjustment process, adjusting the tension of the metal fabric to remove surface foreign matter; and a double-sided double coating process, coating both sides of the metal fabric while maintaining a specified tension.
[0078] The foreign matter removal process may include a first foreign matter removal process, in which both sides of the metal fabric are subjected to discharge treatment to remove oil. Furthermore, the foreign matter removal process may also include a pinhole inspection process, in which pinholes are confirmed to be generated on both sides of the metal fabric after the oil is removed. Furthermore, the foreign matter removal process may also include a second foreign matter removal process, in which foreign matter is removed from both sides of the metal fabric after the pinhole inspection by a roller.
[0079] In the first coating of water-based and solvent-based coating liquids applied to one side of the metal fabric by the first coater in a combined manner of direct coating (Direct coating) and reverse kiss coating (RKC, Reverse Kiss Coating), the physical properties and changes of the coating liquid need to be considered. For the other side of the metal fabric, a second coating of the coating liquid can be applied by RKC and film up / down coating. On the other hand, the uniformity of coating and the working speed can be improved by adjusting the position of the substrate contact surface and the coating roller (Coating Roll) and the doctor (Doctor). In particular, in order to precisely control the coating agent, the viscosity of the coating agent can be adjusted by constructing a chamber method (closed piping), thereby preventing the entry of foreign matter from the source.
[0080] Between the above-mentioned two-sided surface treatment step and the one-side coating step for forming an adhesive layer, there is also included: a physical property stabilization drying step, in which the metal fabric coated on both sides is dried in a floating manner to stabilize the physical properties; a cooling step, in which the dried metal fabric is cooled; and a surface inspection step, in which the surface of the cooled metal fabric is inspected.
[0081] After the two-side surface treatment step is completed, the metal fabric coated on both sides can be dried by floating to stabilize the physical properties. In this case, the air floating method can be used as a drying method to dry the coated substrate in a non-contact manner in a floating state. In this way, the metal fabric treated on both sides can be dried while minimizing contact with structures such as transfer rollers. Then, after the dried metal fabric is cooled, the surface of the cooled metal fabric can be inspected.
[0082] The one-side coating step for forming the above-mentioned adhesive layer refers to the process of coating the adhesive on one side of the metal fabric treated by the two-coating surface treatment, which is performed by the third coating machine and is prepared for bonding after drying and other processes. After coating the adhesive, the metal fabric coated with the adhesive is dried to form the adhesive layer, and then the thickness of the dried adhesive layer can be measured and the adhesive force can be strengthened by corona treatment of the surface of the adhesive layer.
[0083] After the above-mentioned laminating step, one embodiment of the above-mentioned method may further include an inner surface adhesive layer coating step, in which an inner surface adhesive is coated on the other side of the above-mentioned metal fabric that is not laminating the outer layer to form an inner surface adhesive layer. And, after the above-mentioned coating step, one embodiment may further include a drying step. One embodiment may further include a step of laminating a sealing layer fabric to the lower part of the above-mentioned inner surface adhesive layer.
[0084] In one embodiment, in order to prevent the fabric used in each step before the outer layer bonding step from being dented and / or pressed, the above method may include a total of no more than two winding steps. Specifically, the above metal fabric may be wound no more than twice in total. More specifically, the above winding step may include a total of one winding step. In one embodiment, the above winding step may be included after the above outer surface adhesive layer coating step and before the above outer layer fabric bonding step. For example, the above winding step may be Figure 2 Execute step 10 of .
[0085] In one embodiment, the step of laminating the outer layer fabric to the upper part of the outer surface adhesive layer and the step of laminating the sealing layer fabric to the lower part of the inner surface adhesive layer are respectively the process of laminating the functional fabric to one side of the metal fabric coated with the adhesive, and the sealing layer fabric mainly used to stabilize the heat resistance and cold resistance of the battery can be laminated to the inner side, and the outer layer fabric used for heat resistance, pinhole resistance and wear resistance can be laminated to the outer side. In one embodiment, each of the above laminating steps can laminate the outer layer fabric or the sealing fabric prepared in advance.
[0086] Between the third coating step and the bonding step, the following may also be included: an adhesive drying step, in which the metal fabric coated with the adhesive is dried to form an adhesive layer; an adhesive layer thickness measuring step, in which the thickness of the dried adhesive layer is measured; and an adhesive layer surface treatment step, in which the surface of the adhesive layer is subjected to corona treatment to enhance the adhesive force.
[0087] After the above-mentioned laminating step, a surface inspection step may be further included to inspect the surface of the above-mentioned sealing layer or outer layer.
[0088] On the other hand, in order to minimize the occurrence of foreign matter and scratches during the transfer of each fabric, a tendency structure that separates the guide roller from the substrate contact roller and the shaft and a shaft structure that operates as an integrated type can be adopted. The ordinary drive method of the guide roller is to transmit the rotation transmitted by the motor to the shaft-integrated guide roller and drive it at a speed of 1:1, while the tendency drive method separates the guide roller and the shaft to compensate for the small rotation speed of the roller, which can be applied to the required range.
[0089] On the other hand, the rewinder section and the unwinder section (fabric supply section) can be constructed separately so that they can be operated separately when a problem occurs in the operation of the equipment due to a problem with the equipment.
[0090] Moreover, as an embodiment, the present disclosure may further include a aging step. In the process of preparing the battery bag, the aging step is a necessary process for improving the reliability of adhesion, electrolytic resistance, peel strength, etc., but it takes a long time, so the optimal aging process is particularly important. Preferably, in terms of productivity, only one aging process is performed for the final structure of the battery bag to prepare the product. Specifically, the method may include a aging step. More specifically, the method may not perform the aging step after the two-sided surface treatment step and apply the adhesive to one side of the surface-treated metal fabric, and the aging step may be included after the bonding step of the sealing layer. For example, if the aging step includes a two-sided surface treatment step before the bonding step, as the film is exposed to the air for more than a specified time during the preparation process, the unlaminated surface treatment agent may fall off. For example, if the adhesive layer molding step includes a aging step, as the adhesive layer undergoes a partial reaction, the adhesion phenomenon of the adhesive layer adhering to other layers may occur.
[0091] The first intermediate structure of the battery bag film can be constituted as a structure of outer layer / adhesive layer / surface treatment layer / barrier layer / surface treatment layer / adhesive layer, and the second intermediate structure can be constituted as a structure of outer layer / adhesive layer / surface treatment layer / barrier layer / surface treatment layer. Preferably, if two agings are unavoidable, the second intermediate structure is subjected to the first aging, and then the final structure is subjected to the second aging. In the case where the first intermediate structure is subjected to the first aging, problems in the preparation process, reduction in physical properties, and other problems may arise. More specifically, in the product in which the first intermediate structure is subjected to the first aging, due to the partial reaction of the inner surface adhesive layer (sealing layer side), adhesion of the inner surface adhesive layer to the outer layer may occur.
[0092] Furthermore, when the sealing layer is formed after the first aging, it is necessary to strengthen the adhesive force of the inner surface adhesive layer through an additional process, and therefore there is a risk of reduced productivity.
[0093] On the other hand, in the process of transferring the fabric, in order to minimize the occurrence of foreign matter and scratches, a suction roller can be used in the tension control zone. In order to prevent the appearance defects (dents, scratches, etc.) caused by foreign matter adhering to the roller during operation, a contact cleaning roller for removing foreign matter can be used.
[0094] In one implementation example, the transfer of the battery bag film can be performed by a driving roller, and all or part of the driving roller is a suction roller. A plurality of holes are formed in the suction roller for sucking air from the outer peripheral surface. As the holes suck air, the suction roller can pull the film to contact the outer peripheral surface.
[0095] In one embodiment, the pulling force applied by the suction roller to the battery bag film is 0.02 kgf / cm 2Up to 2.5kgf / cm 2 .
[0096] In one implementation example, during the preparation process of the battery pouch film, the metal fabric of the battery pouch film is wound twice or less in total.
[0097] Battery bag film preparation device
[0098] Another exemplary implementation example of the present invention provides a battery bag film preparation device including: a two-sided surface treatment device, including a first coater 3 and a second coater 4, for surface treating both sides of a metal fabric used to form a barrier layer; a third coater 7, for applying an adhesive to one side of the surface-treated metal fabric; and a bonding portion 9, for bonding a functional fabric to one side of the adhesive layer.
[0099] Figure 2 Schematic diagram of a battery bag film preparation device according to an embodiment of the present invention.
[0100] The two-sided surface treatment device may include a fabric supply unit 1, a foreign matter removal device 2, a tension adjustment unit, a first coating machine 3, and a second coating machine 4. The fabric supply unit 1 is used to unwind and supply the wound metal fabric. The foreign matter removal device 2 is used to remove foreign matter on the surface of the supplied metal fabric. The tension adjustment unit is used to adjust the tension of the metal fabric from which the foreign matter is removed. The first coating machine 3 and the second coating machine 4 are used to coat both sides of the metal fabric while maintaining a specified tension.
[0101] The foreign matter removal device 2 may include a first foreign matter removal unit for performing discharge treatment on both sides of the metal fabric to remove oil. In addition, it may include a pinhole inspection unit for confirming whether pinholes are generated on both sides of the metal fabric after the oil is removed. It may also include a second foreign matter removal unit for removing foreign matter from both sides of the metal fabric by rollers when the confirmation result is normal.
[0102] A physical property stabilization drying section 5 can be formed between the above-mentioned double-sided surface treatment device and the third coater 7, and the metal fabric coated on both sides is dried by floating to stabilize the physical properties. In this case, the air floating method can be used as a drying method to dry the coated substrate in a non-contact manner in a floating state. In this way, the metal fabric coated on both sides can be dried while minimizing the contact with structures such as transfer rollers. Then, after the dried metal fabric is cooled by the cooling section 6, the surface of the cooled metal fabric can be inspected by the surface inspection section.
[0103] Between the third coater 7 and the laminating section 9, there may also be included: an adhesive drying section 8 for drying the metal fabric coated with the adhesive to form an adhesive layer; an adhesive layer measuring section for measuring the thickness of the dried adhesive layer; and an adhesive layer surface treatment section for performing corona treatment on the surface of the adhesive layer to enhance the adhesive force.
[0104] In addition to the laminating unit 9, a surface inspection unit may be included to inspect the surfaces of the sealing layer and the outer layer.
[0105] According to the needs, Figure 2 The laminating section 9 and the final winding section (End, 2 nd A fourth coater (not shown) for applying adhesive to the other side of the surface-treated metal fabric, a drying section (not shown), a functional layer laminating section (not shown), an extrusion section (including co-extrusion) (not shown), etc. are additionally added between the re-wind and the coating section.
[0106] Hereinafter, the embodiments are described in detail with reference to the preferred embodiments of the present invention so that those skilled in the art can easily implement the present invention. However, the present invention can be implemented in various embodiments and is not limited to the embodiments described herein.
[0107] {Example}
[0108] <Preparation Example 1> Preparation of battery bag film
[0109] The two sides of the aluminum foil metal fabric used to form the barrier layer are surface treated by the first coating and the second coating. Then, the metal fabric with the coated surfaces on both sides is dried by floating to stabilize the physical properties. Subsequently, after the dried metal fabric is cooled, a polyurethane adhesive is applied to one side of the surface-treated metal fabric by a third coater to form an adhesive layer. Then, a pre-prepared PET film / polyamide film is attached to one side of the adhesive layer to form an outer layer. An adhesive is applied to the other side of the adhesive layer and an unstretched polypropylene film is attached to form a sealing layer, thereby preparing a film for a battery bag and winding it (Example 1: a sample at 700m point based on the branch pipe part on a winding roller with a total length of 2000m; Example 2: a sample at 1300m point based on the branch pipe part on a winding roller with a total length of 2000m; Example 3: a sample at 1900m point based on the branch pipe part on a winding roller with a total length of 2000m).
[0110] <Preparation Example 2> Preparation of battery bag film
[0111] The two sides of the aluminum foil metal fabric used to form the barrier layer are surface treated by the first coating, and then wound up after drying. The other side of the aluminum foil metal fabric used to form the barrier layer is surface treated by the second coating, and then wound up after drying. After applying a polyurethane adhesive to one side of the aluminum foil metal fabric with both sides treated on the surface and drying, a pre-prepared PET film / polyamide film is attached to form an outer layer and wound up. Next, an inner surface adhesive is applied, and after drying, an inner layer (sealing film) is attached and wound up (Comparative Example 1: a sample at 700m point based on the branch pipe part on a winding roller with a total length of 2000m; Comparative Example 2: a sample at 1300m point based on the branch pipe part on a winding roller with a total length of 2000m; Comparative Example 3: a sample at 1900m point based on the branch pipe part on a winding roller with a total length of 2000m).
[0112] <Experimental Example 1> Evaluation of the Difference between the Physical Properties in the Machine Direction (MD) and the Physical Properties in the Transverse Direction (TD) of the Film
[0113] The battery pouch films prepared in Preparation Example 1 and Preparation Example 2 were evaluated for differences in physical properties in the machine direction (MD) and in the transverse direction (TD).
[0114] More specifically, a 130 mm x 15 mm test piece was taken from the winding roll along the longitudinal direction (MD) and transverse direction (TD). The tensile strength of the taken test piece was measured using a UTM (manufacturer: INSTRON) universal testing machine based on ASTM D638 at a tensile speed of 50 mm / min and a clamp spacing of 50 mm. The strength of the test piece at the time of cutting and breaking was measured as the breaking strength, and the elongation was measured by measuring the length increased after breaking after marking a length of 30 mm in the middle of the taken test piece.
[0115] The results are as follows Figure 3 As shown in Tables 1 and 2 below. Figure 3 FIG. 1 is a stress-strain curve of a battery bag film according to an embodiment of the present invention.
[0116] Table 1
[0117] Breaking strength (N / 15mm) Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Machine Direction (MD) 221 205 209 200 209 216 Horizontal direction (TD) 231 238 232 275 255 268 Difference 10 33 23 75 46 52
[0118]
Table 2
[0119] Elongation(%) Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Machine Direction (MD) 73 70 67 90 73 83 Horizontal direction (TD) 70 73 70 63 66 64 Difference 3 3 3 27 7 19
[0120] according to Figure 3 From the above Tables 1 and 2, it can be confirmed that the battery pouch film of the present invention not only has excellent mechanical strength but also has low variation in mechanical strength.
[0121] <Experimental Example 2> Evaluation of the Difference Between the Longitudinal (MD) Formability and the Transverse (TD) Formability of the Film
[0122] The battery pouch films prepared in Preparation Example 1 and Preparation Example 2 were evaluated for differences in physical properties in the machine direction (MD) and in the transverse direction (TD).
[0123] More specifically, a 266 mm x 240 mm test piece was taken from the winding roll along the longitudinal direction (MD) and the transverse direction (TD). The taken test piece was formed into a rectangular shape (lateral length 190 mm, longitudinal length 90 mm) (the R value was different for each test piece in the chrome-coated high-molding bag formability evaluation device, but the corner R value used as the benchmark was 4).
[0124] When the depth after forming is measured, if none of 10 out of 10 cracks at the depth, a deeper depth is used. In this case, if only one crack occurs, the depth before the crack is defined as the maximum depth to define the formability.
[0125] The longitudinal (MD) formability means that the rectangular shape formed has a transverse length of 190 mm (TD direction) and a longitudinal length of 90 mm (MD direction). The transverse (TD) formability means that the rectangular shape formed has a transverse length of 190 mm (MD direction) and a longitudinal length of 90 mm (TD direction). The results are shown in Table 3 below.
[0126] Table 3
[0127] Formability(mm) Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Machine Direction (MD) 17.0 17.0 16.5 12.0 13.0 12.5 Horizontal direction (TD) 17.0 16.5 17.0 11.5 12.0 10.5
[0128] From Table 3 above, it can be confirmed that the battery pouch film of the present invention has the most excellent moldability.
[0129] Although the exemplary embodiments of the present invention have been described with reference to the above preferred embodiments, various modifications and variations can be made without departing from the scope of the present invention. Therefore, all modifications and variations within the scope of the present invention belong to the scope of protection claimed by the present invention.
Claims
1. A battery bag film, characterized in that: include: The barrier layer is made of metal and has surface treatment on both sides; Adhesive layers formed on both sides of the barrier layer; and The functional fabric layer is formed on both sides of the adhesive layer. The difference between the breaking strength in the machine direction (MD) and the breaking strength in the transverse direction (TD) is 40 N / 15 mm or less.
2. The battery bag film according to claim 1, characterized in that: The functional fabric layer formed on one side of the adhesive layer is an outer layer made of synthetic resin fabric. The functional fabric layer formed on the other side of the bonding layer is a sealing layer made of sealing fabric.
3. The battery bag film according to claim 1, characterized in that: The film has a transverse direction (TD) breaking strength of 250 N / 15 mm or less.
4. The battery bag film according to claim 1, characterized in that: The difference between the elongation in the machine direction (MD) and the elongation in the transverse direction (TD) of the film is 6% or less.
5. The battery bag film according to claim 1, characterized in that: The product of the difference between the longitudinal (MD) breaking strength and the transverse (TD) breaking strength of the above-mentioned film and the difference between the longitudinal (MD) elongation and the transverse (TD) elongation of the above-mentioned film is less than 240, wherein the unit of the difference in breaking strength is N / 15mm, and the unit of the difference in elongation is %.
6. The battery bag film according to claim 1, characterized in that: The film has a longitudinal (MD) formability and a transverse (TD) formability of 16.5 mm or more.
7. The battery bag film according to claim 2, characterized in that: The metal of the barrier layer is aluminum or aluminum alloy. The outer layer comprises one or more resins selected from the group consisting of polyethylene terephthalate resin and polyamide resin. The sealant layer comprises one or more polyolefin resins selected from the group consisting of polypropylene, low-density polyethylene, linear low-density polyethylene, very low-density polyethylene, medium-density polyethylene, high-density polyethylene, polybutene and ethylene / propylene copolymer.
8. A battery bag, characterized in that: The invention comprises the battery pouch film according to any one of claims 1 to 7.
9. A method for preparing a battery bag film, for preparing the battery bag film according to any one of claims 1 to 7, characterized in that: include: a double-side surface treatment step, performing surface treatment on both sides of the metal fabric used to form the barrier layer; a side coating step of applying an adhesive to one side of the surface-treated metal fabric to form an adhesive layer; and The laminating step is to laminate the functional fabric onto one side of the adhesive layer to form a functional fabric layer.
10. The method for preparing a battery bag film according to claim 9, characterized in that: The battery bag film is conveyed by a driving roller, and all or part of the driving roller is a suction roller.
11. The method for preparing a battery bag film according to claim 10, characterized in that: The pulling force applied by the suction roller to the battery bag film is 0.02 kgf / cm 2 Up to 2.5kgf / cm 2 .
12. The method for preparing a battery bag film according to claim 10, characterized in that: In the process of preparing the battery pouch film, the metal fabric of the battery pouch film is wound twice or less in total.
Citation Information
Patent Citations
Packaging material for battery
CN106663755A
Preparation method of aluminum-plastic composite film for lithium battery flexible package film