Preparation method of boron-doped diamond

High boron-doped diamond is prepared through sol-condensation technology and electric field-assisted sintering, which solves the problems of low efficiency of the CVD method and insufficient boron doping concentration of the HPHT method, and achieves high activity and excellent electrochemical performance, which is suitable for sewage treatment.

CN118771371AActive Publication Date: 2024-10-15ZHENGZHOU SINO CRYSTAL DIAMOND CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411122380.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-10-15
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The existing boron-doped diamond prepared by the low-pressure chemical vapor deposition (CVD) method has low efficiency and high energy consumption when electrochemically oxidizing and degrading organic wastewater, and the low boron doping concentration prepared by the high-temperature and high-pressure method (HPHT) affects the electrochemical performance. , limiting its industrial promotion.

Method used

The metal catalyst is prepared in situ using sol-condensation technology, using electric field-assisted sintering, using graphene, nano-boron nitride and o-carborane as raw materials, combined with polymer network gel technology and hydrogen reduction to form a high boron doping amount. Boron doped diamond.

Benefits of technology

The highly active boron-doped diamond has high thermal shock strength, wear resistance and chemical inertness, improves electrical conductivity, and is suitable for sewage treatment in the electrochemical field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771371A_ABST
    Figure CN118771371A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of superhard materials, and particularly relates to a preparation method of boron-doped diamond, graphene, nano boron nitride, o-carborane and the like are taken as raw materials, a metal catalyst is prepared in situ by adopting a sol-condensation technology, and a high-activity graphite column is prepared by utilizing electric field assisted sintering; and synthesizing the graphite column into the boron-doped diamond with high boron doping amount by using a cubic press.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of superhard materials, and in particular relates to a method for preparing boron-doped diamond. Background Art

[0002] Since BDD is superior to ordinary diamond in terms of heat resistance, wear resistance, chemical inertness, oxidation resistance and compressive strength, with the rapid development of modern industry in recent years, boron-containing diamond has shown great application prospects in various industries and has gradually become an ideal material for the development of electron emission electrodes, photodetectors, field effect transistors and vacuum tunnel microscope probes. The discovery of its superconducting properties has further expanded the utilization prospects of boron-containing diamond. Its good wear resistance and grinding characteristics also make BDD extremely valuable in the application of hard and tough materials in the field of process applications.

[0003] As an electrode material with excellent performance, BDD can oxidize water molecules to produce a large number of high-oxidation-position hydroxyl radicals (·OH) under the action of an electric field. Therefore, researchers apply BDD electrodes as anodes of electrochemical advanced oxidation technologies to the field of environmental pollution control. Similar to other advanced oxidation technologies, such as ozone oxidation, Fenton oxidation, and photocatalytic oxidation, the hydroxyl radicals produced during the reaction process thoroughly mineralize and oxidize various organic pollutants or microorganisms in the water to generate carbon dioxide, water, and inorganic ions, thereby achieving the purpose of degrading various high-concentration, toxic, and difficult-to-degrade sewage. In recent years, research on electrochemical treatment of organic pollutants based on BDD anodes has been very extensive, involving phenols, fuels, surfactants, pesticides, organic acids, medicines, and biochemical pretreatment of wastewater. At the same time, there are also literature reports on the use of BDD in wastewater treatment of heavy metal ions at cyanide anodes. At present, high-temperature and high-pressure methods (HPHT) and low-pressure chemical vapor deposition (CVD) are commonly used methods for preparing BDD electrodes. The CVD method for preparing BDD has the advantages of easy control of boron doping concentration and good diamond purity. The boron doping concentration can reach 1020 mg / L, and its hole mobility can reach 1500 cm at room temperature. 2 v -1 s -1 , the resistivity is 10 -2 Ω·cm, making it possible to use the electrode in the electrochemical field for sewage treatment. However, the CVD method has a small active area and slow mass transfer rate for BDD production. It has low efficiency and high energy consumption in electrochemical oxidation and degradation of organic wastewater, which limits its industrial promotion. Therefore, it has been in the research stage and has not been industrialized. Compared with the CVD method, the HPHT method has the advantages of short synthesis cycle and low cost when synthesizing BDD. However, the BDD prepared by the HPHT method currently exhibits low conductivity due to the low boron doping concentration, which in turn affects its electrochemical performance. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing boron-doped diamond, using graphene, nano-boron nitride, ortho-carborane and the like as raw materials, adopting sol-condensation technology to in-situ prepare metal catalysts, utilizing electric field assisted sintering to prepare highly active graphite pillars, and utilizing a six-sided top press to synthesize the graphite pillars into boron-doped diamonds with a high boron doping amount.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] A method for preparing boron-doped diamond comprises the following steps:

[0007] S1. dissolving ortho-carborane in cyclohexane and mixing well, then sequentially adding graphene and nano-boron nitride thereto and treating in an ultrasonic device for 2h until the mixture is well mixed;

[0008] S2. The solution after ultrasonic treatment in step S1 is placed in an oven at 40-60° C. for 8-12 hours to remove cyclohexane, dissolve ortho-carborane in cyclohexane, and then volatilize the cyclohexane, and ortho-carborane will form a coating on the surface of graphene;

[0009] S3. Dissolve N, N'-methylenebisacrylamide, acrylamide, cobalt nitrate hexahydrate, iron nitrate nonahydrate, nickel nitrate hexahydrate, and citric acid in 80-100 ml of distilled water and stir evenly for use. In order to evenly disperse graphene and nano-boron nitride, the mixed solution is added with the graphene treated in step S2 to the solution, and treated in an ultrasonic mechanical stirring device for 2 hours until evenly mixed. Then, ammonium persulfate solution and tetramethylethylenediamine solution are added thereto and stirred to form a gel, wherein ammonium persulfate is an initiator that can cause N, N'-methylenebisacrylamide and acrylamide to undergo a cross-linking reaction, and tetramethylethylenediamine is a catalyst that accelerates the above reaction. The reaction solidifies the entire solution and turns it into a gel to form a coprecipitation effect, which can be called a polymer network gel technology. Citric acid is a complexing agent that forms a metal ion complex, which can also be understood as a coprecipitation of iron, cobalt, and nickel; the iron, cobalt, and nickel alloy is grown in situ on the graphite surface by hydrogen reduction;

[0010] S4. The gel was placed in an oven at 120°C for 10 to 15 hours, the dry gel was crushed into powder with a fineness of less than 325# by a ball mill, and then reduced in a furnace in a hydrogen atmosphere at 600 to 800°C for 3 to 5 hours to be pressed into a graphite column, and then treated in an electric field of 800 to 3000V for 3 to 5 hours;

[0011] S5. The graphite column treated in step S4 is treated at a pressure of 3.5 to 4.5 GPa and 1300 to 1500° C. for 5 to 20 min using a six-sided top press to synthesize boron-doped diamond.

[0012] Furthermore, in step S1, both graphene and nano-boron nitride are single-layer or multi-layer structures, and the mass ratio of o-carborane, graphene, and nano-boron nitride is 1-6:20-60:1-10.

[0013] Furthermore, in the steps S2 and S3, the ultrasonic treatment is performed at an ultrasonic power of 1000 to 3000 W and a mechanical stirring speed of 10 to 40 rpm.

[0014] Furthermore, in step S3, the mass ratio of N,N'-methylenebisacrylamide, acrylamide, cobalt nitrate hexahydrate, ferric nitrate nonahydrate, nickel nitrate hexahydrate, and citric acid is 0.2-0.4:3-7:10-20:20-30:13-20:2-6, and the mass ratio of ammonium persulfate solution to tetramethylethylenediamine solution is 0.2-0.5:0.1-0.3.

[0015] The mechanism of the present invention is: graphene containing orthocarborane and single multilayer boron nitride on the surface is converted into boron-containing diamond with high boron content under the action of catalyst (iron, cobalt, nickel) at high temperature and high pressure. The boron source has two sources: 1 orthocarborane and 2 nano boron nitride. The catalyst is an iron-cobalt-nickel catalyst prepared on the surface of raw materials such as graphene using polymer network gel and hydrogen reduction technology.

[0016] The advantages of the present invention are as follows: compared with the prior art, the present invention uses graphene, nano boron nitride, ortho-carborane and the like as raw materials, adopts sol-condensation technology to in-situ prepare metal catalysts, and utilizes electric field assisted sintering to prepare highly active graphite columns. The synthesized diamond has high thermal shock strength, high wear resistance, high chemical inertness and electrical conductivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is the XRD spectrum of boron-doped diamond prepared by the method of Example 1 of the present invention.

[0018] Figure 2 This is a SEM image of boron-doped diamond prepared by the method of Example 1 of the present invention. DETAILED DESCRIPTION

[0019] Example 1

[0020] like Figure 1-2 As shown, a method for preparing boron-doped diamond comprises the following steps:

[0021] 1. Weigh 10 g of o-carborane and dissolve it in 500 g of cyclohexane;

[0022] 2. Weigh 200g of single-layer or multi-layer graphene and 30g of single-layer or multi-layer nano-boron nitride, add them to the above solution, and treat them in an ultrasonic mechanical stirring device for 2h, wherein the ultrasonic power is 2000W and the mechanical stirring speed is 40rpm to mix them evenly.

[0023] 3. Place the above solution in an oven at 60°C for 12 hours to evaporate and remove the cyclohexane.

[0024] 4. Weigh 0.4g of N,N'-methylenebisacrylamide, 5g of acrylamide, 15g of cobalt nitrate hexahydrate, 23g of ferric nitrate nonahydrate, 18g of nickel nitrate hexahydrate, and 4g of citric acid, dissolve them in 100ml of distilled water, stir evenly and set aside. Add the above-treated graphene to the solution and treat it in an ultrasonic mechanical stirring equipment for 2h, where the ultrasonic power is 2000W and the mechanical stirring speed is 40rpm to mix it evenly.

[0025] 5. Take 0.3 g of 10% ammonium persulfate solution and 0.2 g of 2% tetramethylethylenediamine solution, add them to the above solution, stir for 3 hours to form a gel.

[0026] 6. The above gel was placed in an oven at 120°C for 12 hours, and then the dry gel was crushed into 325# fine powder using a ball mill.

[0027] 7. The above powder was reduced in a furnace with hydrogen atmosphere at 700°C for 4 h.

[0028] 8. The above powder was pressed into a Φ30 mm graphite column and treated under an electric field of 2000 V for 4 h.

[0029] 9. Using a six-sided top press, treat the above-treated graphite column at a pressure of 3.5 GPa and 1400° C. for 20 minutes to synthesize diamond.

[0030] Example 2

[0031] The difference between Example 2 and Example 1 is that the graphene has a single-layer structure.

[0032] Example 3

[0033] The difference between Example 3 and Example 1 is that o-carborane is not used.

[0034] Example 4

[0035] The difference between Example 4 and Example 1 is that there is no step of treating the graphite column under an electric field of 2000 V for 4 hours.

[0036] Performance Testing

[0037] According to the national standard requirements, the hardness, impact toughness, boron content and average conductivity of the boron-doped diamonds prepared in Examples 1-4 were tested respectively. The specific test results are shown in Table 1. The test process is as follows:

[0038] Diamond TTI test method: 100g of agglomerated diamond particles and steel balls are placed in a test tube, heated to 900℃ and subjected to oscillation impact at a frequency of 2000r / min. The breakage rate is calculated after impact, and the impact toughness of the sample is characterized by the number of impacts when the unbroken rate is 50%.

[0039] Boron element measurement method: Boron element is tested by inductively coupled plasma-atomic emission spectrometer;

[0040] Conductivity measurement equipment: The prepared diamond was measured using a HADFM100H powder resistivity tester.

[0041] Table 1

[0042] Sample source Diamond hardness (GPa) Impact toughness Boron content mg / L Average conductivity mS / cm Example 1 21.8 810 10.57 10.3317 Example 2 17.1 625 6.31 3.2668 Example 3 12.3 560 5.52 4.7433 Example 4 4.9 379 3.18 1.0941

Claims

1. A method for preparing boron-doped diamond, characterized in that: The following steps are involved: S1. dissolving ortho-carborane in cyclohexane and mixing well, then sequentially adding graphene and nano-boron nitride thereto and treating in an ultrasonic device for 2h until the mixture is well mixed; S2. The solution after ultrasonic treatment in step S1 is placed in an oven at 40-60°C for 8-12 h to remove cyclohexane; S3. Dissolve N,N'-methylenebisacrylamide, acrylamide, cobalt nitrate hexahydrate, iron nitrate nonahydrate, nickel nitrate hexahydrate, and citric acid in 80-100 ml of distilled water and stir evenly for use, add the graphene treated in step S2 to the solution, treat in an ultrasonic mechanical stirring device for 2 h until mixed evenly, then add ammonium persulfate solution and tetramethylethylenediamine solution thereto, and stir to form a gel; S4. Place the gel in a 120°C oven for 10-15 h, crush the dry gel into powder with a fineness of less than 325# using a ball mill, and then reduce it in a furnace in a hydrogen atmosphere at 600-800°C for 3-5 h to press it into a graphite column, and then treat it in an electric field of 800-3000 V for 3-5 h; S5. The graphite column treated in step S4 is treated at a pressure of 3.5-4.5 GPa and 1300-1500° C. for 5-20 min using a six-sided top press to synthesize boron-doped diamond.

2. The method for preparing boron-doped diamond according to claim 1, characterized in that: In the step S1, the graphene and the nano-boron nitride are both single-layer or multi-layer structures, and the mass ratio of o-carborane, graphene, and nano-boron nitride is 1-6:20-60:1-10.

3. The method for preparing boron-doped diamond according to claim 1, characterized in that: The ultrasonic treatment in steps S2 and S3 is performed at an ultrasonic power of 1000-3000 W and a mechanical stirring speed of 10-40 rpm.

4. The method for preparing boron-doped diamond according to claim 3, characterized in that: In the step S3, the mass ratio of N,N'-methylenebisacrylamide, acrylamide, cobalt nitrate hexahydrate, ferric nitrate nonahydrate, nickel nitrate hexahydrate, and citric acid is 0.2-0.4:3-7:10-20:20-30:13-20:2-6, and the mass ratio of ammonium persulfate solution to tetramethylethylenediamine solution is 0.2-0.5:0.1-0.3.

Citation Information

Patent Citations

  • Method for manufacturing boron nitride toughened polycrystalline diamond

    CN103883257A

  • Synthesis method and synthesis device of monocrystalline diamond

    CN114029002A

  • Preparation method of uniform boron-doped diamond single crystal

    CN117026372A

  • Alloyed diamond production method

    RU1345581C