Process for producing battery-grade sodium carbonate by low-temperature refining crystallization method
Through low-temperature refining crystallization method and multiple crystallization treatments, combined with carbon dioxide gas treatment and recycling of filter residue, the problems of low yield and high impurity content in the production of battery-grade sodium carbonate are solved, product purity and yield are improved, and energy consumption is reduced and cost.
Patent Information
- Application Number
- CN202410945341.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-15
AI Technical Summary
The existing battery-grade sodium carbonate production process has problems such as low yield and high content of metal impurities, especially the problem of excessive crystal water content and introduction of impurities during the cooling and crystallization process, which affects product quality and production costs.
The low-temperature refining crystallization method is adopted, and through multiple low-temperature crystallization and carbon dioxide gas treatment, the sodium carbonate crystallization is gradually precipitated, inhibiting the crystallization of sodium carbonate decahydrate, and returning the filter residue containing metal impurities to the dissolution step for further processing, reducing Drying treatment of impurities.
It improves the yield and purity of battery-grade sodium carbonate, reduces crystal water content and energy consumption, meets the standards of "T/HNSDCHYXH 001-2023 Battery Grade Sodium Carbonate", and reduces production costs.
Smart Images

Figure CN118771418A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of battery-grade sodium carbonate, and in particular to a process for producing battery-grade sodium carbonate by a low-temperature refined crystallization method. Background Art
[0002] Sodium carbonate, commonly known as soda ash, is a white crystalline solid and an important basic raw material in the chemical industry. According to the purity level, sodium carbonate can be divided into battery grade sodium carbonate and industrial grade sodium carbonate.
[0003] Battery-grade sodium carbonate is a key raw material for the preparation of positive electrode materials for sodium-ion batteries. In order to ensure the comprehensive performance of the battery, strict requirements are placed on quality indicators. For example, the purity of battery-grade sodium carbonate is required to be above 99.5%, and the higher the better; the metal impurities (such as lead, chromium, etc.) and chloride ion content contained in battery-grade sodium carbonate also need to meet the standards of "T / HNSDCHYXH 001-2023 Battery-Grade Sodium Carbonate".
[0004] Patent application number CN202211096637.6 discloses a method for the combined preparation of battery-grade sodium carbonate and basic magnesium carbonate by the soda ash industry, which includes a method for preparing battery-grade sodium carbonate using low-salt soda ash produced by the soda ash industry as a raw material, and the specific operation steps are: mixing the low-salt soda ash produced by the soda ash industry with water to obtain a Na2CO3 solution of a preset concentration; adjusting the pH of the Na2CO3 solution to alkaline using a NaOH solution of a preset concentration to obtain a mixed solution; filtering the mixed solution to remove insoluble impurities to obtain a Na2CO3 solution rich in Na + and CO3 2- The clear liquid A is cooled and crystallized, and after a preset crystallization time, it is separated by suction to obtain a filter cake and a mother liquor I; the filter cake is washed and dried to obtain a battery-grade high-purity sodium carbonate product.
[0005] In the above-mentioned step of preparing battery-grade sodium carbonate using soda ash as raw material, water is first used to dissolve Na2CO3, and then a NaOH solution is used to adjust the pH, and then the temperature is lowered and cooled to crystallize Na2CO3, and then washed and dried to obtain battery-grade sodium carbonate. This method has the following problems:
[0006] 1) During the cooling and crystallization process, sodium carbonate decahydrate (Na2CO3·10H2O) crystals will precipitate together with Na2CO3, resulting in a higher content of crystal water in the battery-grade sodium carbonate product, which can easily lead to water-soluble impurities being introduced into the product, affecting the quality and failing to meet the standards. In addition, the crystal water content is too high, resulting in high energy consumption during drying, which increases the production cost.
[0007] 2) Lead and chromium metals still remain in the filter cake obtained directly after cooling and crystallization, resulting in high content of lead and chromium in the battery-grade sodium carbonate obtained after the filter cake is dried, which does not meet the standard of battery-grade sodium carbonate; and the precipitate in the cooling and crystallization solution is thick, so that the sodium carbonate crystals are less than 30% of the total amount, and the crystallization is incomplete, which greatly reduces the yield of battery-grade sodium carbonate.
[0008] In summary, there is an urgent need to provide a process for producing battery-grade sodium carbonate by a low-temperature refined crystallization method to solve the problems of low yield and high nickel and chromium metal content in the existing process for producing battery-grade sodium carbonate. Summary of the invention
[0009] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a process for producing battery-grade sodium carbonate by a low-temperature refined crystallization method which can improve the yield and purity of battery-grade sodium carbonate.
[0010] The technical solution adopted by the present invention to solve the technical problem is: a process for producing battery-grade sodium carbonate by a low-temperature refined crystallization method, comprising the following steps:
[0011] 1) Dissolving: dissolving industrial grade sodium carbonate in pure water, and adjusting the pH to 12-13 with sodium hydroxide solution, reacting for a period of time, filtering once at room temperature, collecting the filtrate, and obtaining a first clear liquid and a first filter residue;
[0012] 2) Primary crystallization: the first clear liquid is fed into the first crystallization kettle, the temperature of the solution in the kettle is controlled to be 16°C-20°C, carbon dioxide gas is introduced, the pH value is adjusted to 8-10, and after a period of reaction, secondary filtration is performed, and the filtrate is collected to obtain a second filter residue and a second clear liquid;
[0013] 3) Secondary crystallization: the second clear liquid is fed into the second crystallization kettle, the temperature of the solution in the kettle is controlled to be 12°C-15°C, carbon dioxide gas is introduced, and after a period of reaction, three filtrations are performed to obtain a filtrate and a third filter residue; the third filter residue is centrifuged and dehydrated to obtain a first mixed crystal; the filtrate and the centrifuged liquid are combined to obtain a third clear liquid;
[0014] 4) Tertiary crystallization: the third clear liquid is sent to the third crystallization kettle, the temperature of the solution in the kettle is controlled to be 6°C-10°C, and carbon dioxide gas is introduced. After a period of reaction, the mixture is filtered four times to obtain a filtrate and a fourth filter residue; the fourth filter residue is centrifuged and dehydrated to obtain a second mixed crystal and a centrifuge; the filtrate and the centrifuge are combined to obtain a fourth clear liquid;
[0015] 5) Drying: The first mixed crystal and the second mixed crystal are combined to obtain a crystalline mixture which is dried to obtain battery-grade sodium carbonate.
[0016] Furthermore, in step 1), the ratio of the weight of industrial-grade sodium carbonate to the volume of pure water is 280-380 g:1 L, and the reaction time is 1-4 h.
[0017] Preferably, the reaction time in step 1) is 1-1.5 h
[0018] Furthermore, the reaction time in step 2) is 2-4 hours, and the temperature during the secondary filtration is 20°C.
[0019] Furthermore, the second filter residue obtained in step 2) is returned to step 1) for dissolution again.
[0020] Furthermore, the reaction time in step 3) is 3-5 hours, and the temperature during the three filtrations is 20°C.
[0021] Furthermore, the reaction time in step 4) is 3-6 hours, and the temperature during the four filtrations is 20°C.
[0022] Furthermore, in step 5), the drying temperature is 200° C. and the drying time is 1-2 hours.
[0023] Furthermore, the fourth clear liquid obtained in step 4) is returned to step 1) to dissolve industrial-grade sodium carbonate.
[0024] Furthermore, when the fourth clear liquid is returned to step 1), the ratio of the weight of industrial-grade sodium carbonate to the volume of the fourth clear liquid is 280-380 g:1 L.
[0025] Furthermore, the excess carbon dioxide gas discharged from the first crystallization kettle, the second crystallization kettle and the third crystallization kettle and the carbon dioxide gas decomposed during drying are compressed by a compressor and collected in a gas-liquid separation tower, and the carbon dioxide gas obtained after purification in the gas-liquid separation tower is returned to the first crystallization kettle, the second crystallization kettle and the third crystallization kettle for reuse.
[0026] Beneficial effects of the process for producing battery-grade sodium carbonate by a low-temperature refined crystallization method of the present invention:
[0027] (1) The process of the present invention is simple. By adopting the method of three low-temperature crystallizations, the clear liquid separated by the previous crystallization is further subjected to low-temperature crystallization treatment, so that the sodium carbonate crystals are completely precipitated step by step, thereby greatly improving the yield of battery-grade sodium carbonate;
[0028] (2) In the present invention, carbon dioxide gas is introduced during the three crystallization processes. The carbon dioxide gas can effectively inhibit the crystallization of sodium carbonate decahydrate (Na2CO3·10H2O) under low temperature conditions and precipitate together with sodium carbonate into the battery-grade sodium carbonate product, effectively reducing the content of crystal water in the battery-grade sodium carbonate product, preventing the occurrence of water-soluble impurities being introduced into the product, thereby improving the purity of the battery-grade sodium carbonate, greatly shortening the drying time, and reducing energy consumption and production costs;
[0029] (3) In the present invention, the second filter residue containing metal impurities and semi-alkali obtained by primary crystallization and filtration separation is returned to the dissolution step to be used for dissolving alkali ingredients. In the dissolution step, the metal impurities in the second filter residue can be further removed instead of directly drying the second filter residue, thereby effectively reducing the metal content in battery-grade sodium carbonate, so that the metal content in the produced battery-grade sodium carbonate meets the standard of "T / HNSDCHYXH 001-2023 Battery-Grade Sodium Carbonate". BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 — is a process flow chart of a process for producing battery-grade sodium carbonate by a low-temperature refined crystallization method according to the present invention. DETAILED DESCRIPTION
[0031] The present invention is further described below in conjunction with the accompanying drawings and examples, but these specific implementation schemes do not limit the protection scope of the present invention in any way.
[0032] Example 1
[0033] A process for producing battery-grade sodium carbonate by low-temperature refined crystallization, the process flow chart of which is as follows: Figure 1 As shown, the following steps are included:
[0034] 1) Dissolution: Dissolve 380g of industrial grade sodium carbonate (purity 96%) in 1L of pure water at 35°C, and adjust the pH to 12-13 with a 30% sodium hydroxide solution. React for 1.5h to precipitate alkali metals and metal impurities with alkaline hydroxide, and then filter them out at room temperature. Collect the filtrate to obtain a first clear liquid and a first filter residue. Discard the first filter residue.
[0035] 2) primary crystallization: the first clear liquid is sent into a first crystallization kettle, which is a jacketed crystallization kettle, cold water at 5-6°C is introduced into the jacket to reduce the temperature of the solution in the kettle to 20°C, and then carbon dioxide gas is introduced, the amount of carbon dioxide gas introduced = (the weight of industrial grade Na2CO3) / 2×(44 / 53 / 0.8)=380g / 2×(44 / 53 / 0.8)=190g, the pH value is adjusted to 8-10, and after reacting for 4h, secondary filtration is performed at 20°C, and the filtrate is collected to obtain a second filter residue and a second clear liquid, wherein the second filter residue contains not only metal impurities that are not completely removed in the dissolution step, but also half alkali (half alkali refers to the precipitated Na2CO3 and NaHCO3 mixed crystals, and the half alkali is named Na2CO3·NaHCO3 in the present invention); the second filter residue is returned to the dissolution step of step 1) to be recovered for dissolving alkali ingredients;
[0036] 3) Secondary crystallization: the second clear liquid is sent into a second crystallization kettle, which is a jacketed crystallization kettle, cold water at 5-6°C is introduced into the jacket to reduce the temperature of the solution in the kettle to 15°C, and then carbon dioxide gas is introduced, the amount of carbon dioxide gas introduced = (the weight of industrial-grade Na2CO3) / 2×(44 / 53 / 0.8)=380g / 2×(44 / 53 / 0.8)=190g, after reacting for 5h, filtering three times at 20°C to obtain a filtrate and a third filter residue; the third filter residue is centrifuged and dehydrated to obtain a first mixed crystal (semi-alkali); the filtrate and the centrifuge are combined to obtain a third clear liquid;
[0037] 4) Three crystallizations: the third clear liquid is sent to the third crystallization kettle, which is a jacketed crystallization kettle, cold water at 5-6°C is introduced into the jacket to reduce the temperature of the solution in the kettle to 10°C, and then carbon dioxide gas is introduced, the amount of carbon dioxide gas introduced = (the weight of industrial grade Na2CO3) / 2×(44 / 53 / 0.8)=380g / 2×(44 / 53 / 0.8)=190g, after reacting for 6h, it is filtered four times at 20°C to obtain a filtrate and a fourth filter residue; the fourth filter residue is centrifuged and dehydrated to obtain a second mixed crystal (semi-alkali) and a centrifuge; the filtrate and the centrifuge are combined to obtain a fourth clear liquid;
[0038] The fourth clear liquid is returned to step 1) and used to dissolve industrial-grade sodium carbonate, wherein 380 g of industrial-grade sodium carbonate is dissolved in 1 L of the fourth clear liquid at 35° C., and the pH is adjusted to 12-13 with a 30% sodium hydroxide solution, and the reaction is performed for 1.5 hours to precipitate alkali metals and metal impurities by alkaline hydrogenation, and then filtered to remove them, and the filtrate is continuously produced according to the subsequent step 2);
[0039] 5) Drying: The crystal mixture obtained by combining the first mixed crystal and the second mixed crystal is dried at a temperature of 200° C. for 2 h, so that the semi-alkali is decomposed into Na2CO3, CO2 and H2O at high temperature to obtain battery-grade sodium carbonate; CO2 and H2O are sent to a gas-liquid separation tower.
[0040] In the above steps 2)-5), the excess carbon dioxide gas discharged from the first crystallization kettle, the second crystallization kettle, and the third crystallization kettle and the carbon dioxide gas decomposed during drying are compressed by a compressor and collected in a gas-liquid separation tower. The carbon dioxide gas obtained after purification in the gas-liquid separation tower is returned to the first crystallization kettle, the second crystallization kettle, and the third crystallization kettle for reuse.
[0041] Example 2
[0042] A process for producing battery-grade sodium carbonate by low-temperature refined crystallization, the process flow chart of which is as follows: Figure 1 As shown, the following steps are included:
[0043] 1) Dissolution: Dissolve 320g of industrial grade sodium carbonate (purity 96%) in 1L of pure water at 32°C, and adjust the pH to 12-13 with a 30% sodium hydroxide solution. React for 1.2h to precipitate alkali metals and metal impurities with alkaline hydroxide, and then filter them out at room temperature. Collect the filtrate to obtain a first clear liquid and a first filter residue. Discard the first filter residue.
[0044] 2) primary crystallization: the first clear liquid is sent into a first crystallization kettle, which is a jacketed crystallization kettle, cold water at 5-6°C is introduced into the jacket to reduce the temperature of the solution in the kettle to 18°C, and then carbon dioxide gas is introduced, the amount of carbon dioxide gas introduced = (the weight of industrial grade Na2CO3) / 2×(44 / 53 / 0.8)=320g / 2×(44 / 53 / 0.8)=160g, the pH value is adjusted to 8-10, and after reacting for 3h, secondary filtration is performed at 20°C, and the filtrate is collected to obtain a second filter residue and a second clear liquid, wherein the second filter residue contains not only metal impurities that are not completely removed in the dissolution step, but also half alkali (half alkali refers to the precipitated Na2CO3 and NaHCO3 mixed crystals, and the half alkali is named Na2CO3·NaHCO3 in the present invention); the second filter residue is returned to the dissolution step of step 1) to be recovered for dissolving alkali ingredients;
[0045] 3) Secondary crystallization: the second clear liquid is sent into a second crystallization kettle, which is a jacketed crystallization kettle, cold water at 5-6°C is introduced into the jacket to reduce the temperature of the solution in the kettle to 13°C, and then carbon dioxide gas is introduced, the amount of carbon dioxide gas introduced = (the weight of industrial grade Na2CO3) / 2×(44 / 53 / 0.8)=320g / 2×(44 / 53 / 0.8)=160g, after reacting for 4h, filtering three times at 20°C to obtain a filtrate and a third filter residue; the third filter residue is centrifuged and dehydrated to obtain a first mixed crystal (semi-alkali); the filtrate and the centrifuge are combined to obtain a third clear liquid;
[0046] 4) Three crystallizations: the third clear liquid is sent to the third crystallization kettle, which is a jacketed crystallization kettle, cold water at 5-6°C is introduced into the jacket to reduce the temperature of the solution in the kettle to 8°C, and then carbon dioxide gas is introduced, the amount of carbon dioxide gas introduced = (the weight of industrial grade Na2CO3) / 2×(44 / 53 / 0.8)=320g / 2×(44 / 53 / 0.8)=160g, after reacting for 5h, it is filtered four times at 20°C to obtain a filtrate and a fourth filter residue; the fourth filter residue is centrifuged and dehydrated to obtain a second mixed crystal (semi-alkali) and a centrifuge; the filtrate and the centrifuge are combined to obtain a fourth clear liquid;
[0047] The fourth clear liquid is returned to step 1) and used to dissolve industrial-grade sodium carbonate, wherein 320 g of industrial-grade sodium carbonate is dissolved in 1 L of the fourth clear liquid at 30-35° C., and the pH is adjusted to 12-13 with a 30% sodium hydroxide solution, and the reaction is performed for 1.2 hours to precipitate alkali metals and metal impurities by alkaline hydrogenation, and then filtered to remove them, and the filtrate is continuously produced according to the subsequent step 2);
[0048] 5) Drying: The crystal mixture obtained by combining the first mixed crystal and the second mixed crystal is dried at a temperature of 200° C. for 1.5 h, so that the semi-alkali is decomposed into Na2CO3, CO2 and H2O at high temperature to obtain battery-grade sodium carbonate; CO2 and H2O are sent to a gas-liquid separation tower.
[0049] In the above steps 2)-5), the excess carbon dioxide gas discharged from the first crystallization kettle, the second crystallization kettle, and the third crystallization kettle and the carbon dioxide gas decomposed during drying are compressed by a compressor and collected in a gas-liquid separation tower. The carbon dioxide gas obtained after purification in the gas-liquid separation tower is returned to the first crystallization kettle, the second crystallization kettle, and the third crystallization kettle for reuse.
[0050] Example 3
[0051] A process for producing battery-grade sodium carbonate by low-temperature refined crystallization, the process flow chart of which is as follows: Figure 1 As shown, the following steps are included:
[0052] 1) Dissolution: Dissolve 280g of industrial grade sodium carbonate (purity 96%) in 1L of pure water at 30°C, and adjust the pH to 12-13 with 30% sodium hydroxide solution. React for 1h to precipitate alkali metals and metal impurities by alkaline hydroxide, and then filter them out at room temperature. Collect the filtrate to obtain a first clear liquid and a first filter residue. Discard the first filter residue.
[0053] 2) primary crystallization: the first clear liquid is sent into a first crystallization kettle, which is a jacketed crystallization kettle, cold water at 5-6°C is introduced into the jacket to reduce the temperature of the solution in the kettle to 16°C, and then carbon dioxide gas is introduced, the amount of carbon dioxide gas introduced = (the weight of industrial grade Na2CO3) / 2×(44 / 53 / 0.8)=280g / 2×(44 / 53 / 0.8)=140g, the pH value is adjusted to 8-10, and after reacting for 2h, secondary filtration is performed at 20°C, and the filtrate is collected to obtain a second filter residue and a second clear liquid, wherein the second filter residue contains not only metal impurities that are not completely removed in the dissolving step, but also half alkali (half alkali refers to the precipitated Na2CO3 and NaHCO3 mixed crystals, and the half alkali is named Na2CO3·NaHCO3 in the present invention); the second filter residue is returned to the dissolving step of step 1) to be recovered for dissolving alkali ingredients;
[0054] 3) Secondary crystallization: the second clear liquid is sent into a second crystallization kettle, which is a jacketed crystallization kettle, cold water at 5-6°C is introduced into the jacket to reduce the temperature of the solution in the kettle to 12°C, and then carbon dioxide gas is introduced, the amount of carbon dioxide gas introduced = (the weight of industrial-grade Na2CO3) / 2×(44 / 53 / 0.8)=280g / 2×(44 / 53 / 0.8)=140g, after reacting for 3h, filtering three times at 20°C to obtain a filtrate and a third filter residue; the third filter residue is centrifuged and dehydrated to obtain a first mixed crystal (semi-alkali); the filtrate and the centrifuge are combined to obtain a third clear liquid;
[0055] 4) Three crystallizations: the third clear liquid is sent to the third crystallization kettle, which is a jacketed crystallization kettle, cold water at 5-6°C is introduced into the jacket to reduce the temperature of the solution in the kettle to 6°C, and then carbon dioxide gas is introduced, the amount of carbon dioxide gas introduced = (the weight of industrial grade Na2CO3) / 2×(44 / 53 / 0.8)=280g / 2×(44 / 53 / 0.8)=140g, after reacting for 3h, it is filtered four times at 20°C to obtain a filtrate and a fourth filter residue; the fourth filter residue is centrifuged and dehydrated to obtain a second mixed crystal (semi-alkali) and a centrifuge; the filtrate and the centrifuge are combined to obtain a fourth clear liquid;
[0056] The fourth clear liquid is returned to step 1) and used to dissolve industrial-grade sodium carbonate, wherein 280 g of industrial-grade sodium carbonate is dissolved in 1 L of the fourth clear liquid at 30° C., and a 30% sodium hydroxide solution is used to adjust the pH to 12-13, and the reaction time is 1 hour to precipitate alkali metals and metal impurities by alkaline hydrogenation, and then filtered to remove them, and the filtrate is continued to be continuously produced according to the subsequent step 2);
[0057] 5) Drying: The crystal mixture obtained by combining the first mixed crystal and the second mixed crystal is dried at a temperature of 200° C. for 1 hour, so that the semi-alkali is decomposed into Na2CO3, CO2 and H2O at high temperature to obtain battery-grade sodium carbonate; CO2 and H2O are sent to a gas-liquid separation tower.
[0058] In the above steps 2)-5), the excess carbon dioxide gas discharged from the first crystallization kettle, the second crystallization kettle, and the third crystallization kettle and the carbon dioxide gas decomposed during drying are compressed by a compressor and collected in a gas-liquid separation tower. The carbon dioxide gas obtained after purification in the gas-liquid separation tower is returned to the first crystallization kettle, the second crystallization kettle, and the third crystallization kettle for reuse.
[0059] Comparative Example 1
[0060] A process for producing battery-grade sodium carbonate by a low-temperature refined crystallization method comprises the following steps:
[0061] 1) Dissolution: Dissolve 380g of industrial grade sodium carbonate (purity 96%) in 1L of pure water at 35°C, and adjust the pH to 12-13 with a 30% sodium hydroxide solution. React for 1.5h to precipitate alkali metals and metal impurities with alkaline hydroxide, and then filter them out at room temperature. Collect the filtrate to obtain a first clear liquid and a first filter residue. Discard the first filter residue.
[0062] 2) Primary crystallization: the first clear liquid is sent into the first crystallization kettle, which is a jacketed crystallization kettle, cold water at 5-6°C is introduced into the jacket to reduce the temperature of the solution in the kettle to 20°C, the pH value is adjusted to 8-10, and after reacting for 4 hours, secondary filtration is performed at 20°C, and the filtrate is collected to obtain a second filter residue and a second clear liquid; the second filter residue is dried at a temperature of 200°C for 2 hours to obtain the product.
[0063] Comparative Example 2
[0064] The difference between this comparative example and Example 1 is that the second filter residue obtained in step 2) is combined with the first mixed crystals and the second mixed crystals in step 5) and then dried.
[0065] Comparative Example 3
[0066] The difference between this comparative example and Example 1 is that carbon dioxide gas is not introduced in step 2) to step 4), and the carbon dioxide gas generated during drying is not recovered for utilization in step 2) to step 4).
[0067] Comparative Example 4
[0068] The difference between this comparative example and Example 1 is that the fourth clear liquid in step 4) is not returned to step 1) for dissolving industrial grade sodium carbonate.
[0069] Comparative Example 5
[0070] The difference between this comparative example and Example 1 is that the temperature during step 3) secondary crystallization and step 4) secondary crystallization is both 20°C.
[0071] Comparative Example 6
[0072] The difference between this comparative example and Example 1 is that: in step 2), the second filter residue obtained by primary crystallization and filtration is directly dried at a temperature of 200° C. for 2 h to obtain the product.
[0073] Comparative Example 7
[0074] The difference between this comparative example and Example 1 is that: in step 3), the first mixed crystal obtained by secondary crystallization, filtration and centrifugal dehydration is directly dried at a temperature of 200° C. for 2 h to obtain the product.
[0075] Comparative Example 8
[0076] This comparative example also produces battery-grade lithium carbonate with reference to the process of Example 1, wherein the difference is that the raw material is industrial-grade lithium carbonate with a purity of 96%.
[0077] The similarities and differences of each operating step in the process of producing battery-grade sodium carbonate in Example 1 and Comparative Examples 1-7 are shown in Table 1:
[0078] Table 1 The similarities and differences of each operating step in the process of producing battery grade sodium carbonate in Example 1 and Comparative Examples 1-7
[0079]
[0080] The present invention measured the yield and chemical composition of battery-grade sodium carbonate prepared in Examples 1-3 and Comparative Examples 1-8, and the results are shown in Table 2-4:
[0081] Table 2 The yield / % of battery-grade sodium carbonate prepared in Examples 1-3 and the content / % of its chemical components
[0082]
[0083]
[0084] It can be seen from Table 2 that the yield of battery-grade sodium carbonate produced by the process for producing battery-grade sodium carbonate in this application reached more than 99.7%, wherein the content of sodium carbonate (i.e., the purity of battery-grade sodium carbonate) reached more than 99.992%, and the contents of other impurities met the standards of "T / HNSDCHYXH 001-2023 Battery Grade Sodium Carbonate".
[0085] Table 3 Yield (%) and content (%) of battery-grade sodium carbonate prepared in Example 1 and Comparative Examples 1-7
[0086]
[0087] It can be seen from the above table that the yields of battery-grade sodium carbonate corresponding to Comparative Examples 1-3 and Comparative Examples 5-7 are significantly lower than that of Example 1, indicating that the process of the present invention can significantly improve the yield of battery-grade sodium carbonate; the chemical composition of the battery-grade sodium carbonate prepared in Comparative Examples 1-3 and Comparative Examples 5-7 is compared with the standard of "T / HNSDCHYXH 001-2023 Battery Grade Sodium Carbonate". Although the content of sodium carbonate contained meets the requirements of the standard (not less than 99.5%), the contents of other impurities have at least 2 impurities exceeding the upper limit of the standard, so that the battery-grade sodium carbonate produced by the process of Comparative Examples 1-3 and Comparative Examples 5-7 does not meet the standard of "T / HNSDCHYXH 001-2023 Battery Grade Sodium Carbonate".
[0088] Compared with Example 1, the contents of two metal impurities, nickel and chromium, in the battery-grade sodium carbonate produced in Comparative Example 2 exceeded the upper limit of the standard, and the yield and content thereof were lower than those in Example 1. It is shown that the present invention adds the treatment of returning the second filter residue to the dissolution step, which can not only further reduce the content of nickel and chromium metal impurities, so that the content of nickel and chromium metal impurities reaches the standard of "T / HNSDCHYXH 001-2023 Battery-Grade Sodium Carbonate", but also the semi-alkali in the second filter residue is further crystallized and precipitated after returning to the dissolution step, which can improve the yield and purity of battery-grade sodium carbonate.
[0089] Compared with Example 1, the content of K, Mg, and chloride impurities in the battery-grade sodium carbonate produced in Comparative Example 3 exceeds the upper limit of the standard, and the yield and content are lower than those in Example 1. It is shown that the present invention introduces carbon dioxide gas treatment in the primary crystallization, secondary crystallization, and tertiary crystallization treatments, which can not only effectively inhibit the crystallization of sodium carbonate decahydrate, but also reduce the content of crystal water in battery-grade sodium carbonate, thereby inhibiting the phenomenon that water-soluble impurities formed by potassium ions, chloride ions, and magnesium ions that are easily soluble in water are brought into the product, so that the content of K, Mg, and chloride impurities reaches the standard of "T / HNSDCHYXH 001-2023 Battery Grade Sodium Carbonate", and can also improve the yield and purity of battery-grade sodium carbonate.
[0090] Compared with Example 1, the yield of battery-grade sodium carbonate corresponding to Comparative Example 4 is slightly lower than that of Example 1, but there is no significant difference between the two, and the purity is lower than that of Example 1, indicating that returning the fourth clear liquid to the dissolution step can improve the yield and purity of battery-grade sodium carbonate to a certain extent.
[0091] Compared with Example 1, the contents of two metal impurities, nickel and chromium, in the battery-grade sodium carbonate produced in Comparative Example 5 exceeded the upper limit of the standard, and the yield and content thereof were significantly lower than those in Example 1. The temperatures of the primary crystallization, secondary crystallization, and tertiary crystallization treatments of the present invention showed a trend of decreasing successively, while the temperatures of the primary crystallization, secondary crystallization, and tertiary crystallization treatments of Comparative Example 5 were all consistent, indicating that the crystallization method with gradually decreasing temperature used in the present invention is more sensitive to the removal of nickel and chromium, and can also effectively improve the yield and purity of battery-grade sodium carbonate.
[0092] Compared with Example 1, the contents of chloride, nickel, chromium and other impurities corresponding to Comparative Examples 6 and 7 all exceed the upper limit of the standard, and their yields and contents are significantly lower than those in Example 1. It is shown that the use of three crystallization treatments can not only effectively reduce the content of impurities compared with two and one crystallization treatments, but also greatly improve the yield and purity of battery-grade sodium carbonate, so that the produced battery-grade sodium carbonate meets the standard of "T / HNSDCHYXH 001-2023 Battery-Grade Sodium Carbonate".
[0093] Table 4 Yield (%) and content of chemical components (%) of battery-grade sodium carbonate prepared in Example 1 and Comparative Example 8
[0094]
[0095]
[0096] It can be seen from the above table that the process of the present application for treating industrial-grade sodium carbonate to prepare battery-grade sodium carbonate has higher yield and purity than the process of the present application for treating industrial-grade lithium carbonate to prepare battery-grade lithium carbonate, and the prepared product contains fewer impurities, indicating that the process of the present invention is more sensitive to the treatment of industrial-grade sodium carbonate than industrial-grade lithium carbonate, and has a better effect of improving yield and purity.
[0097] It should be noted that the terms "primary", "secondary", "first", "second", "third", "fourth", etc. are used herein to describe the various operation steps and products, but these operation steps and products should not be limited by these terms. These terms are only used to separate the various operation steps and products.
[0098] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. A process for producing battery-grade sodium carbonate by low-temperature refined crystallization. It is characterized in that The following steps are involved: 1) Dissolving: dissolving industrial grade sodium carbonate in pure water, and adjusting the pH to 12-13 with sodium hydroxide solution, reacting for a period of time, filtering once at room temperature, collecting the filtrate, and obtaining a first clear liquid and a first filter residue; 2) Primary crystallization: the first clear liquid is fed into the first crystallization kettle, the temperature of the solution in the kettle is controlled to be 16°C-20°C, carbon dioxide gas is introduced, the pH value is adjusted to 8-10, and after a period of reaction, secondary filtration is performed, and the filtrate is collected to obtain a second filter residue and a second clear liquid; 3) Secondary crystallization: the second clear liquid is fed into the second crystallization kettle, the temperature of the solution in the kettle is controlled to be 12°C-15°C, carbon dioxide gas is introduced, and after a period of reaction, three filtrations are performed to obtain a filtrate and a third filter residue; the third filter residue is centrifuged and dehydrated to obtain a first mixed crystal; the filtrate and the centrifuged liquid are combined to obtain a third clear liquid; 4) Tertiary crystallization: the third clear liquid is sent to the third crystallization kettle, the temperature of the solution in the kettle is controlled to be 6°C-10°C, and carbon dioxide gas is introduced. After a period of reaction, the mixture is filtered four times to obtain a filtrate and a fourth filter residue; the fourth filter residue is centrifuged and dehydrated to obtain a second mixed crystal and a centrifuge; the filtrate and the centrifuge are combined to obtain a fourth clear liquid; 5) Drying: The first mixed crystal and the second mixed crystal are combined to obtain a crystalline mixture which is dried to obtain battery-grade sodium carbonate.
2. A process for producing battery-grade sodium carbonate by a low-temperature refined crystallization method as claimed in claim 1, It is characterized in that In the step 1), the ratio of the weight of industrial-grade sodium carbonate to the volume of pure water is 280-380 g:1 L, and the reaction time is 1-4 h.
3. A process for producing battery-grade sodium carbonate by a low-temperature refined crystallization method as claimed in claim 1, It is characterized in that The reaction time in step 2) is 2-4 hours, and the temperature during the secondary filtration is 20°C.
4. A process for producing battery-grade sodium carbonate by a low-temperature refined crystallization method as claimed in claim 1, It is characterized in that The second filter residue obtained in step 2) is returned to step 1) for dissolution again.
5. A process for producing battery-grade sodium carbonate by a low-temperature refined crystallization method as claimed in claim 1, It is characterized in that The reaction time in step 3) is 3-5 hours, and the temperature during the three filtrations is 20°C.
6. A process for producing battery-grade sodium carbonate by a low-temperature refined crystallization method as claimed in claim 1, It is characterized in that The reaction time in step 4) is 3-6 hours, and the temperature during the four filtrations is 20°C.
7. A process for producing battery-grade sodium carbonate by a low-temperature refined crystallization method as claimed in claim 1, It is characterized in that The drying temperature in step 5) is 200° C. and the drying time is 1-2 hours.
8. A process for producing battery-grade sodium carbonate by a low-temperature refined crystallization method as claimed in claim 1, It is characterized in that The fourth clear liquid obtained in step 4) is returned to step 1) to dissolve industrial-grade sodium carbonate.
9. A process for producing battery-grade sodium carbonate by a low-temperature refined crystallization method as claimed in claim 8, It is characterized in that When the fourth clear liquid is returned to step 1), the ratio of the weight of industrial-grade sodium carbonate to the volume of the fourth clear liquid is 280-380 g:1 L.
10. A process for producing battery-grade sodium carbonate by a low-temperature refined crystallization method as claimed in claim 1, It is characterized in that The excess carbon dioxide gas discharged from the first crystallization kettle, the second crystallization kettle and the third crystallization kettle and the carbon dioxide gas decomposed during drying are compressed by a compressor and collected in a gas-liquid separation tower. The carbon dioxide gas obtained after purification in the gas-liquid separation tower is returned to the first crystallization kettle, the second crystallization kettle and the third crystallization kettle for reuse.