Core-shell structure sodium battery positive electrode precursor as well as preparation method and application thereof

By adopting a core-shell structure design in the sodium-ion battery cathode material and using a combination of a dense core and a loose outer shell, the stability and cost issues of the sodium-ion battery material are solved, and the overall performance and market competitiveness of the battery are improved.

CN118771484APending Publication Date: 2024-10-15JINGMEN GEM NEW MATERIAL CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410996932.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Layered oxide cathode materials for sodium-ion batteries have problems such as irreversible phase change, unstable storage and poor interface stability. Metal resources such as nickel are expensive, which limits the cost reduction and market competitiveness of sodium-ion batteries.

Method used

The core-shell structure sodium electrode cathode precursor is used. The core is a dense nickel-iron-manganese structure. The outer shell is added with copper elements and uses loose stacking to improve the air stability and porosity of the material, reduce the nickel element content, and enhance the compaction density and energy of the material. density.

Benefits of technology

It improves the air stability and cost-effectiveness of the material, while improving the capacity during the charge and discharge process, especially the performance under high-rate conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004960492990000121
    Figure BDA0004960492990000121
Patent Text Reader

Abstract

The invention provides a core-shell structure sodium battery positive electrode precursor and a preparation method and application thereof.The core-shell structure sodium battery positive electrode precursor comprises an inner core and an outer shell on the surface of the inner core, the inner core comprises NiaFebMn1-a-b-cMc (OH) 2, 0.3 < = a < = 0.5, 0.2 < = b < = 0.4, 0 < = c < = 0.01, the outer shell comprises NixCuyFezMn1-x-y-z-vNv (OH) 2, 0.1 < = x < 0.3, 0.02 < = y < = 0.2, 0.2 < = z < = 0.4, 0 < = v < = 0.01, 0 < = c < = 0.5, 0 < = z < = 0.5, 0 < = v < = 0.01, 0 < = c < = 0.5, 0 < = c < = 0.5, 0 < = c < = 0.5 and 0 < = and pores are formed in the shell. The core primary particles of the core-shell structure sodium battery positive electrode precursor are densely stacked, and the shell primary particles are loosely stacked, so that the compaction density, the energy density, the porosity and the specific surface area of the material are improved, and the performance of the material is promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries and relates to a core-shell structure sodium battery positive electrode precursor and a preparation method and application thereof. Background Art

[0002] With the rapid development and popularization of renewable energy such as solar and wind power, there is a growing demand for energy storage to cope with the volatility and intermittency of renewable energy. Traditional power systems have difficulty coping with this volatility, so large-scale energy storage technology is needed to balance the difference between supply and demand. Currently, lithium-ion batteries are one of the most common commercial energy storage technologies. However, the scarcity of lithium resources and the instability of the supply chain have led to the high cost of lithium batteries and certain safety risks. Therefore, it has become crucial to find alternative energy storage technologies.

[0003] Sodium and lithium are adjacent elements in the same main group and have similar physical and chemical properties. Therefore, sodium-ion batteries have similar structures and working principles to lithium-ion batteries. At the same time, sodium resources are abundant and widely distributed on the earth, and are considered to be a cost-effective alternative to lithium-ion batteries in the field of large-scale energy storage. The development of high-performance electrode materials is the research focus of sodium-ion batteries. As positive electrode materials for sodium-ion batteries, transition metal layered oxides have the advantages of high specific capacity and easy industrialization, and have received increasing attention. However, layered oxides still face many challenges, such as irreversible phase changes, unstable storage, and insufficient performance, which seriously restrict the commercialization process of sodium-ion batteries. The preparation of high-quality precursor materials is the key to solving this problem.

[0004] For example, CN115196691A discloses a nickel-iron-manganese ternary precursor for sodium-ion batteries, and a preparation method and application thereof. The preparation method comprises: subjecting ferrous salt, nickel salt, manganese salt and hydroxide to a coprecipitation reaction in a solvent in the presence of a chelating agent to generate a nickel-iron-manganese ternary precursor; and subjecting the coprecipitation reaction to a first pH value (11.3-11.5) for generating new crystal nuclei; after the generation of new crystal nuclei is completed, adjusting the pH value to subject the coprecipitation reaction to a second pH value (10.5-11.0) until the crystal grows to a preset median particle size, and controlling the difference between the first pH value and the second pH value and the concentration of the chelating agent to a specific degree. However, the air stability of the sodium nickel-iron-manganese oxide cathode material prepared thereby is poor, which is not conducive to the production, transportation and storage of the material, and the higher nickel content increases the manufacturing cost.

[0005] Therefore, layered oxide positive electrode materials for sodium-ion batteries still face problems such as irreversible changes in electrochemical processes, unstable storage in air, and poor interface stability. Moreover, although sodium resources are relatively abundant, some metal resources such as nickel used in the preparation of layered oxides are still limited and expensive. Further reducing costs is an inevitable requirement to improve the market competitiveness of sodium-ion batteries. Summary of the invention

[0006] The object of the present invention is to provide a core-shell structure sodium battery positive electrode precursor and a preparation method and application thereof. The core primary particles of the core-shell structure sodium battery positive electrode precursor are densely stacked, which is beneficial to improve the compaction density and energy density of the material. Copper elements are added to the outer shell to improve stability while reducing costs. The primary particles of the outer shell are loosely stacked, which increases the porosity and specific surface area, thereby promoting the capacity of the material.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a core-shell structure sodium positive electrode precursor, the core-shell structure sodium positive electrode precursor comprising a core and a shell on the surface of the core, the core comprising Ni a Fe b Mn 1-a-b-c M c (OH) 2 , wherein 0.3≤a≤0.5, 0.2≤b≤0.4, 0≤c≤0.01, the shell comprises Ni x Cu y Fe z Mn 1-x-y-z-v N v (OH) 2 , wherein 0.1≤x<0.3, 0.02≤y≤0.2, 0.2≤z≤0.4, 0≤v≤0.01, M and N independently include doped metal elements, and the shell contains pores.

[0009] The main components of the kernel of the present invention are nickel, iron and manganese, and the primary particles are densely packed, which is beneficial to improving the compaction density and energy density of the material; copper element is added to the shell to reduce the nickel element content, so as to improve the air stability of the material and reduce the overall cost of the material, and the primary particles of the shell are loosely packed, which improves the porosity and specific surface area, and is beneficial to the capacity of the material during charging and discharging, especially charging and discharging at high rates.

[0010] The core includes Ni a Fe b Mn 1-a-b-c M c (OH) 2, wherein 0.3≤a≤0.5, for example, 0.3, 0.4 or 0.5, 0.2≤b≤0.4, for example, 0.2, 0.3 or 0.4, 0≤c≤0.01, for example, 0, 0.005 or 0.01, and the shell includes Ni x Cu y Fe z Mn 1-x-y-z-v N v (OH) 2 , wherein 0.1≤x<0.3, for example, it can be 0.1, 0.2 or 0.28, 0.02≤y≤0.2, for example, it can be 0.02, 0.1 or 0.2, 0.2≤z≤0.4, for example, it can be 0.2, 0.3 or 0.4, 0≤v≤0.01, for example, it can be 0, 0.005 or 0.01, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0011] Preferably, the inner core is a dense structure, and the outer shell is a loose porous structure.

[0012] Preferably, the doping metal elements of M and N are of different types.

[0013] The present invention uses different doping elements in the core and shell structures to effectively improve the comprehensive performance of the material.

[0014] Preferably, the M includes any one of Zn, Mg or Sr or a combination of at least two of them.

[0015] Preferably, the N includes any one of Ti, Al or Zr or a combination of at least two of them.

[0016] Preferably, the particle size D50 of the inner core is 4-6 μm, for example, 4 μm, 5 μm or 6 μm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0017] Preferably, the particle size D50 of the core-shell structured sodium cathode precursor is 8-12 μm, for example, 8 μm, 10 μm or 12 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] In a second aspect, the present invention provides a method for preparing a core-shell structured sodium cathode precursor as described in the first aspect, the preparation method comprising the following steps:

[0019] (1) introducing a first mixed metal salt solution, a precipitant and a complexing agent into a base solution to perform a first coprecipitation reaction;

[0020] The first mixed metal salt solution includes a core formula amount of Ni source, Fe source, Mn source and M source;

[0021] (2) After the first coprecipitation reaction in step (1) is completed, the first mixed metal salt solution is replaced with a second metal salt solution and introduced into the reaction system to perform a second coprecipitation reaction to obtain the core-shell structure sodium cathode precursor;

[0022] The second mixed metal salt solution includes a Ni source, a Cu source, a Fe source, a Mn source and a N source in shell formula amounts.

[0023] Preferably, the base liquid comprises pure water, a precipitant and a complexing agent.

[0024] Preferably, in the reaction system of the first coprecipitation reaction in step (1), the concentration of the complexing agent is 4-8 g / L, for example, 4 g / L, 6 g / L or 8 g / L, and the pH is 10.0-11.0, for example, 10.0, 10.5 or 11.0, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0025] The present invention prepares a core-shell structured sodium ion battery layered oxide positive electrode material precursor by precisely controlling the reaction conditions during the coprecipitation process, wherein the core and the shell have different elemental compositions and microstructures; in particular, the structure of the core and the shell is regulated by controlling the concentration of the complexing agent and / or the pH of the reaction.

[0026] Preferably, the temperature of the first coprecipitation reaction in step (1) is 40-60°C, for example, 40°C, 50°C or 60°C, the stirring speed is 300-400r / min, for example, 300r / min, 350r / min or 400r / min, and is carried out in a protective gas.

[0027] Preferably, the protective gas includes any one of nitrogen, helium or argon, or a combination of at least two of them, preferably nitrogen.

[0028] The precipitant in step (1) comprises sodium hydroxide solution and / or potassium hydroxide solution.

[0029] Preferably, the complexing agent in step (1) comprises any one of ammonia, citric acid or oxalic acid, or a combination of at least two of them.

[0030] Preferably, the Ni source includes any one of nickel sulfate, nickel chloride or nickel nitrate, or a combination of at least two thereof, preferably nickel sulfate.

[0031] Preferably, the Fe source includes any one of ferrous sulfate, ferrous chloride or ferrous nitrate, or a combination of at least two thereof, preferably ferrous sulfate.

[0032] Preferably, the Mn source includes any one of manganese sulfate, manganese chloride or manganese nitrate, or a combination of at least two thereof, preferably manganese sulfate.

[0033] Preferably, the M source includes any one of sulfate, chloride or nitrate or a combination of at least two thereof, preferably sulfate.

[0034] Preferably, the N source includes any one of sulfate, chloride or nitrate, or a combination of at least two of them, preferably sulfate.

[0035] Preferably, after the second coprecipitation reaction in step (2) is completed, the reaction is stopped, and the precursor is obtained after aging, washing and drying.

[0036] Preferably, in the reaction system of the second coprecipitation reaction in step (2), the concentration of the complexing agent is 2-5 g / L, for example, 2 g / L, 3 g / L, 4 g / L or 5 g / L, and the pH is 9.5-10.5, for example, 9.5, 10.0 or 10.5, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0037] Preferably, the temperature of the second coprecipitation reaction in step (2) is 40-60°C, for example, 40°C, 50°C or 60°C, the stirring speed is 300-400r / min, for example, 300r / min, 350r / min or 400r / min, and is carried out in a protective gas.

[0038] As a preferred embodiment of the preparation method of the present invention, the preparation method comprises the following steps:

[0039] (1) introducing a first mixed metal salt solution, a precipitant and a complexing agent into a base liquid, and performing a first coprecipitation reaction in a protective gas at a temperature of 40-60° C. and a stirring speed of 300-400 r / min;

[0040] The first mixed metal salt solution includes a core formula amount of Ni source, Fe source, Mn source and M source;

[0041] In the reaction system of the first coprecipitation reaction, the concentration of the complexing agent is 4-8 g / L, and the pH is 10.0-11.0;

[0042] (2) After the first coprecipitation reaction in step (1) is completed, the first mixed metal salt solution is replaced with a second metal salt solution and introduced into the reaction system, and a second coprecipitation reaction is carried out in a protective gas at a temperature of 40-60° C. and a stirring speed of 300-400 r / min to obtain the core-shell structure sodium cathode precursor;

[0043] In the reaction system of the second coprecipitation reaction, the concentration of the complexing agent is 2-5 g / L, and the pH is 9.5-10.5;

[0044] The second mixed metal salt solution includes a Ni source, a Cu source, a Fe source, a Mn source and a N source in shell formula amounts.

[0045] In a third aspect, the present invention provides a sodium ion battery positive electrode material, which is obtained by mixing and sintering a sodium source and a core-shell structure sodium battery positive electrode precursor as described in the first aspect.

[0046] In a fourth aspect, the present invention provides a sodium ion battery, comprising the sodium ion battery positive electrode material as described in the third aspect.

[0047] Compared with the prior art, the present invention has the following beneficial effects:

[0048] The main components of the kernel of the present invention are nickel, iron and manganese, and the primary particles are densely packed, which is beneficial to improving the compaction density and energy density of the material; copper element is added to the shell to reduce the nickel element content, so as to improve the air stability of the material and reduce the overall cost of the material, and the primary particles of the shell are loosely packed, which improves the porosity and specific surface area, and is beneficial to the capacity of the material during charging and discharging, especially charging and discharging at high rates. DETAILED DESCRIPTION

[0049] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0050] Example 1

[0051] This embodiment provides a core-shell structure sodium battery positive electrode precursor, the core-shell structure sodium battery positive electrode precursor comprises a core and a shell on the surface of the core, the core comprises Ni 0.33 Fe 0.33 Mn 0.33 Zn 0.01 (OH) 2 , the shell includes Ni 0.275 Cu 0.02 Fe 0.3 Mn 0.4 Ti 0.005 (OH) 2 , and the shell contains pores;

[0052] The method for preparing the core-shell structure sodium cathode precursor comprises the following steps:

[0053] (1) adding pure water, sodium hydroxide solution and ammonia water into a reactor to prepare a reaction base liquid, and introducing nitrogen. After the base liquid is qualified, a mixed salt solution I of nickel sulfate, ferrous sulfate, manganese sulfate and zinc sulfate with a molar ratio of Ni:Fe:Mn:Zn of 0.33:0.33:0.33:0.01, a sodium hydroxide solution and ammonia water are simultaneously introduced into the reactor to carry out a first stage of coprecipitation reaction, and the reaction temperature is controlled to be 40° C., pH to be 10.0, ammonia water concentration to be 4 g / L, and stirring speed to be 300 r / min to obtain a zinc-doped precursor slurry with a particle size of 5 μm;

[0054] (2) Stop introducing the mixed salt solution I, and introduce a mixed salt solution II of nickel sulfate, copper sulfate, ferrous sulfate, manganese sulfate and titanyl sulfate with a molar ratio of Ni:Cu:Fe:Mn:Ti of 0.275:0.02:0.3:0.4:0.005 to carry out the second stage of coprecipitation reaction, control the reaction pH to 9.5, and the ammonia concentration to 2 g / L. Stop the reaction when the particle size grows to 8 μm, and obtain a core-shell structure precursor after aging, washing and drying.

[0055] Example 2

[0056] This embodiment provides a core-shell structure sodium battery positive electrode precursor, the core-shell structure sodium battery positive electrode precursor comprises a core and a shell on the surface of the core, the core comprises Ni 0.4 Fe 0.3 Mn 0.292 Mg 0.008 (OH) 2 , the shell includes Ni 0.248 Cu 0.1 Fe 0.35 Mn 0.3 Al 0.002 (OH) 2 , and the shell contains pores;

[0057] The method for preparing the core-shell structure sodium cathode precursor comprises the following steps:

[0058] (1) adding pure water, sodium hydroxide solution and ammonia water into a reactor to prepare a reaction base liquid, and introducing nitrogen. After the base liquid is qualified, a mixed salt solution I of nickel sulfate, ferrous sulfate, manganese sulfate and magnesium sulfate with a molar ratio of Ni:Fe:Mn:Mg of 0.4:0.3:0.292:0.008, sodium hydroxide solution and ammonia water are simultaneously introduced into the reactor to carry out a first stage of coprecipitation reaction, and the reaction temperature is controlled to be 50°C, pH to be 10.5, ammonia water concentration to be 6g / L, and stirring speed to be 350r / min, to obtain a magnesium-doped precursor slurry with a particle size of 6μm;

[0059] (2) Stop introducing the mixed salt solution I, and introduce a mixed salt solution II of nickel sulfate, copper sulfate, ferrous sulfate, manganese sulfate and aluminum sulfate with a molar ratio of Ni:Cu:Fe:Mn:Al of 0.248:0.1:0.35:0.3:0.002 to carry out the second stage of coprecipitation reaction, control the reaction pH to 10, and the ammonia concentration to 3 g / L. Stop the reaction when the particle size grows to 9 μm, and obtain a core-shell structure precursor after aging, washing and drying.

[0060] Example 3

[0061] This embodiment provides a core-shell structure sodium battery positive electrode precursor, the core-shell structure sodium battery positive electrode precursor comprises a core and a shell on the surface of the core, the core comprises Ni 0.394 Fe 0.2 Mn 0.4 Sr 0.006 (OH) 2 , the shell includes Ni 0.146 Cu 0.2 Fe 0.35 Mn 0.3 Zr 0.004 (OH) 2 , and the shell contains pores;

[0062] The method for preparing the core-shell structure sodium cathode precursor comprises the following steps:

[0063] (1) adding pure water, sodium hydroxide solution and ammonia water into a reaction kettle to prepare a reaction base liquid, and introducing nitrogen. After the base liquid is qualified, a mixed salt solution I of nickel sulfate, ferrous sulfate, manganese sulfate and strontium sulfate with a molar ratio of Ni:Fe:Mn:Sr of 0.394:0.2:0.4:0.006, a sodium hydroxide solution and ammonia water are simultaneously introduced into the reaction kettle to carry out a first stage of coprecipitation reaction. The reaction temperature is controlled to be 60° C., the pH is 11.0, the ammonia concentration is 8 g / L, and the stirring speed is 400 r / min to obtain a strontium-doped precursor slurry with a particle size of 4 μm;

[0064] (2) Stop introducing the mixed salt solution I, and introduce a mixed salt solution II of nickel sulfate, copper sulfate, ferrous sulfate, manganese sulfate and zirconium sulfate with a molar ratio of Ni:Cu:Fe:Mn:Zr of 0.146:0.2:0.35:0.3:0.004 to carry out the second stage of coprecipitation reaction, control the reaction pH to 10.5, and the ammonia concentration to 5 g / L. Stop the reaction when the particle size grows to 8 μm, and obtain a core-shell structure precursor after aging, washing and drying.

[0065] Example 4

[0066] This embodiment provides a core-shell structure sodium battery positive electrode precursor, wherein the core-shell structure sodium battery positive electrode precursor includes Ni 0.33 Fe 0.33 Mn 0.33 Ti 0.01 (OH) 2 Except for this, the rest are the same as in Example 1;

[0067] The preparation method of the core-shell structure sodium cathode precursor is the same as that of Example 1 except for the adaptive changes.

[0068] Example 5

[0069] This embodiment provides a core-shell structure sodium battery positive electrode precursor, wherein the core-shell structure sodium battery positive electrode precursor has a shell including Ni 0.275 Cu 0.02 Fe 0.3 Mn 0.4 Zn 0.005 (OH) 2 Except for this, the rest are the same as in Example 1;

[0070] The preparation method of the core-shell structure sodium cathode precursor is the same as that of Example 1 except for the adaptive changes.

[0071] Example 6

[0072] This embodiment provides a core-shell structure sodium battery positive electrode precursor, wherein the core-shell structure sodium battery positive electrode precursor includes Ni 0.33 Fe 0.33 Mn 0.34 (OH) 2 Except for this, the rest are the same as in Example 1;

[0073] The preparation method of the core-shell structure sodium cathode precursor is the same as that of Example 1 except for the adaptive changes.

[0074] Example 7

[0075] This embodiment provides a core-shell structure sodium battery positive electrode precursor, wherein the core-shell structure sodium battery positive electrode precursor has a shell including Ni 0.28 Cu 0.02 Fe 0.3 Mn 0.4 (OH) 2 Except for this, the rest are the same as in Example 1;

[0076] The preparation method of the core-shell structure sodium cathode precursor is the same as that of Example 1 except for the adaptive changes.

[0077] Example 8

[0078] This embodiment provides a core-shell structure sodium cathode precursor. The core-shell structure sodium cathode precursor is the same as that in Embodiment 1 except that in the preparation method thereof, the pH of the reaction in step (2) is 9 to make the core-shell structure sodium cathode precursor adaptable.

[0079] Example 9

[0080] This embodiment provides a core-shell structure sodium cathode precursor. The core-shell structure sodium cathode precursor is the same as that in Embodiment 1 except that in the preparation method thereof, the pH of the reaction in step (2) is 11.5 to make the core-shell structure sodium cathode precursor adaptable.

[0081] Example 10

[0082] This embodiment provides a core-shell structure sodium cathode precursor. The core-shell structure sodium cathode precursor is the same as that of Embodiment 1 except that in the preparation method, the pH of the reaction in step (1) is 9.5 to make the core-shell structure sodium cathode precursor adaptable.

[0083] Embodiment 11

[0084] This embodiment provides a core-shell structure sodium cathode precursor. The core-shell structure sodium cathode precursor is the same as that in Embodiment 1 except that in the preparation method, the pH of the reaction in step (1) is 11.5 to make the core-shell structure sodium cathode precursor adaptable.

[0085] Comparative Example 1

[0086] This comparative example provides a sodium battery positive electrode precursor, which is the same as Example 1 except that it does not include a shell;

[0087] The method for preparing the sodium cathode precursor is the same as that of Example 1 except that the reaction in step (2) is not performed.

[0088] Comparative Example 2

[0089] This comparative example provides a sodium positive electrode precursor, wherein the sodium positive electrode precursor is Ni 0.275 Cu 0.02 Fe 0.3 Mn 0.4 Ti 0.005 (OH) 2 ;

[0090] The method for preparing the sodium positive electrode precursor comprises the following steps:

[0091] Pure water, sodium hydroxide solution and ammonia water were added into the reactor to prepare a reaction base liquid, and nitrogen was introduced. After the base liquid was qualified, a mixed salt solution II of nickel sulfate, copper sulfate, ferrous sulfate, manganese sulfate and titanyl sulfate with a molar ratio of Ni:Cu:Fe:Mn:Ti of 0.275:0.02:0.3:0.4:0.005 was introduced for coprecipitation reaction. The reaction pH was controlled to be 9.5, the ammonia concentration was 2 g / L, the temperature was 40°C, the stirring speed was 300 r / min, and the reaction was stopped when the particle size grew to 8 μm. The precursor was obtained after aging, washing and drying.

[0092] The precursors described in the above examples and comparative examples are respectively prepared into positive electrode materials for sodium ion batteries: the precursor powder is mixed with sodium carbonate according to a molar ratio of sodium content to transition metal of 0.9:1, heated to 600°C at a heating rate of 5°C / min in an air atmosphere for 5 hours, then heated to 800°C at a heating rate of 3°C / min for 10 hours, and cooled naturally to obtain positive electrode materials for sodium ion batteries. The positive electrode materials for sodium ion batteries obtained in each example are prepared into sodium ion batteries, wherein the negative electrode is a sodium sheet, the diaphragm is a polyethylene diaphragm, and the electrolyte is a sodium hexafluorophosphate electrolyte; the specific capacity, cycle capacity retention rate and rate performance of the obtained sodium ion battery are tested, and the test results are shown in Table 1.

[0093] The test method for specific capacity is: using the Blue Electric Battery Test System, at 25°C, the sodium ion battery is charged and discharged three times in the voltage range of 2V to 4.1V at a charge and discharge rate of 0.04A / g (calculated based on the mass of the positive electrode material), and the battery specific capacity is measured;

[0094] The test method for the cycle capacity retention rate is: at 25°C, cycle at a charge and discharge rate of 0.19A / g (calculated based on the mass of the positive electrode material). After 100 cycles, the discharge capacity of the battery at this time is divided by the discharge capacity of the first cycle, which is the 100-cycle cycle capacity retention rate of the battery.

[0095] The test method for rate performance is: at 25°C, with a charge and discharge rate of 0.04A / g (calculated based on the mass of the positive electrode material), within a voltage range of 2V to 4.1V, charge and discharge three times to obtain the discharge capacity C0 of the last cycle; then, with a charging rate of 0.04A / g (calculated based on the mass of the positive electrode material), charge the battery to 4.1V, and with a discharge rate of 0.12A / g (calculated based on the mass of the positive electrode material), discharge the battery to 2V to obtain the discharge capacity C2 of the last cycle; the ratio of C2 / C0 is the rate performance.

[0096] Table 1

[0097]

[0098] From Table 1 we can see that:

[0099] It can be seen from Example 1 and Comparative Examples 1-2 that the present invention can significantly improve the comprehensive performance of the battery through the design of the core-shell structure; it can be seen from Example 1 and Examples 4-7 that the doping of specific elements in the core and shell of the present invention can improve the comprehensive performance of the battery; it can be seen from Example 1 and Examples 8-11 that the pH changes in the first coprecipitation stage and the second coprecipitation stage of the present invention will affect the density of the core and the looseness of the shell, thereby affecting the battery performance.

[0100] In summary, the present invention provides a core-shell structured sodium cathode precursor and a preparation method and application thereof. The core primary particles of the core-shell structured sodium cathode precursor are densely stacked, which is beneficial to improving the compaction density and energy density of the material. Copper elements are added to the outer shell to improve stability while reducing costs, and the outer shell primary particles are loosely stacked to increase porosity and specific surface area, thereby promoting the capacity of the material.

[0101] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A core-shell structure sodium cathode precursor, It is characterized in that The core-shell structured sodium cathode precursor comprises a core and a shell on the surface of the core, wherein the core comprises Ni a Fe b Mn 1-a-b-c M c (OH) 2 , wherein 0.3≤a≤0.5, 0.2≤b≤0.4, 0≤c≤0.01, the shell comprises Ni x Cu y Fe z Mn 1-x-y-z-v N v (OH) 2 , wherein 0.1≤x<0.3, 0.02≤y≤0.2, 0.2≤z≤0.4, 0≤v≤0.01, M and N independently include doped metal elements, and the shell contains pores.

2. The core-shell structure sodium cathode precursor according to claim 1, It is characterized in that The doping metal elements of M and N are different in types; Preferably, the M includes any one of Zn, Mg or Sr or a combination of at least two thereof; Preferably, the N includes any one of Ti, Al or Zr or a combination of at least two of them.

3. The core-shell structure sodium cathode precursor according to claim 1 or 2, It is characterized in that The particle size D50 of the core is 4-6 μm; Preferably, the particle size D50 of the core-shell structured sodium cathode precursor is 8-12 μm.

4. A method for preparing a core-shell structure sodium cathode precursor according to any one of claims 1 to 3, It is characterized in that The preparation method comprises the following steps: (1) introducing a first mixed metal salt solution, a precipitant and a complexing agent into a base solution to perform a first coprecipitation reaction; The first mixed metal salt solution includes a core formula amount of Ni source, Fe source, Mn source and M source; (2) After the first coprecipitation reaction in step (1) is completed, the first mixed metal salt solution is replaced with a second metal salt solution and introduced into the reaction system to perform a second coprecipitation reaction to obtain the core-shell structure sodium cathode precursor; The second mixed metal salt solution includes a Ni source, a Cu source, a Fe source, a Mn source and a N source in shell formula amounts.

5. The preparation method according to claim 4, It is characterized in that Step (1) In the reaction system of the first coprecipitation reaction, the concentration of the complexing agent is 4-8 g / L and the pH is 10.0-11.0; Preferably, the temperature of the first coprecipitation reaction in step (1) is 40-60° C., the stirring speed is 300-400 r / min, and it is carried out in a protective gas.

6. The preparation method according to claim 4 or 5, It is characterized in that The precipitant in step (1) comprises sodium hydroxide solution and / or potassium hydroxide solution; Preferably, the complexing agent in step (1) comprises any one of ammonia, citric acid or oxalic acid, or a combination of at least two of them.

7. The preparation method according to any one of claims 4 to 6, It is characterized in that Step (2) In the reaction system of the second coprecipitation reaction, the concentration of the complexing agent is 2-5 g / L and the pH is 9.5-10.5; Preferably, the temperature of the second coprecipitation reaction in step (2) is 40-60° C., the stirring speed is 300-400 r / min, and it is carried out in a protective gas.

8. The preparation method according to any one of claims 4 to 7, It is characterized in that The preparation method comprises the following steps: (1) introducing a first mixed metal salt solution, a precipitant and a complexing agent into a base liquid, and performing a first coprecipitation reaction in a protective gas at a temperature of 40-60° C. and a stirring speed of 300-400 r / min; The first mixed metal salt solution includes a core formula amount of Ni source, Fe source, Mn source and M source; In the reaction system of the first coprecipitation reaction, the concentration of the complexing agent is 4-8 g / L, and the pH is 10.0-11.0; (2) After the first coprecipitation reaction in step (1) is completed, the first mixed metal salt solution is replaced with a second metal salt solution and introduced into the reaction system, and a second coprecipitation reaction is carried out in a protective gas at a temperature of 40-60° C. and a stirring speed of 300-400 r / min to obtain the core-shell structure sodium cathode precursor; In the reaction system of the second coprecipitation reaction, the concentration of the complexing agent is 2-5 g / L, and the pH is 9.5-10.5; The second mixed metal salt solution includes a Ni source, a Cu source, a Fe source, a Mn source and a N source in shell formula amounts.

9. A sodium ion battery cathode material, It is characterized in that The sodium ion battery positive electrode material is obtained by mixing and sintering a sodium source and a core-shell structure sodium battery positive electrode precursor as described in any one of claims 1 to 3.

10. A sodium ion battery, It is characterized in that The sodium ion battery comprises the sodium ion battery positive electrode material as claimed in claim 9.

Citation Information

Cited By

  • Active-inactive element co-coated sodium electric precursor as well as preparation method and application thereof

    CN119706974A

  • Sodium-ion battery positive electrode precursor having core-shell structure, manufacturing method therefor, and use thereof

    WO2026020712A1