AgBr-doped CsPbBr3 quantum dot glass ceramic as well as preparation and application thereof
By doping AgBr in CsPbBr3 quantum dot glass, using its decomposition and pre-crystallization capabilities, combined with a specific glass matrix, the problem of poor stability of CsPbBr3 quantum dot glass is solved, and AgBr-doped CsPbBr3 quantum dots with high stability and high quantum efficiency are achieved. Dot glass, suitable for LCD backlight panels.
Patent Information
- Application Number
- CN202410857683.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-28
AI Technical Summary
The poor stability of CsPbBr3 quantum dot glass when exposed to water, heat and light limits its use in practical applications.
By doping AgBr into CsPbBr3 quantum dot glass, AgBr is decomposed in the glass matrix to produce Br- to fill the vacancies of CsPbBr3, and silver nanoparticles are used to improve the pre-crystallization ability and plasmon resonance effect, combined with B2O3-SiO2-ZnO-MgO-CaO The base glass system is prevented from being damaged, and AgBr-doped CsPbBr3 quantum dot glass with high stability and high quantum efficiency is prepared.
It significantly improves the photostability and quantum efficiency of CsPbBr3 quantum dot glass, achieves stability under high humidity, high temperature and high blue light conditions, and expands the color gamut, making it suitable for liquid crystal display backlight panels.
Smart Images

Figure BDA0004918480420000021 
Figure BDA0004918480420000022 
Figure BDA0004918480420000031
Abstract
Description
Technical Field
[0001] The invention relates to AgBr-doped CsPbBr3 quantum dot microcrystalline glass and preparation and application thereof, belonging to the field of luminescent glass. Background Art
[0002] With the development of high-quality synthesis processes, all-inorganic CsPbX3 (X=I, Br, Cl) perovskite nanocrystals have attracted extensive research attention due to their excellent optoelectronic properties. By controlling the size and composition of CsPbX3, high color purity, high photoluminescence quantum yield (PLQY) and a wide range of tunable colors across the entire visible spectrum can be achieved. These remarkable properties show the great potential of CsPbX3 in backlight displays, LEDs, lasers and photodetectors. However, their practical applications are severely limited due to their extremely poor stability when exposed to water, heat, light and oxygen.
[0003] In order to improve the moisture stability, thermal stability and light stability of CsPbX3 quantum dots, surface modification, encapsulation protection, synthesis improvement, structural modification and addition of stabilizers can be used. These methods can be used alone or in combination to improve the stability and optoelectronic properties of perovskite quantum dots. These improvement methods are of great significance for the practical application of perovskite quantum dots. Among these strategies, embedding CsPbX3 into glass has been shown to have particular practical application prospects. At present, CsPbX3 has been successfully encapsulated into borosilicate, germanium borate, phosphoborate, phosphosilicate and tellurium borate glass matrices, which tightly surround CsPbX3 and prevent CsPbX3 from being exposed to water and oxygen through a dense network structure. In addition, due to the small number of free electrons in the glass structure, its thermal conductivity is poor, which can partially reduce the effect of temperature on perovskite quantum dots. Unfortunately, when CsPbX3 quantum dots are encapsulated in an inorganic glass matrix, their characteristic of being easily decomposed by light still cannot be solved. In order to improve its photostability, doping modifiers into the CsPbX3 nanocrystal glass matrix is one of the effective methods to improve its stability. Summary of the invention
[0004] In view of the problem that the current CsPbBr3 quantum dot glass has poor photostability, the present invention provides a method for preparing AgBr-doped CsPbBr3 quantum dot glass to achieve high quantum efficiency and high stability.
[0005] The technical solution adopted by the present invention is as follows:
[0006] In a first aspect, the present invention provides a AgBr-doped CsPbBr3 quantum dot glass-ceramics, which is obtained by taking raw materials according to a glass formula, mixing and melting, water quenching, drying, grinding and screening, heat treatment and crystallization, and cooling; the glass formula is composed of the following raw material components, wherein the component content is calculated by the amount of the substance:
[0007]
[0008] Preferably, the glass formula consists of the following raw material components:
[0009]
[0010]
[0011] As a further preference, the glass formula consists of the following raw material components:
[0012]
[0013] As a further preferred embodiment, the glass formula consists of the following raw material components:
[0014]
[0015]
[0016] The glass formulation of the present invention is most preferably composed of the following raw material components:
[0017]
[0018] In a second aspect, the present invention provides a method for preparing the AgBr-doped CsPbBr3 quantum dot glass-ceramics according to the first aspect, comprising the following steps:
[0019] (1) weighing raw material components according to the glass formula, mixing the raw material components and grinding them evenly, and then placing the ground raw material components in a crucible;
[0020] (2) placing the crucible obtained in step (1) into a lifting furnace, raising the temperature to 1100-1400° C., keeping the high temperature for 5-30 minutes, then pouring the molten glass into water for water quenching to obtain glass slag;
[0021] (3) placing the glass residue obtained in step (2) into an oven for drying at a temperature of 40-100° C. for a time of 1-15 hours to obtain a precursor glass;
[0022] (4) grinding and sieving the precursor glass obtained in step (3) to obtain precursor glass powder; and ball-milling the precursor glass through a 200-1000 mesh sieve to obtain precursor glass powders of different particle sizes;
[0023] (5) placing the precursor glass powder obtained in step (4) into a crystallization furnace, heating it to 440-540° C. and keeping it warm for 100-1000 min to allow CsPbBr3 to precipitate and grow in the glass, and then cooling the furnace to obtain AgBr-doped CsPbBr3 quantum dot glass material.
[0024] Preferably, in step (1) of the present invention, the crucible used is a corundum crucible.
[0025] Preferably, in step (2) of the present invention, the melting temperature is 1200°C.
[0026] Preferably, in step (2) of the present invention, the melting time is 10 minutes.
[0027] Preferably, in step (5) of the present invention, heating is performed to 500° C. and the temperature is maintained for 300 min.
[0028] In a third aspect, the present invention provides the use of the AgBr-doped CsPbBr3 quantum dot glass described in the first aspect in the preparation of a liquid crystal display backlight panel.
[0029] The application is specifically as follows: AgBr-doped CsPbBr3 quantum dot glass material is mixed with PS, and melt-extruded to obtain a backlight panel.
[0030] Preferably, the mixing mass ratio of the AgBr-doped CsPbBr3 quantum dot glass material to PS is 4-7:1000.
[0031] Compared with the prior art, the advantages of the present invention are:
[0032] (1) The B2O3-SiO2-ZnO-MgO-Al2O3-CaO-based glass system used in the present invention can effectively prevent CsPbBr3 from being destroyed in the air and obtain CsPbBr3 quantum dots.
[0033] (2) AgBr has the property of being easily decomposed by light. In the present invention, it is doped into the glass matrix, and it decomposes into Br when exposed to light. - , thus filling the Br vacancies generated when CsPbBr3 is illuminated. + During the cooling process of the glass melt, part of it is reduced to silver nanoparticles, which can act as a nucleating agent to improve the pre-crystallization ability of CsPbBr3. It can also produce a plasma resonance effect in the glass matrix, obtain excellent quantum efficiency and higher stability, and realize the control of the optical properties of CsPbBr3 quantum dot glass.
[0034] (3) The PS liquid crystal display backlight panel of the present invention still has good stability under the aging conditions of high humidity, high temperature and high blue light. After being doped with 1.0 AgBr, its stability is significantly improved compared with that without AgBr doping.
[0035] (4) The AgBr-doped CsPbBr3 quantum dot glass material of the present invention has a wider color gamut in display.
[0036] The present invention will be further described below in conjunction with the accompanying drawings and specific implementation methods. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, without paying creative labor, other drawings obtained based on these drawings still belong to the scope of the present invention.
[0038] Figure 1 This is a sample picture of the precursor glass prepared in an embodiment of the present invention; through the photos taken under sunlight and ultraviolet light, it can be seen that as the AgBr doping concentration increases, the color of the five samples becomes darker and darker under normal light, and the green light becomes more and more obvious under ultraviolet light irradiation, indicating that AgBr can promote the pre-crystallization ability of CsPbBr3.
[0039] Figure 2 This is a sample picture of the CsPbBr3 quantum dot glass-ceramic material prepared in an embodiment of the present invention.
[0040] Figure 3 This is the XRD diagram of the CsPbBr3 quantum dot glass-ceramic material prepared in an embodiment of the present invention. It can be seen from the figure that as the AgBr concentration increases, the position of the 110 crystal plane peak changes.
[0041] Figure 4 PL fluorescence and absorption diagram of the CsPbBr3 quantum dot glass-ceramic material prepared in an embodiment of the present invention.
[0042] Figure 5 These are sample images of a backlight panel A prepared according to an embodiment of the present invention, with the left image being a normal light image and the right image being a purple light image.
[0043] Figure 6 Stability diagrams of backlight panels A and B prepared according to embodiments of the present invention.
[0044] Figure 7 The third embodiment of the present invention and the commercial phosphor K2SiF6:Mn 4+ Color gamut diagram of blue light chip excitation after combination. DETAILED DESCRIPTION
[0045] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below with reference to the accompanying drawings.
[0046] Examples 1-5
[0047] (1) Weighing raw material components according to the glass formula shown in Table 1, mixing the raw material components and grinding them evenly, and then placing the ground raw material components in a corundum crucible;
[0048] (2) Place the corundum crucible in a muffle furnace, heat the temperature from room temperature to 1200°C in 120 minutes, and keep it warm for 10 minutes. Then pour the glass melt into water for water quenching to obtain glass slag;
[0049] (3) The glass slag was placed in a 60°C oven for drying for 500 minutes and the glass precursor was dried to obtain the precursor glass. The sample pictures under sunlight and ultraviolet light are as follows Figure 1 As shown;
[0050] (4) then mechanically ball-milling the precursor glass and passing it through a 350-mesh sieve to obtain a precursor glass powder;
[0051] (5) The precursor glass powder is placed in an annealing furnace, heated to 500°C and heat treated for 300 min to allow CsPbBr3 to precipitate and grow in the glass, and then cooled in the furnace to obtain CsPbBr3 quantum dot glass material. The sample images under sunlight and ultraviolet light are shown in FIG. Figure 2 shown.
[0052] Table 1
[0053]
[0054]
[0055] The prepared quantum dot glass-ceramics were subjected to structural analysis and photoelectric performance tests, such as Figure 3 As shown, the standard peak of CsPbBr3 appears in XRD, confirming that the CsPbBr3 quantum dot glass is successfully prepared, and with the addition of AgBr, the 110 crystal plane peak changes, proving that AgBr affects the structure of CsPbBr3.
[0056] Test the PL and absorption of CsPbBr3 quantum dot glass-ceramics. The results are as follows Figure 4 As shown, it indicates that when the AgBr doping amount is 1.0, its PL reaches the maximum value.
[0057] Example 6
[0058] The CsPbBr3 quantum dot glass powder prepared in Example 3 was mixed with a commercial PS masterbatch at a mass ratio of 5:1000, and extruded at 220° C. using a twin-screw extruder to obtain a backlight plate A. Figure 5 As shown, the left picture is the normal light picture, and the right picture is the purple light picture.
[0059] The CsPbBr3 quantum dot glass powder prepared in Example 1 was mixed with a commercial PS masterbatch at a mass ratio of 5:1000, and a backlight plate B was obtained by extruding the mixture at 220° C. using a twin-screw extruder.
[0060] The backlight panels A and B were tested under high humidity (RH=90%), high temperature (60 degrees Celsius), strong blue light (200W / m 2 ) under aging conditions, the results are as follows Figure 6 As shown, backlight panel A has higher stability, and its fluorescence intensity still remains above 90% after 1000 hours.
[0061] Example 7
[0062] The CsPbBr3 quantum dot glass powder prepared in Example 3 and the commercial phosphor K2SiF6:Mn 4+ Mixed in a mass ratio of 3:2, tested in an optical integrating sphere, the color gamut diagram measured by 450nm blue light chip excitation is shown in Figure 7 .
[0063] The above disclosure is only the preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.
Claims
1. An AgBr-doped CsPbBr3 quantum dot microcrystalline glass, which is obtained by taking raw materials according to a glass formula, mixing and melting, water quenching, drying, grinding and screening, heat treatment and crystallization, and cooling; characterized in that: The glass formula is composed of the following raw material components, wherein the component contents are calculated by the amount of substance:
2. The AgBr-doped CsPbBr3 quantum dot glass-ceramics according to claim 1, characterized in that: The glass formula is composed of the following raw material components:
3. The AgBr-doped CsPbBr3 quantum dot glass-ceramics according to claim 2, characterized in that: The glass formula is composed of the following raw material components:
4. The AgBr-doped CsPbBr3 quantum dot glass-ceramics according to claim 3, characterized in that: The glass formula is composed of the following raw material components:
5. The AgBr-doped CsPbBr3 quantum dot glass-ceramics according to claim 4, characterized in that: The glass formula is composed of the following raw material components:
6. A method for preparing AgBr-doped CsPbBr3 quantum dot glass-ceramics as claimed in any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: (1) weighing raw material components according to the glass formula, mixing the raw material components and grinding them evenly, and then placing the ground raw material components in a crucible; (2) placing the crucible obtained in step (1) into a lifting furnace, raising the temperature to 1100-1400° C., keeping the high temperature for 5-30 minutes, then pouring the molten glass into water for water quenching to obtain glass slag; (3) placing the glass residue obtained in step (2) into an oven for drying at a temperature of 40-100° C. for a time of 1-15 hours to obtain a precursor glass; (4) grinding and sieving the precursor glass obtained in step (3) to obtain precursor glass powder; and ball-milling the precursor glass powder through a 200-1000 mesh sieve to obtain precursor glass powders of different particle sizes; (5) placing the precursor glass powder obtained in step (4) into a crystallization furnace, heating it to 440-540° C. and keeping it warm for 100-1000 min to allow CsPbBr3 to precipitate and grow in the glass, and then cooling the furnace to obtain AgBr-doped CsPbBr3 quantum dot glass material.
7. The preparation method according to claim 6, characterized in that: In step (5), the temperature is heated to 500° C. and kept at this temperature for 300 min.
8. Use of the AgBr-doped CsPbBr3 quantum dot glass as claimed in any one of claims 1 to 5 in the preparation of a liquid crystal display backlight panel.
9. The use according to claim 8, characterized in that: The application is specifically as follows: AgBr-doped CsPbBr3 quantum dot glass material is mixed with PS, and melt-extruded to obtain a backlight panel.
10. The use according to claim 9, characterized in that: The mixing mass ratio of the AgBr-doped CsPbBr3 quantum dot glass material to PS is 4-7:1000.
Citation Information
Patent Citations
Al < 3 + >-doped CsPbBr3 quantum dot glass ceramic and preparation method thereof
CN114634312A
Full-inorganic perovskite quantum dot microcrystalline glass material and preparation method thereof
CN115124247A