Preparation method of bio-based degradable material

By melt-blending materials such as PPCP, PBAT and modified corn starch, and using specific catalyst and modifier ratios, the problems of insufficient mechanical properties, transparency and barrier properties of existing biodegradable materials have been solved, and a product with excellent High-performance and low-cost biodegradable materials suitable for large-scale promotion.

CN118772602AInactive Publication Date: 2024-10-15DONGGUAN LONGXIN BIO-ENVIRONMENTAL TECH CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411050752.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing biodegradable materials have deficiencies in mechanical properties, transparency and barrier properties, as well as high cost, which limits their wide application.

Method used

A new type of carbon dioxide copolymer (PPCP) synthesized from monomers such as carbon dioxide and propylene oxide is melt-blended with materials such as polybutylene adipate/terephthalate (PBAT) and modified corn starch, and is passed through a specific catalyst. Mixed with modifiers to prepare biodegradable materials with high biodegradability, heat sealing performance and transparency.

Benefits of technology

The prepared biodegradable material has excellent biodegradability and heat sealing performance, good water and air barrier effect, high transparency and barrier properties, low cost, and is suitable for large-scale promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004974839790000101
    Figure BDA0004974839790000101
Patent Text Reader

Abstract

The invention provides a preparation method of a bio-based degradable material, which comprises the following steps: drying raw materials, uniformly mixing, carrying out melt blending, extruding to obtain granules, and carrying out film blowing and blow molding on the granules to obtain the bio-based degradable material. The raw materials comprise the following components in parts by weight: 20-40 parts of PPCP, 60-80 parts of PBAT, 10-25 parts of modified corn starch, 1-3 parts of an initiator and 2-6 parts of maleic anhydride. The biodegradable material prepared by the preparation method of the bio-based degradable material is excellent in biodegradability and heat sealability, good in water and gas insulation effect, excellent in fresh-keeping and aroma-keeping functions and high in transparency and barrier property, is very suitable for preparing a film bag material, is low in cost and can be popularized and prepared in a large scale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of degradable materials, and specifically relates to a method for preparing a bio-based degradable material. Background Art

[0002] Traditional plastic materials are usually derived from fossil fuels, which are limited resources and produce a lot of carbon emissions during mining and use. A large amount of plastic waste is difficult to degrade in the natural environment, causing long-term pollution and damage to soil, water and organisms.

[0003] With the improvement of environmental awareness, more and more consumers begin to pay attention to the environmental performance of products, and the demand for biodegradable materials is gradually increasing. Biodegradable materials can use renewable resources, such as plant fiber, starch, etc. These resources are widely available and have low carbon emissions during use. They can be processed by composting and other methods and converted into resources such as organic fertilizers, which improves waste treatment efficiency and resource utilization, and helps save resources and mitigate global climate change.

[0004] Poly(methyl ethylene carbonate) (PPC) synthesized from carbon dioxide and propylene oxide is an important biodegradable plastic. PPC is an amorphous polymer with high barrier properties, which enriches the variety of biodegradable plastics. However, the low glass transition temperature and mechanical properties of PPC limit its wide application. Polybutylene adipate / terephthalate (PBAT) has good ductility and elongation at break, as well as good heat resistance and impact resistance, but its high price limits its market application.

[0005] Therefore, it is necessary to develop a biodegradable material that has high biodegradability and heat-sealing properties, high transparency and barrier properties, good mechanical properties, low cost, and can be promoted on a large scale. Summary of the invention

[0006] The object of the present invention is to provide a method for preparing a bio-based degradable material. The biodegradable material prepared by the method has excellent biodegradability and heat sealing properties, good water and air barrier effects, excellent freshness and fragrance preservation functions, high transparency and barrier properties, is very suitable for preparing film bag materials, has low cost, and can be promoted and prepared on a large scale.

[0007] In order to achieve the above object, the present invention provides the following technical solutions:

[0008] The preparation method of the bio-based degradable material comprises the following steps: drying the raw materials and mixing them uniformly, extruding them after melt blending to obtain pellets, and forming the pellets by film blowing.

[0009] Preferably, the melt blending temperature is 135-150° C., and the rotation speed is 30-50 r / min.

[0010] Preferably, the film blowing temperature zone is 135-150° C., the screw speed is 10-15 r / min, the traction speed is 3-6 r / min, and the winding speed is 3-5 r / min.

[0011] The raw materials include the following components by weight: 20 to 40 parts of PPCP, 60 to 80 parts of PBAT, 10 to 25 parts of modified corn starch, 1 to 3 parts of initiator, and 2 to 6 parts of maleic anhydride. Among them, PPCP refers to a new type of carbon dioxide copolymer synthesized from monomers such as carbon dioxide and propylene oxide.

[0012] The preparation method of PPCP comprises the following steps: adding phthalic anhydride, epichlorohydrin and a catalyst into a high-pressure reactor, introducing carbon dioxide to carry out a ternary ring-opening copolymerization reaction, cooling the high-pressure reactor to room temperature after the reaction is completed, releasing carbon dioxide, dissolving the mixture in the reactor in chloroform, removing the catalyst in the system with hydrochloric acid with a volume concentration of 5%, washing with distilled water for three times, concentrating and precipitating with methanol, filtering and vacuum drying at 80°C for 48 hours to obtain the PPCP.

[0013] Preferably, the catalyst is tetra-n-butylammonium chloride and triethylboron.

[0014] Preferably, the molar ratio of tetra-n-butylammonium chloride to triethylboron is 1:(3-7); more preferably, it is 1:5.

[0015] The inventors found that the use of tetra-n-butylammonium chloride and triethylboron as catalysts to catalyze the generation of PPCP can improve the reaction efficiency while not affecting the degradability of PPCP. This may be because on the one hand, the stable ion pair and keratolytic properties of tetra-n-butylammonium chloride complement the initiator effect of triethylboron and jointly promote the reaction. On the other hand, tetra-n-butylammonium chloride and triethylboron synergistically contribute to the transfer of reactants between the aqueous phase and the organic phase, quickly forming active intermediates, making the reaction more uniform, improving the reaction efficiency, and accelerating the copolymerization reaction. In addition, the catalyst system composed of triethylboron and tetra-n-butylammonium chloride does not contain metal components, and while forming a new PPCP structure, the biodegradability of the PPC material is retained, and the PPCP material has extremely high light transmittance while still having excellent degradability.

[0016] Preferably, the molar ratio of tetra-n-butylammonium chloride, phthalic anhydride and propylene oxide is 1:(200-400):(2000-3000).

[0017] The inventors found that by introducing phthalic anhydride and reacting under specific conditions, PPCP can be prepared, and it is applied to the preparation of biodegradable materials, which can improve the mechanical properties of biodegradable materials while improving the transparency and heat sealing properties of its biodegradable materials. This may be because the introduction of phthalic anhydride changes the molecular chain structure of PPC, and an aromatic polyester structure is introduced into the PPC main chain through copolymerization. The introduction of this structure strengthens the interaction between molecular chains on the one hand, thereby improving the mechanical strength of PPC, and on the other hand, it may make the PPC molecular chain more regular, reduce light scattering, thereby improving the transparency of the material, and may also make the PPC molecular chain more compact, thereby effectively blocking the penetration of materials such as gas and liquid. In addition, although the introduction of phthalic anhydride can reduce the melt index (i.e., the fluidity of the molecular chain) of PPC to a certain extent, under appropriate phthalic anhydride content, this reduction may help to form a more compact and uniform sealing interface in the heat sealing process, thereby improving the heat sealing performance. But too much phthalic anhydride may cause excessive cross-linking of molecular chains, which reduces mechanical properties instead and affects the various properties of the prepared bio-based degradable materials.

[0018] Preferably, the carbon dioxide pressure of the ternary ring-opening copolymerization reaction is 0.5-1.5 MPa, the reaction temperature is 70-80° C., and the reaction time is 10-15 h.

[0019] Preferably, the elongation at break of the PBAT is ≥300%, the melt flow rate at 190°C is 1-5g / 10min, and the Vicat softening temperature is ≥80°C; further preferably, the elongation at break of the PBAT is ≥400%, the melt flow rate at 190°C is 2.5-4.5g / 10min, and the Vicat softening temperature is ≥80°C.

[0020] In some preferred embodiments, the PBAT is purchased from Xinjiang Blue Mountain Tunhe Chemical Industry, TH-801T.

[0021] The preparation method of the modified corn starch comprises the following steps: vacuum drying the corn starch at 70-90° C. to constant weight, adding a modifier, stirring evenly and sealing, vacuum drying at 70-90° C. for 5-8 hours and then taking out, and melt blending at 110-130° C. to obtain the modified corn starch.

[0022] Preferably, the amount of the modifier added is 20-30% of the corn starch.

[0023] Preferably, the modifiers are glycerol and sorbitol.

[0024] Preferably, the mass ratio of glycerol to sorbitol is 1:(0.5-2); further preferably, it is 1:1.

[0025] Corn starch is a natural biodegradable material with low price, but its own structural limitations make it impossible to process and shape it by melting method. The inventors found that the use of glycerol and sorbitol with a mass ratio of 1: (0.5-2) as modifiers to modify corn starch can improve the mechanical properties of biodegradable materials while also improving processing performance. This may be because the two modifiers work synergistically to destroy the original crystalline structure of starch, making the starch molecules loose, thereby improving the thermoplasticity of starch, allowing it to be processed and shaped by melting method, thereby improving the various properties of the biodegradable materials obtained by molding. At the same time, the two substances will also react with starch to form new bonds, further enhancing the strength of starch, and the smaller glycerol molecules also have a certain lubricating effect, thereby further improving the processing performance. The inventors found in actual experiments that although glycerol has a better plasticizing effect than sorbitol and can improve the biodegradability of biodegradable materials, excessive addition of glycerol will cause corn starch to be over-plasticized, and molecules are more likely to slip, resulting in a decrease in tensile strength, affecting the mechanical properties of biodegradable materials. Even if corn starch is modified, its compatibility with PPCP and PBAT is still poor, and the three substances are only physically blended, which affects the performance of the final biodegradable material.

[0026] Preferably, the mass ratio of the PPCP, PBAT and modified corn starch is (1-2): (3-4): 1; more preferably, it is 3:7:2.

[0027] Preferably, the initiator is benzoyl peroxide.

[0028] Preferably, the total mass of the initiator and maleic anhydride is 4% to 6% of the total mass of PPCP, PBAT and modified corn starch.

[0029] The inventors found that by selecting a specific PBAT, and the mass ratio of the PPCP, PBAT and modified corn starch is (1-2): (3-4): 1, and introducing maleic anhydride at the same time, the various properties of the biodegradable material finally prepared can be optimized. This may be because on the one hand, the chain segments of PPCP will form an interpenetrating network structure with the chain segments of PBAT, thereby enhancing the interaction between molecules, and can also change the crystallization behavior of PBAT, thereby improving the mechanical properties and heat sealing properties of the biodegradable material. On the other hand, the filling effect and interfacial interaction of the modified corn starch can not only reduce the movement of the PBAT chain segments, thereby improving the heat sealing properties and mechanical properties of the biodegradable material, but also can be compounded with PPCP to improve the barrier properties of the biodegradable material. However, excessive addition of corn starch will greatly reduce the melt strength, which is not conducive to the processing and molding of materials to obtain plastic film products. In addition, the introduction of an appropriate amount of maleic anhydride can not only promote the cutoff reaction of glycerol on the corn starch molecular chain, but also promote the grafting effect of corn starch and PBAT, improve the interaction between the two phases, and increase the compatibility of corn starch in the system, thereby improving the various properties of the biodegradable material. However, if the amount of maleic anhydride added is too high, its molecules will interact with each other, which is not conducive to the dispersion of corn starch in the system, thereby affecting the molding effect and further affecting the various properties of the final material.

[0030] Compared with the prior art, the advantages and beneficial effects of the present invention are:

[0031] The present invention provides a method for preparing a bio-based degradable material. The prepared biodegradable material has excellent biodegradability and heat sealing properties, good water and air barrier effects, excellent freshness and fragrance preservation functions, high transparency and barrier properties, and good mechanical properties. The material does not contain metal, thereby expanding the application scope of the material, has low cost, and can be prepared on a large scale.

[0032] The present invention introduces phthalic anhydride and reacts under specific conditions to prepare PPCP, which is applied to prepare biodegradable materials, thereby improving the mechanical properties of the biodegradable materials while improving the transparency and heat-sealing properties of the biodegradable materials.

[0033] The present invention selects tetra-n-butylammonium chloride and triethylboron as catalysts to catalyze the generation of PPCP, which can improve the reaction efficiency while not affecting the degradability of PPCP.

[0034] The invention selects glycerol and sorbitol in a mass ratio of 1: (0.5-2) as modifiers to modify corn starch, thereby improving the mechanical properties of the biodegradable material and the processing performance.

[0035] The present invention selects a specific PBAT, and the mass ratio of the PPCP, PBAT and modified corn starch is (1-2): (3-4): 1, and maleic anhydride is introduced, so that the properties of the finally prepared biodegradable material can be optimized. DETAILED DESCRIPTION

[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] The raw materials used in the present invention are all commercially available, specifically:

[0038] The elongation at break of PBAT is ≥400%, the melt flow rate is 2.5-4.5 g / 10 min at 190°C, and the Vicat softening temperature is ≥80°C. It was purchased from Xinjiang Lanshan Tunhe Chemical Industry, TH-801T.

[0039] Example 1

[0040] This embodiment provides a method for preparing a bio-based degradable material, the steps of which are: drying the raw materials and mixing them evenly, extruding them after melt blending to obtain pellets, and forming the pellets by film blowing.

[0041] The melt blending temperature is 140° C. and the rotation speed is 40 r / min.

[0042] The film blowing zone is divided into a feeding section, a melting section and a homogenizing section, the temperatures are 135° C., 140° C. and 150° C. respectively, the screw speed is 13 r / min, the traction speed is 5 r / min, and the winding speed is 4 r / min.

[0043] The raw materials include the following components by weight: 30 parts of PPCP, 70 parts of PBAT, 20 parts of modified corn starch, 2 parts of initiator, and 4 parts of maleic anhydride.

[0044] The preparation method of PPCP comprises the following steps: adding phthalic anhydride, epichlorohydrin and a catalyst into a high-pressure reactor, introducing carbon dioxide to carry out a ternary ring-opening copolymerization reaction, cooling the high-pressure reactor to room temperature after the reaction is completed, releasing carbon dioxide, dissolving the mixture in the reactor in chloroform, removing the catalyst in the system with hydrochloric acid having a volume concentration of 5%, washing with distilled water for three times, concentrating, precipitating with methanol, filtering and vacuum drying at 80° C. for 48 hours to obtain the PPCP.

[0045] The catalyst is tetra-n-butylammonium chloride and triethylboron.

[0046] The molar ratio of tetra-n-butylammonium chloride to triethylboron is 1:5.

[0047] The molar ratio of tetra-n-butylammonium chloride, phthalic anhydride and propylene oxide is 1:300:2500.

[0048] The carbon dioxide pressure of the ternary ring-opening copolymerization reaction is 1 MPa, the reaction temperature is 75° C., and the reaction time is 12 h.

[0049] The preparation method of the modified corn starch comprises the following steps: vacuum drying the corn starch at 80°C to constant weight, adding a modifier, stirring evenly and sealing, vacuum drying at 80°C for 6 hours and then taking out, and melt blending at 120°C to obtain the modified corn starch.

[0050] The added amount of the modifier is 25% of the corn starch.

[0051] The modifiers are glycerol and sorbitol.

[0052] The mass ratio of the glycerol to sorbitol is 1:1.

[0053] The initiator is benzoyl peroxide.

[0054] Example 2

[0055] The difference between this embodiment and embodiment 1 is that the raw materials, by weight, include the following components: 40 parts of PPCP, 80 parts of PBAT, 20 parts of modified corn starch, 2 parts of initiator, and 4 parts of maleic anhydride.

[0056] Example 3

[0057] The difference between this embodiment and embodiment 1 is that the raw materials, by weight, include the following components: 20 parts of PPCP, 60 parts of PBAT, 20 parts of modified corn starch, 2 parts of initiator, and 4 parts of maleic anhydride.

[0058] Comparative Example 1

[0059] The difference between this comparative example and Example 1 is that the raw materials, by weight, include the following components: 50 parts of PPCP, 50 parts of PBAT, 20 parts of modified corn starch, 2 parts of initiator, and 4 parts of maleic anhydride.

[0060] Comparative Example 2

[0061] The difference between this comparative example and Example 1 is that the raw materials, by weight, include the following components: 30 parts of PPCP, 70 parts of PBAT, 20 parts of modified corn starch, 2 parts of initiator, and 10 parts of maleic anhydride.

[0062] Comparative Example 3

[0063] The difference between this comparative example and Example 1 is that the molar ratio of tetra-n-butylammonium chloride, phthalic anhydride and propylene oxide is 1:1000:2500.

[0064] Comparative Example 4

[0065] The difference between this comparative example and Example 1 is that the molar ratio of tetra-n-butylammonium chloride to triethylboron is 1:1.

[0066] Comparative Example 5

[0067] The difference between this comparative example and Example 1 is that the PBAT has an elongation at break of ≥150%, a melt flow rate of 4-7 g / 10 min at 190° C., and a Vicat softening temperature of ≥80° C., and is purchased from Xinjiang Blue Mountain Tunhe Chemical Industry, TH-803S.

[0068] Comparative Example 6

[0069] The difference between this comparative example and Example 1 is that the modifier is glycerol.

[0070] Comparative Example 7

[0071] The difference between this comparative example and Example 1 is that the raw materials, by weight, include the following components: 30 parts of PPCP, 70 parts of PBAT, 35 parts of modified corn starch, 2 parts of initiator, and 4 parts of maleic anhydride.

[0072] Performance Testing

[0073] Refer to GB / T 38082-2019 "Biodegradable Plastic Shopping Bags" to test the biodegradability and heat sealability of the material. The relative biodegradability should be ≥90%, and the heat seal strength should be ≥8N. Refer to GB / T 1040-2006 "Determination of Tensile Properties of Plastics" to test the tensile properties of the material. Refer to GB / T 2410-2008 "Determination of Light Transmittance and Haze of Transparent Plastics" to test the light transmittance of the material. Refer to GB / T 19789-2021 "Oxygen Permeability Test for Plastic Films and Sheets for Packaging Materials - Coulometer Test Method" to test the oxygen permeability of the material, unit: cm 3 / (m 2 ·24h·0.1MPa). Refer to GB 1037-70 "Test method for water vapor permeability of plastic film and sheet - cup method" to test the water vapor permeability of the material, unit: g / (m 2 The results are shown in Table 1.

[0074] Table 1 Measurement results

[0075]

[0076] According to statistics, the bio-based degradable materials prepared in Examples 1 to 3 of the present invention have high relative biodegradability and heat-sealing strength, which meet the national standard requirements, high tensile strength and transparency, and low oxygen permeability and water vapor permeability. In Comparative Example 1, the amount of PPCP added is too high, the amount of PBAT added is too low, the amount of maleic anhydride added is too high in Comparative Example 2, the amount of phthalic anhydride added is too high in Comparative Example 3, the amount of triethyl boron added is too low in Comparative Example 4, the elongation at break of the selected PBAT in Comparative Example 5 is too low, sorbitol is not added in Comparative Example 6, and the amount of modified corn starch added in Comparative Example 7 is too high. The various properties of the prepared bio-based degradable materials do not fully meet the requirements. Therefore, the relative biodegradability and heat-sealing strength prepared by the method described in this application meet the national standard requirements, the tensile strength and light transmittance are high, the oxygen permeability and water vapor permeability are low, the water-proof and air-proof effect is good, and the fresh-keeping and fragrance-preserving functions are excellent.

[0077] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a biodegradable material, It is characterized in that The method comprises the following steps: drying the raw materials and mixing them uniformly, extruding the raw materials after melt blending to obtain pellets, and forming the pellets by film blowing; The raw materials include the following components by weight: 20 to 40 parts of PPCP, 60 to 80 parts of PBAT, 10 to 25 parts of modified corn starch, 1 to 3 parts of initiator, and 2 to 6 parts of maleic anhydride; The preparation method of PPCP comprises the following steps: adding phthalic anhydride, epichlorohydrin and a catalyst into a high-pressure reactor, introducing carbon dioxide to carry out a ternary ring-opening copolymerization reaction, cooling the high-pressure reactor to room temperature after the reaction is completed, releasing carbon dioxide, dissolving the mixture in the reactor in chloroform, removing the catalyst in the system with hydrochloric acid with a volume concentration of 5%, washing with distilled water three times, concentrating and precipitating with methanol, filtering and vacuum drying at 80°C for 48 hours to obtain the PPCP; The catalyst is tetra-n-butylammonium chloride and triethyl boron; The molar ratio of tetra-n-butylammonium chloride to triethylboron is 1:(3-7); The PBAT has an elongation at break of ≥300%, a melt flow rate of 1-5 g / 10 min at 190° C., and a Vicat softening temperature of ≥80° C.; The mass ratio of the PPCP, PBAT and modified corn starch is (1-2):(3-4):

1.

2. The method for preparing the biodegradable material according to claim 1, It is characterized in that The molar ratio of tetra-n-butylammonium chloride, phthalic anhydride and propylene oxide is 1:(200-400):(2000-3000).

3. The method for preparing the biodegradable material according to claim 1, It is characterized in that The carbon dioxide pressure of the ternary ring-opening copolymerization reaction is 0.5-1.5 MPa, the reaction temperature is 70-80° C., and the reaction time is 10-15 hours.

4. The method for preparing the biodegradable material according to claim 1, It is characterized in that The preparation method of the modified corn starch comprises the following steps: vacuum drying the corn starch at 70-90° C. to constant weight, adding a modifier, stirring evenly and sealing, vacuum drying at 70-90° C. for 5-8 hours and then taking out, and melt blending at 110-130° C. to obtain the modified corn starch.

5. The method for preparing the biodegradable material according to claim 4, It is characterized in that The added amount of the modifier is 20-30% of the corn starch.

6. The method for preparing the biodegradable material according to claim 5, It is characterized in that The modifiers are glycerol and sorbitol.

7. The method for preparing the biodegradable material according to claim 6, It is characterized in that The mass ratio of the glycerol to sorbitol is 1:(0.5-2).

8. The method for preparing the biodegradable material according to claim 1, It is characterized in that The initiator is benzoyl peroxide.

9. The method for preparing the biodegradable material according to claim 1, It is characterized in that The total mass of the initiator and maleic anhydride is 4% to 6% of the total mass of PPCP, PBAT and modified corn starch.

10. A bio-based degradable material prepared according to the method for preparing a bio-based degradable material according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Starch foaming packaging material with full biodegradable property and preparation method thereof

    CN109880183A

  • Preparation method of biodegradable carbon dioxide-based polyester-polycarbonate terpolymer

    CN111378101A

  • High-strength PBAT / starch biodegradable master batch and preparation method thereof

    CN114316524A

  • High-toughness composition of semi-aromatic carbon dioxide-based copolymer and preparation method of high-toughness composition

    CN114525017A

  • Method for predicting service life of biodegradable mulching film

    CN115711845A