Binder for secondary battery, preparation method thereof, diaphragm, battery monomer, battery and electric device

By using an organic polymer binder with a specific glass transition temperature, the battery cell opening problem is solved and the hardness and cycle performance of the battery cell are improved.

CN118772805APending Publication Date: 2024-10-15CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
CN202310369599.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Battery cells have a problem with large openings, and gaps are easily formed between the pole pieces and the separators, resulting in poor battery cycle performance.

Method used

Adopt a binder including an organic polymer, the organic polymer has a first glass transition temperature less than or equal to 25°C and a second glass transition temperature greater than 25°C, so that the binder has both The soft and hard properties can penetrate into the pores of the diaphragm and the pole piece, improving the bonding force between the diaphragm and the pole piece.

Benefits of technology

The cold-pressed adhesion between the separator and the positive and negative electrode sheets is improved, and the hardness of the battery core and the cycle performance of the secondary battery are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772805A_ABST
    Figure CN118772805A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of secondary batteries, in particular to a binder for a secondary battery, a preparation method of the binder, and a diaphragm, a battery monomer, a battery and an electric device containing the binder. The binder for a secondary battery includes an organic polymer including a first glass transition temperature less than or equal to 25 DEG C and a second glass transition temperature greater than 25 DEG C. When the diaphragm is coated, the adhesive is non-viscous at room temperature, so that the diaphragm is convenient to wind and unwind. However, when the cold pressing process is performed after the positive and negative pole pieces are wound, the binder has better binding power, so that the positive and negative pole pieces and the diaphragm are tightly attached to each other. Therefore, according to the binder disclosed by the invention, the cold pressing binding power of the diaphragm and the positive and negative pole pieces is improved, so that the hardness of a battery cell and the cycle performance of the secondary battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of secondary batteries, and in particular to a binder for secondary batteries and a preparation method thereof, as well as a diaphragm, a battery cell, a battery and an electrical device. Background Art

[0002] With the rapid growth of portable electronic devices and electric vehicles, the demand for power batteries is also growing. Among them, the electrochemical performance of batteries is also attracting more and more attention.

[0003] At present, battery cells have the problem of large openings, that is, gaps are easily formed between the pole pieces and the diaphragms, resulting in poor battery cycle performance. Summary of the invention

[0004] The main purpose of the present invention is to provide a binder, which aims to improve the bonding force between the separator and the pole piece and improve the cycle performance of the battery.

[0005] To achieve the above object, the present invention provides a binder for a secondary battery, the binder includes an organic polymer, the organic polymer includes a first glass transition temperature and a second glass transition temperature, the first glass transition temperature is less than or equal to 25°C, and the second glass transition temperature is greater than 25°C.

[0006] At a certain temperature, the structure of the organic polymer including the first glass transition temperature is in a soft state and can be deformed with the extrusion force, while the structure of the diaphragm and the electrode has pores. As the extrusion force acts on the organic polymer, part of the structure of the organic polymer can penetrate into the pores of the diaphragm and the electrode, bonding the diaphragm and the adhesive together, achieving a mechanical interlocking effect and realizing the bonding function.

[0007] Since there is a significant difference between the first glass transition temperature and the second glass transition temperature of the organic polymer, when cold pressed at a certain temperature, the structure of the organic polymer including the first glass transition temperature is in a rubber state, and the structure of the organic polymer including the second glass transition temperature is in a glass state, so that the binder has the characteristics of "both soft and hard". After it is coated on the diaphragm, the binder is non-sticky when there is no pressure at a certain temperature, which can meet the requirements of winding and unwinding the diaphragm. When a certain pressure is applied, the binder shows pressure sensitivity and better adhesion, which meets the bonding requirements of the diaphragm and the positive and negative pole pieces.

[0008] Therefore, when the adhesive of the present application is used to coat the diaphragm, the adhesive has no adhesiveness at a certain temperature to facilitate the winding and unwinding of the diaphragm, but after being wound with the positive and negative pole pieces and undergoing a cold pressing process, the adhesive has better adhesiveness, so that the positive and negative pole pieces and the diaphragm fit closely to each other. Therefore, the adhesive of the present application improves the cold pressing adhesiveness between the diaphragm and the positive and negative pole pieces, thereby improving the hardness of the battery cell and the cycle performance of the secondary battery.

[0009] Preferably, the first glass transition temperature ranges from -80°C to 25°C, preferably from -60°C to 25°C.

[0010] Within the above range, the organic polymer including the structure of the first glass transition temperature is in a rubbery state at a certain temperature, which is conducive to exerting its adhesion during the cold pressing process, and is conducive to the adhesion between the diaphragm and the electrode after cold pressing, thereby improving the performance of the battery.

[0011] Preferably, the second glass transition temperature ranges from 26°C to 100°C, preferably from 26°C to 90°C.

[0012] Within the above range, the organic polymer includes a structure with a second glass transition temperature that is in a glassy state at a certain temperature, which is beneficial as a skeleton structure of the adhesive at a certain temperature, making the adhesive non-sticky and facilitating the winding and unwinding steps of the diaphragm at a certain temperature.

[0013] Preferably, the organic polymer includes an acrylic ester copolymer, and / or the organic polymer includes at least one of an ester group, a carboxyl group, an acrylamide group, a carbonyl group, an amide group, and a nitrile group.

[0014] Acrylate copolymers have good adhesion. The use of acrylic copolymers can improve the adhesion between the diaphragm and the pole piece after cold pressing.

[0015] The ester group can improve the anti-swelling ability of the polymer, and as a flexible monomer segment in the molecular chain segment, it can adjust the glass transition temperature of the organic polymer, which helps to adjust the glass transition temperature of the polymer within a suitable range.

[0016] The carboxyl group can form a bonding force with the functional groups on the electrode and diaphragm materials to improve the bonding effect.

[0017] The acrylamide group is beneficial to the polymerization of the monomer. This type of monomer plays a role in regulating the molecular weight and also has good adhesion.

[0018] The carbonyl group and amide group are beneficial to improving the viscosity of the adhesive.

[0019] The nitrile group helps to increase ionic conductivity and improve adhesion.

[0020] Preferably, the shape of the binder includes a spherical shape.

[0021] The spherical shape facilitates uniform dispersion during the stirring of the slurry, which is conducive to uniform coating.

[0022] Preferably, the volume particle size distribution Dv50 of the binder is 1 μm to 15 μm, preferably 5 μm to 10 μm, and / or the number particle size distribution Dn10 of the binder is 1 μm to 5 μm, preferably 1 μm to 3 μm.

[0023] Theoretically, the volume average particle size Dv50 of the binder in this application can be lower than 1 μm or higher than 15 μm, but considering that the binder in this application is used on the diaphragm, the volume average particle size Dv50 of the binder cannot be too large or too small, so as to improve the pores of the diaphragm blocked by the binder, reduce the problem of lithium ions (here taking lithium ion secondary batteries as an example, of course, other types of secondary batteries can also be used) passing through the diaphragm, and improve the problem of the binder being coated on the diaphragm to form a thicker coating, affecting the energy density of the battery prepared later. Therefore, the volume particle size distribution Dv50 of the binder is 1 μm to 15 μm, preferably 5 μm to 10 μm.

[0024] The number particle size distribution Dn10 of the binder is within the above range, which can improve the problem of the binder blocking the pores of the diaphragm, reduce the problem of lithium ions (here taking lithium ion secondary batteries as an example, of course, other types of secondary batteries can also be used) passing through the diaphragm, and improve the problem of the binder coating the diaphragm to form a thicker coating, which affects the energy density of the battery prepared later. Therefore, the number particle size distribution Dn10 of the binder is 1 μm to 5 μm, preferably 1 μm to 3 μm.

[0025] Preferably, the organic polymer includes a first polymer and a second polymer, and the first polymer and the second polymer include an acrylic copolymer.

[0026] The organic polymer includes a first polymer and a second polymer. It can be understood that the organic polymer includes the first polymer and the second polymer, and the organic polymer includes a first glass transition temperature and a second glass transition temperature.

[0027] Acrylate copolymers have good adhesion. The use of acrylic copolymers can improve the adhesion between the diaphragm and the pole piece after cold pressing.

[0028] Preferably, the mass ratio of the first polymer to the second polymer is in the range of 1:(0.1-10), preferably 1:(0.5-3).

[0029] Setting the mass ratio of the first polymer to the second polymer in the above range can improve the problem that the binder is too soft and affects the performance of the battery core, for example, improving the problem that the binder may block the pores of the diaphragm when the binder is too soft, and improving the problem that the binder is too hard and affects the bonding effect. Therefore, the mass ratio of the first polymer to the second polymer ranges from 1: (0.1 to 10), preferably 1: (0.5 to 3).

[0030] Preferably, the first polymer and / or the second polymer comprises a first polymerized monomer, and the structure of the first polymerized monomer comprises:

[0031]

[0032] Among them, R1 includes a hydrogen atom or an alkyl group of 1 to 12 carbon atoms, and R2 includes an alkyl group of 1 to 12 carbon atoms.

[0033] The first polymerizable monomer includes an unsaturated ester group, which is beneficial to the polymerization of the monomer and can improve the anti-swelling ability of the polymer. Moreover, as a flexible monomer segment in the molecular segment, it can adjust the glass transition temperature of the organic polymer and help to adjust the glass transition temperature of the polymer within a suitable range.

[0034] Preferably, the first polymerizable monomer comprises one or more of methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-propyl acrylate, cyclohexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate.

[0035] By using any one or more of the above first polymerizable monomers, the glass transition temperature of the polymer can be adjusted and the anti-swelling ability of the polymer can be improved.

[0036] Preferably, the first polymer includes a second polymerized monomer, and the structure of the second polymerized monomer includes:

[0037]

[0038] Wherein, R3 includes a hydrogen atom, a substituted or unsubstituted alkyl group of 1 to 6 carbon atoms.

[0039] The second polymerizable monomer includes an unsaturated carboxyl group, which is beneficial to the polymerization of the monomer. The first polymer includes a second polymerizable monomer containing a carboxyl group, so that in the process of pressing the diaphragm and the electrode using a cold pressing process, the carboxyl group can form a bonding force with the functional groups on the electrode and the diaphragm material, thereby improving the bonding effect.

[0040] Preferably, the second polymerizable monomer comprises one or more of acrylic acid, methacrylic acid, butenoic acid, and heptenoic acid.

[0041] By using any one or more of the above-mentioned second polymerizable monomers, the adhesive properties of the first polymer can be adjusted.

[0042] Preferably, the first polymer and / or the second polymer comprises a third polymerized monomer, and the structure of the third polymerized monomer comprises:

[0043]

[0044] Among them, R4 includes a hydrogen atom or an alkyl group of 1 to 6 carbon atoms, and R5 includes a hydrogen atom, an alkyl group of 1 to 6 carbon atoms substituted with a hydroxyl group, or an alkoxy group of 1 to 6 carbon atoms.

[0045] The structure of the third polymerizable monomer includes an unsaturated amide group, which is beneficial to the polymerization of the monomer. This type of monomer plays a role in regulating the molecular weight and also has good adhesion.

[0046] Preferably, the third polymerizable monomer includes one or more of acrylamide, N-hydroxymethyl acrylamide and N-butoxymethyl acrylamide.

[0047] The use of any one or more third polymerizable monomers mentioned above can play a role in regulating the molecular weight, so as to adjust the molecular weight of the polymer. The molecular weight of the adhesive is helpful to improve the adhesiveness within a certain range.

[0048] Preferably, the second polymer includes a fourth polymerized monomer, and the structure of the fourth polymerized monomer includes:

[0049]

[0050] Here, R6 includes a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.

[0051] The structure of the fourth polymerizable monomer includes an unsaturated cyano group, which is beneficial to the polymerization of the monomer, helps to improve the ionic conductivity, and improves the adhesion.

[0052] Preferably, the fourth polymerizable monomer includes one or more of acrylonitrile and methacrylonitrile.

[0053] By using any one or more of the fourth polymerizable monomers mentioned above, the ionic conductivity of the binder can be improved.

[0054] The present application also provides a method for preparing a binder, comprising:

[0055] Mixing water, an emulsifier, an initiator, and monomers constituting the first polymer, stirring, and heating for reaction to obtain a first polymer emulsion;

[0056] Mixing water, an emulsifier, an initiator, and monomers constituting the second polymer, stirring, and heating for reaction to obtain a second polymer emulsion;

[0057] The first polymer emulsion and the second polymer emulsion are mixed and stirred, and then spray-dried to obtain a binder.

[0058] In the present application, the first polymer emulsion and the second polymer emulsion are obtained by emulsion polymerization, and the binder is obtained by spray drying.

[0059] Preferably, the step of mixing and stirring the first polymer emulsion and the second polymer emulsion and obtaining the binder by spray drying comprises:

[0060] The first polymer emulsion and the second polymer emulsion are mixed and stirred to obtain a mixed emulsion, wherein the mass ratio of the first polymer to the second polymer in the mixed emulsion is in the range of 1:(0.1-10), preferably 1:(0.5-3).

[0061] In order to obtain a second polymer and a second polymer having a suitable ratio in the binder to obtain a binder with suitable properties, the first polymer emulsion and the second polymer emulsion are mixed and stirred to obtain a mixed emulsion, and the mass ratio of the first polymer to the second polymer in the mixed emulsion is in the range of 1: (0.1~10), preferably 1: (0.5~3).

[0062] An embodiment of the present application provides a separator, which includes the above-mentioned binder for secondary batteries or a binder prepared by the above-mentioned method for preparing the binder for secondary batteries.

[0063] An embodiment of the present application provides a battery cell, wherein the battery cell includes the separator as described above.

[0064] An embodiment of the present application provides a battery, which includes the above-mentioned battery cell.

[0065] An embodiment of the present application provides an electrical device, which includes the above-mentioned battery cell or the above-mentioned battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0066] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0067] Figure 1 This is a scanning electron microscope image of the binder provided in Example 1 of the present application;

[0068] Figure 2 A schematic diagram of a process for preparing a binder provided in an embodiment of the present application;

[0069] Figure 3 is a schematic diagram of an electrode assembly provided in an embodiment of the present application;

[0070] Figure 4 yes Figure 3 An exploded view of an electrode assembly provided in an embodiment of the present application is shown;

[0071] Figure 5 is a schematic diagram of a battery module provided in an embodiment of the present application;

[0072] Figure 6 is a schematic diagram of a battery pack provided in an embodiment of the present application;

[0073] Figure 7 yes Figure 6 An exploded view of a battery pack provided in an embodiment of the present application is shown;

[0074] Figure 8 It is a schematic diagram of an electrical device provided in an embodiment of the present application.

[0075] Description of Figure Numbers:

[0076] Label name Label name 1 Battery Pack 5 Secondary battery 2 Upper box 51 case 3 Lower box 52 Electrode assembly 4 Battery Module 53 Top cover assembly

[0077] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0078] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0079] Hereinafter, the binder of the present application and its preparation method, as well as the embodiments of the diaphragm, electrode assembly, battery cell, battery and electrical device containing the binder are described in detail with appropriate reference to the drawings. However, there are cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0080] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0081] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0082] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0083] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0084] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0085] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0086] The battery cell has a problem of large openings, that is, a gap is easily formed between the electrode and the diaphragm, resulting in poor battery cycle performance.

[0087] The commonly used adhesive on the diaphragm is polyvinylidene fluoride, but the price of polyvinylidene fluoride has increased sharply at this stage, and the market supply is tight. At the same time, a hot pressing process is required to make the diaphragm and the electrode tightly bonded; but as the production speeds up, the hot pressing process will gradually be replaced by the cold pressing process. The cold pressing of the battery electrode refers to the shaping of the core to reduce the elasticity of the battery cell, improve the qualified rate of the core installation and the consistency of the thickness of the finished battery cell.

[0088] The bonding force between the positive electrode plate, the negative electrode plate and the separator is insufficient, and problems such as cell opening often occur. At the same time, the wettability to the electrolyte is poor, and the performance requirements of the coated separator cannot be met by the secondary battery. The separator and the electrode plate fit tightly, which can improve the discharge capacity of the battery, reduce internal resistance, reduce polarization loss, extend the cycle life of the battery, and improve the utilization rate of the secondary battery.

[0089] It is understandable that the battery cell is formed by bonding the positive electrode sheet, the negative electrode sheet and the separator. The battery cell has a certain hardness, that is, because the positive and negative electrode sheets and the separator bonded together are attached to each other and support each other, a structure with a certain thickness is formed, and a structure with a certain thickness has a certain hardness. The negative electrode will expand during the charging and discharging process. If the bonding force is weak, a gap will be formed between the positive and negative electrode sheets and the separator, and the positive and negative electrode sheets and the separator cannot be attached to each other and support each other, resulting in the battery cell being loose and the hardness being reduced. At this time, the power performance of the battery cell will deteriorate, for example, the rate performance will be reduced, and at the same time, the cycle performance will deteriorate. For example, in electric vehicles, the battery cell is loose, resulting in a slower battery charging speed, and at the same time, the battery cycle performance deteriorates, which directly leads to a shortened battery life. Electric vehicles need to frequently replace batteries, and consumers' costs on electric vehicles increase.

[0090] Based on this, the present application proposes a binder for a secondary battery, the binder includes an organic polymer, the organic polymer includes a first glass transition temperature and a second glass transition temperature, the first glass transition temperature is less than or equal to 25°C, and the second glass transition temperature is greater than 25°C.

[0091] Binder refers to a material with adhesive properties that is used to bond different substances together.

[0092] The glass transition temperature is the temperature at which a polymer changes from a highly elastic state to a glassy state. It refers to the transition temperature of an amorphous polymer (including the non-crystalline part of a crystalline polymer) from a glassy state to a highly elastic state or from the latter to the former. It is the lowest temperature at which the macromolecular segments of an amorphous polymer can move freely, and is usually represented by Tg. Above the glass transition temperature, the polymer exhibits elasticity; below the glass transition temperature, the polymer exhibits brittleness. The glass transition temperature can be measured by methods commonly used in the art, for example, it can be tested by differential scanning calorimetry with reference to GB / T19466.2.

[0093] It can be understood that the first glass transition temperature is less than or equal to 25°C, so that at a certain temperature, the organic polymer including the structure of the first glass transition temperature is in a rubber state, and the second glass transition temperature is greater than 25°C, so that at a certain temperature, the organic polymer including the structure of the second glass transition temperature is in a glassy state.

[0094] For example, the first glass transition temperature is lower than room temperature, and the second glass transition temperature is higher than room temperature. At room temperature, when no pressure is applied to the binder, the second glass transition temperature is higher than room temperature and is in a glassy state. The structure of the organic polymer including the second glass transition temperature is relatively hard and can serve as the skeleton structure of the binder powder, making the binder non-sticky. At room temperature, the first glass transition temperature is lower than room temperature and is in a rubbery state. It can have a certain "fluidity" after applying a certain pressure. The structure of the organic polymer including the first glass transition temperature can fully penetrate into the pores of the positive and negative pole pieces and the diaphragm, increasing the mechanical interlocking effect, and can give full play to its bonding performance, thereby helping to improve the battery's kinetic performance.

[0095] It can be understood that at a certain temperature, the structure of the organic polymer including the first glass transition temperature is in a soft state and can be deformed with the extrusion force, while the structure of the diaphragm and the electrode has pores. As the extrusion force acts on the organic polymer, part of the structure of the organic polymer can penetrate into the pores of the diaphragm and the electrode, bonding the diaphragm and the adhesive together, achieving a mechanical interlocking effect and realizing the bonding function.

[0096] Since there is a significant difference between the first glass transition temperature and the second glass transition temperature of the organic polymer, when cold pressed at a certain temperature, the structure of the organic polymer including the first glass transition temperature is in a rubber state, and the structure of the organic polymer including the second glass transition temperature is in a glass state, so that the binder has the characteristics of "both soft and hard". After it is coated on the diaphragm, the binder is non-sticky when there is no pressure at a certain temperature, which can meet the requirements of winding and unwinding the diaphragm. When a certain pressure is applied, the binder shows pressure sensitivity and better adhesion, which meets the bonding requirements of the diaphragm and the positive and negative pole pieces.

[0097] Therefore, when the adhesive of the present application is applied to the diaphragm, the adhesive is non-sticky at a certain temperature to facilitate the winding and unwinding of the diaphragm, but after being wound with the positive and negative pole pieces and undergoing a cold pressing process, the adhesive has better bonding strength, so that the positive and negative pole pieces and the diaphragm fit closely to each other. Therefore, the adhesive of the present application improves the cold pressing bonding strength between the diaphragm and the positive and negative pole pieces, thereby improving the hardness of the battery cell and the cycle performance of the secondary battery.

[0098] It can be understood that the first glass transition temperature can be any value such as -100℃, -90℃, -80℃, -70℃, -50℃, -30℃, -10℃, 10℃, 20℃, 24℃, 25℃, and the range value between any two of the above point values, without specific limitation.

[0099] It is understandable that the second glass transition temperature can be any value such as 26°C, 30°C, 50°C, 80°C, 100°C, 200°C, and the range value between any two of the above point values, without specific limitation.

[0100] In one embodiment, the first glass transition temperature ranges from -80°C to 25°C, preferably from -60°C to 25°C.

[0101] Within the above range, the organic polymer including the structure of the first glass transition temperature is in a rubbery state at a certain temperature, which is conducive to exerting its adhesion during the cold pressing process, and is conducive to the adhesion between the diaphragm and the electrode after cold pressing, thereby improving the performance of the battery.

[0102] In the above-mentioned -80℃ to 25℃, the values ​​include the minimum and maximum values ​​of the range, and every value between such minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and -80℃, -70℃, -60℃, -50℃, -40℃, -30℃, -20℃, -10℃, 0℃, 10℃, 20℃, 25℃, etc., as well as the range values ​​between any two of the above-mentioned point values.

[0103] In the above-mentioned -60℃ to 25℃, the values ​​include the minimum and maximum values ​​of the range, and every value between such minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and -60℃, -50℃, -40℃, -30℃, -20℃, -10℃, 0℃, 10℃, 20℃, 25℃, etc., as well as the range values ​​between any two of the above-mentioned point values.

[0104] In one embodiment, the second glass transition temperature ranges from 26°C to 100°C, preferably from 26°C to 90°C.

[0105] Within the above range, the organic polymer includes a structure with a second glass transition temperature that is in a glassy state at a certain temperature, which is beneficial as a skeleton structure of the adhesive at a certain temperature, making the adhesive non-sticky and facilitating the winding and unwinding steps of the diaphragm at a certain temperature.

[0106] In the above-mentioned 26°C to 100°C, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 26°C, 28°C, 30°C, 50°C, 80°C, 90°C, 100°C, etc., as well as the range values ​​between any two of the above-mentioned point values.

[0107] In the above-mentioned 26°C to 90°C, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 26°C, 28°C, 30°C, 50°C, 80°C, 90°C, etc., as well as the range values ​​between any two of the above-mentioned point values.

[0108] In one embodiment, the organic polymer includes an acrylic ester copolymer, and / or the organic polymer includes at least one of an ester group, a carboxyl group, an acrylamide group, a carbonyl group, an amide group, and a nitrile group.

[0109] Copolymer, a polymerization reaction in which two or more monomers participate together, is called copolymerization. The polymer formed contains two or more monomer units. This type of polymer is called a copolymer or an interpolymer.

[0110] Acrylate copolymers, acrylic copolymers are a general term for polymers produced by copolymerization of acrylic monomers and other comonomers.

[0111] The acrylic acid ester monomer has an acrylic acid ester group in its structure, for example, methyl acrylate, ethyl acrylate, and n-butyl acrylate.

[0112] Acrylate copolymers have good adhesion. The use of acrylic copolymers can improve the adhesion between the diaphragm and the pole piece after cold pressing.

[0113] Test of ester, carboxyl, acrylamide, carbonyl, amide and nitrile groups in organic polymer structures: Test according to the national standard GB / T 6040-2002 General Rules for Infrared Spectroscopy Analysis Methods. Use the tablet transmission method to press the sample into KBr tablets, and deduct the KBr background blank by the transmission method to obtain the sample test spectrum (resolution: 4cm -1 , wave number range: 400cm -1 ~4000cm -1 ).

[0114] The ester group can improve the anti-swelling ability of the polymer, and as a flexible monomer segment in the molecular chain segment, it can adjust the glass transition temperature of the organic polymer, which helps to adjust the glass transition temperature of the polymer within a suitable range.

[0115] The carboxyl group can form a bonding force with the functional groups on the electrode and diaphragm materials to improve the bonding effect.

[0116] The acrylamide group is beneficial to the polymerization of the monomer. This type of monomer plays a role in regulating the molecular weight and also has good adhesion.

[0117] The carbonyl group and amide group are beneficial to improving the viscosity of the adhesive.

[0118] The nitrile group helps to increase ionic conductivity and improve adhesion.

[0119] In one embodiment, the shape of the binder includes a spherical shape.

[0120] The spherical shape facilitates uniform dispersion during the stirring of the slurry, which is conducive to uniform coating.

[0121] In one embodiment, the volume particle size distribution Dv50 of the binder is 1 μm to 15 μm, preferably 5 μm to 10 μm, and / or the number particle size distribution Dn10 of the binder is 1 μm to 5 μm, preferably 1 μm to 3 μm.

[0122] Dv50: Among the sample particles, 50% of the total volume of the particles have a particle size larger than this value, and another 50% of the total volume of the particles have a particle size smaller than this value; Dv50 can represent the median particle size of the sample.

[0123] Dn10, the particle size of 10% of the total number of particles in the sample particles is smaller than this value. The volume particle size distribution Dv50 and number particle size distribution Dn10 of the binder can be tested by methods known in the art. As an example, GB / T 19077-2016 can be referred to, and a Malvern laser particle size analyzer can be used for characterization testing, such as the Mastersizer-3000 of Malvern.

[0124] Theoretically, the volume average particle size Dv50 of the binder in this application can be lower than 1 μm or higher than 15 μm, but considering that the binder in this application is used on the diaphragm, the volume average particle size Dv50 of the binder cannot be too large or too small, so as to improve the pores of the diaphragm blocked by the binder, reduce the problem of lithium ions (here taking lithium ion secondary batteries as an example, of course, other types of secondary batteries can also be used) passing through the diaphragm, and improve the problem of the binder being coated on the diaphragm to form a thicker coating, affecting the energy density of the battery prepared later. Therefore, the volume particle size distribution Dv50 of the binder is 1 μm to 15 μm, preferably 5 μm to 10 μm.

[0125] The number particle size distribution Dn10 of the binder is within the above range, which can improve the problem of the binder blocking the pores of the diaphragm, reduce the problem of lithium ions (here taking lithium ion secondary batteries as an example, of course, other types of secondary batteries can also be used) passing through the diaphragm, and improve the problem of the binder coating the diaphragm to form a thicker coating, which affects the energy density of the battery prepared later. Therefore, the number particle size distribution Dn10 of the binder is 1 μm to 5 μm, preferably 1 μm to 3 μm.

[0126] In the above-mentioned 1μm to 15μm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, etc., and the range values ​​between any two of the above-mentioned point values.

[0127] In the above-mentioned 5μm to 10μm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, etc., and the range values ​​between any two of the above-mentioned point values.

[0128] In the above-mentioned 1μm to 5μm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1μm, 2μm, 3μm, 4μm, 5μm, etc., as well as the range values ​​between any two of the above-mentioned point values.

[0129] In the above-mentioned 1μm to 3μm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1μm, 1.5μm, 2μm, 2.5μm, 3μm, etc., and the range values ​​between any two of the above-mentioned point values.

[0130] In one embodiment, the organic polymer includes a first polymer and a second polymer, and the first polymer and the second polymer include an acrylic copolymer.

[0131] The organic polymer includes a first polymer and a second polymer. It can be understood that the organic polymer includes the first polymer and the second polymer, and the organic polymer includes a first glass transition temperature and a second glass transition temperature.

[0132] Acrylate copolymers have good adhesion. The use of acrylic copolymers can improve the adhesion between the diaphragm and the pole piece after cold pressing.

[0133] In one embodiment, the mass ratio of the first polymer to the second polymer is in the range of 1:(0.1-10), preferably 1:(0.5-3).

[0134] The binder is a secondary particle formed by the aggregation of primary particles of a first polymer and primary particles of a second polymer. Both the primary particles of the first polymer and the primary particles of the second polymer have the opportunity to be exposed on the surface of the secondary particles. By adjusting the mass ratio of the first polymer and the second polymer, the opportunity of the first polymer to be exposed on the surface of the secondary particles is adjusted to adjust the adhesion of the binder.

[0135] Setting the mass ratio of the first polymer to the second polymer in the above range can improve the problem that the binder is too soft and affects the performance of the battery core, for example, improving the problem that the binder may block the pores of the diaphragm when the binder is too soft, and improving the problem that the binder is too hard and affects the bonding effect. Therefore, the mass ratio of the first polymer to the second polymer ranges from 1: (0.1 to 10), preferably 1: (0.5 to 3).

[0136] In the above 1: (0.1~10), the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1: 0.1, 1: 1, 1: 2, 1: 3, 1: 4, 1: 5, 1: 6, 1: 7, 1: 8, 1: 9, 1: 10, etc., as well as the range values ​​between any two of the above point values.

[0137] In the above 1:(0.5~3), the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1:0.5, 1:1.5, 1:2, 1:2.5, 1:3, etc., as well as the range values ​​between any two of the above point values.

[0138] It is understandable that if Figure 1 As shown, the binder particles are secondary particles formed by agglomerating primary particles of a first polymer and primary particles of a second polymer. In this way, the second polymer serves as a skeleton. When the binder is not squeezed, the binder has no adhesiveness. After being squeezed, the first polymer can be deformed by force and penetrate into the pores of the diaphragm and the electrode to achieve a bonding effect.

[0139] It can be understood that the primary particle size of the polymer latex of the first polymer and the second polymer is about 100nm to 150nm. After the two latexes are mixed and spray-dried, the particles are 1μm to 15μm. The primary particles of the two polymers are mixed together to form secondary particle balls after spray drying.

[0140] In one embodiment, the first polymer and / or the second polymer includes a first polymerized monomer; the first polymer and / or the second polymer includes a first polymerized monomer;

[0141] The structure of the first polymerizable monomer includes: Among them, R1 includes a hydrogen atom or an alkyl group of 1 to 12 carbon atoms, and R2 includes an alkyl group of 1 to 12 carbon atoms.

[0142] The first polymerizable monomer includes an unsaturated ester group, which is beneficial to the polymerization of the monomer and can improve the anti-swelling ability of the polymer. Moreover, as a flexible monomer segment in the molecular segment, it can adjust the glass transition temperature of the organic polymer and help to adjust the glass transition temperature of the polymer within a suitable range.

[0143] In one embodiment, the first polymerizable monomer includes one or more of methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-propyl acrylate, cyclohexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate.

[0144] By using any one or more of the above first polymerizable monomers, the glass transition temperature of the polymer can be adjusted and the anti-swelling ability of the polymer can be improved.

[0145] In one embodiment, the first polymer includes a second polymerized monomer, and the structure of the second polymerized monomer includes: Wherein, R3 includes a hydrogen atom, a substituted or unsubstituted alkyl group of 1 to 6 carbon atoms.

[0146] The second polymerizable monomer includes an unsaturated carboxyl group, which is beneficial to the polymerization of the monomer. The first polymer includes a second polymerizable monomer containing a carboxyl group, so that in the process of pressing the diaphragm and the electrode using a cold pressing process, the carboxyl group can form a bonding force with the functional groups on the electrode and the diaphragm material, thereby improving the bonding effect.

[0147] In one embodiment, the second polymerizable monomer includes one or more of acrylic acid, methacrylic acid, butenoic acid, and heptenoic acid.

[0148] By using any one or more of the above-mentioned second polymerizable monomers, the adhesive properties of the first polymer can be adjusted.

[0149] In one embodiment, the first polymer and / or the second polymer includes a third polymerized monomer, and the structure of the third polymerized monomer includes: Among them, R4 includes a hydrogen atom or an alkyl group of 1 to 6 carbon atoms, and R5 includes a hydrogen atom, an alkyl group of 1 to 6 carbon atoms substituted with a hydroxyl group, or an alkoxy group of 1 to 6 carbon atoms.

[0150] The structure of the third polymerizable monomer includes an unsaturated amide group, which is beneficial to the polymerization of the monomer. This type of monomer plays a role in regulating the molecular weight and also has good adhesion.

[0151] In one embodiment, the third polymerizable monomer includes one or more of acrylamide, N-methylol acrylamide and N-butoxymethyl acrylamide.

[0152] The use of any one or more third polymerizable monomers mentioned above can play a role in regulating the molecular weight, so as to adjust the molecular weight of the polymer. The molecular weight of the adhesive is helpful to improve the adhesiveness within a certain range.

[0153] In one embodiment, the second polymer includes a fourth polymerized monomer, and the structure of the fourth polymerized monomer includes: Here, R6 includes a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.

[0154] The structure of the fourth polymerizable monomer includes an unsaturated cyano group, which is beneficial to the polymerization of the monomer, helps to improve the ionic conductivity, and improves the adhesion.

[0155] In one embodiment, the fourth polymerizable monomer includes one or more of acrylonitrile and methacrylonitrile.

[0156] By using any one or more of the fourth polymerizable monomers mentioned above, the ionic conductivity of the binder can be improved.

[0157] Commonly used polyvinylidene fluoride adhesives need to be hot pressed to better exert their bonding effect. With the acceleration of production and the saving of production capacity, the hot pressing process will gradually be replaced by the cold pressing process. After the battery cell is wound, it will undergo a cold pressing process. Since conventional polyvinylidene fluoride is a homopolymer with a crystallinity of about 50%, the adhesion between the diaphragm and the positive and negative pole pieces is insufficient; the adhesion of traditional polyacrylate adhesives under cold pressing does not meet the requirements, and problems such as cell opening and soft cells often occur; at the same time, the wettability to the electrolyte is poor, and it cannot meet the performance requirements of the secondary battery for the coated diaphragm.

[0158] The above-mentioned monomers are used to prepare acrylic copolymers, so that the binder has good adhesion. It is understandable that the binder includes a first polymer and a second polymer. The first polymer is prepared by emulsion polymerization of at least two of the first polymerized monomer, the second polymerized monomer and the third polymerized monomer. It is understandable that when the first polymer is composed of the above three monomers, its performance is better; the second polymer emulsion is prepared by emulsion polymerization of at least two of the first polymerized monomer, the third polymerized monomer and the fourth polymerized monomer. It is understandable that when the second polymer is composed of the above three monomers, its performance is better. The first polymer and the second polymer prepared by the above-mentioned monomers have a suitable glass transition temperature. When coated on the diaphragm, it can not only meet the requirements of the binder being non-adhesive at room temperature, but also meet the requirements of the cold pressing adhesion between the diaphragm and the positive and negative pole pieces during the cold pressing process, thereby improving the hardness of the battery cell and improving the problems of battery cell opening and soft battery cell; at the same time, the binder is coated on the diaphragm and applied to the secondary battery, which can improve the cycle performance of the secondary battery.

[0159] The present application also provides a method for preparing a binder for secondary batteries, comprising: blending and stirring water, an emulsifier, an initiator, and monomers constituting a first polymer, heating and reacting to obtain a first polymer emulsion; blending and stirring water, an emulsifier, an initiator, and monomers constituting a second polymer, heating and reacting to obtain a second polymer emulsion; mixing and stirring the first polymer emulsion and the second polymer emulsion, and spray-drying to obtain a binder.

[0160] The present application obtains the first polymer emulsion and the second polymer emulsion by emulsion polymerization, and obtains the binder by spray drying. That is, the organic polymer includes the first polymer and the second polymer.

[0161] Emulsion polymerization is a process in which monomers are dispersed in water with the help of emulsifiers and mechanical stirring to form an emulsion, and then an initiator is added to initiate the polymerization of the monomers.

[0162] Emulsifiers are substances that can transform incompatible oil and water into an emulsion that is difficult to separate. Emulsifiers are usually surfactants that have both hydrophilic polar groups and hydrophobic (lipophilic) non-polar groups.

[0163] Initiator: An initiator is a substance that can initiate polymerization of monomers. For example, free radical initiators refer to a class of compounds that are easily decomposed into free radicals (i.e., primary free radicals) by heat, and can be used to initiate free radical polymerization and copolymerization of olefin and diene monomers.

[0164] Water, emulsifier, initiator, and monomers constituting the polymer are mixed and stirred. Water and emulsifier are stirred and dispersed to form an emulsion, that is, the emulsifier forms micelles in the aqueous phase, and monomers are solubilized in most of the micelles. Under heating conditions, the initiator initiates polymerization of the monomers inside the micelles to obtain an emulsion.

[0165] Spray drying, through mechanical action, disperses the material to be dried (a mixture of the first polymer emulsion and the second polymer emulsion) into very fine mist-like particles (increasing the water evaporation area and accelerating the drying process), which are then brought into contact with hot air to remove most of the water in an instant, drying the solid matter in the material into powder.

[0166] A binder composed of the first polymer and the second polymer is obtained through a spray drying process.

[0167] In one embodiment, the step of mixing and stirring the first polymer emulsion and the second polymer emulsion and obtaining the binder by spray drying includes: mixing and stirring the first polymer emulsion and the second polymer emulsion to obtain a mixed emulsion, wherein the mass ratio of the first polymer to the second polymer in the mixed emulsion is in the range of 1:(0.1-10), preferably 1:(0.5-3).

[0168] In order to obtain a second polymer and a second polymer with a suitable ratio in the binder to obtain a binder with suitable properties, the first polymer emulsion and the second polymer emulsion are mixed and stirred to obtain a mixed emulsion, and the mass ratio of the first polymer to the second polymer in the mixed emulsion is in the range of 1: (0.1~10), preferably 1: (0.5~3).

[0169] The embodiment of the present application also provides a diaphragm, which includes the above-mentioned binder or the binder prepared by the above-mentioned method for preparing the binder for secondary batteries. Since the binder adopts all the technical solutions of all the above-mentioned embodiments, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be repeated here one by one.

[0170] The diaphragm is coated with the above-mentioned adhesive, which can improve the bonding performance between the pole piece and the adhesive and improve the opening problem of the existing battery cell pre-cooling pressing process.

[0171] The embodiment of the present application also provides a battery cell, which includes the above-mentioned diaphragm. Since the diaphragm adopts all the technical solutions of all the above-mentioned embodiments, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be described one by one here.

[0172] Applying the above-mentioned separator to a battery cell can improve the large-clamp cycle performance of the battery cell.

[0173] The embodiment of the present application further provides a battery, the battery comprising the above-mentioned battery cell. Since the battery cell adopts all the technical solutions of all the above-mentioned embodiments, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be described one by one here.

[0174] Batteries include battery modules and battery packs.

[0175] The embodiment of the present application also provides an electric device, which includes the above-mentioned battery cell or the above-mentioned battery. Since the battery cell or the battery adopts all the technical solutions of all the above-mentioned embodiments, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be repeated here one by one.

[0176] In addition, the electrode assembly, battery cell, battery, and electric device of the present application will be described below with reference to the drawings as appropriate.

[0177] In one embodiment of the present application, an electrode assembly is provided.

[0178] Typically, the electrode assembly includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. During the battery charging and discharging process, active ions are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, and at the same time allow ions to pass through. The separator is the separator improved above in this application.

[0179] The positive electrode plate includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector.

[0180] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.

[0181] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0182] In some embodiments, when the electrode assembly is a lithium-ion battery, the positive electrode active material may adopt a positive electrode active material for lithium-ion batteries that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: a lithium-containing phosphate with an olivine structure, a lithium transition metal oxide, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3Mn 1 / 3 O2 (also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds, etc. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0183] In some embodiments, the positive electrode film layer may also optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.

[0184] In some embodiments, the positive electrode film layer may further include a conductive agent, for example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0185] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0186] The negative electrode plate includes a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector, and the negative electrode film layer includes a negative electrode active material.

[0187] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0188] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0189] In some embodiments, the negative electrode active material may adopt the negative electrode active material for the battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may include at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may include at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0190] In some embodiments, the negative electrode film layer may further include a binder. The binder may include at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).

[0191] In some embodiments, the negative electrode film layer may further include a conductive agent, which may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0192] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0193] In some embodiments, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0194] The electrolyte plays a role in conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs.

[0195] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.

[0196] In some embodiments, the electrolyte salt may include at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethanesulfonyl imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0197] In some embodiments, the solvent may include at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0198] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.

[0199] In some embodiments, the electrode assembly further includes a diaphragm. The present application has no particular limitation on the type of diaphragm, and any known porous diaphragm with good chemical stability and mechanical stability can be selected.

[0200] In some embodiments, the material of the diaphragm may include at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The diaphragm may be a single-layer film or a multi-layer composite film, without particular limitation. When the diaphragm is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.

[0201] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.

[0202] In some embodiments, the electrode assembly may include an outer packaging, which may be used to package the electrode assembly and the electrolyte.

[0203] In some embodiments, the outer packaging of the electrode assembly may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the electrode assembly may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0204] The present application has no particular limitation on the shape of the electrode assembly, which may be cylindrical, square, or any other shape. Figure 3 The secondary battery 5 is a square structure as an example.

[0205] In some embodiments, reference Figure 4 , the outer package may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the diaphragm can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0206] In some embodiments, the electrode assemblies may be assembled into a battery module. The number of electrode assemblies contained in the battery module may be one or more. The specific number may be selected by those skilled in the art according to the application and capacity of the battery module.

[0207] Figure 5 4 is an example of a battery module. Figure 5 In the battery module 4, the plurality of secondary batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 5 may be fixed by fasteners.

[0208] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0209] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery pack.

[0210] Figure 6 and Figure 7 1 is a battery pack 1 as an example. Figure 6 and Figure 7 The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.

[0211] In addition, the present application also provides an electrical device, which includes at least one of the electrode assembly, battery module, or battery pack provided in the present application. The electrode assembly, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0212] As an electrical device, an electrode assembly, a battery module or a battery pack can be selected according to its usage requirements.

[0213] Figure 8 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the electrode assembly, a battery pack or a battery module can be used.

[0214] As another example, the device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be light and thin, and an electrode assembly may be used as a power source.

[0215] Example

[0216] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0217] Preparation of the first polymer emulsion

[0218] Preparation Example A1

[0219] According to the mass ratio of the three monomers of 90:5:5, weigh the first polymerized monomer methyl acrylate, the second polymerized monomer acrylic acid and the third polymerized monomer acrylamide respectively, and mix the monomers evenly. Add 1000g of mixed monomers, 30g of sodium dodecyl sulfate emulsifier, 10g of ammonium persulfate initiator, and 1200g of deionized water to a 5000mL four-necked flask equipped with a mechanical stirrer, a thermometer and a condenser, and emulsify at high speed for 30min. Under nitrogen protection, heat to 75℃ for 4h, cool to below 40℃, adjust pH to neutral, and filter out the material. Obtain the first polymer emulsion A1.

[0220] Preparation Examples A2 to A14: Preparation Examples A2 to A14, based on Preparation Example A1, the monomer types and mass ratios were adjusted to obtain first polymer emulsions A2 to A14.

[0221] Preparation of the second polymer emulsion

[0222] Preparation Example B1

[0223] According to the mass ratio of the three monomers of 80:10:10, weigh the first polymerized monomer methyl acrylate, the second polymerized monomer acrylamide and the third polymerized monomer acrylonitrile respectively, and mix the monomers evenly. Add 200g of mixed monomers, 6g of sodium dodecyl sulfate emulsifier, 2g of ammonium persulfate initiator, and 300g of deionized water to a 1000mL four-necked flask equipped with a mechanical stirrer, a thermometer and a condenser, and emulsify at high speed for 30min. Under nitrogen protection, heat to 75℃ for reaction for 4h, cool to below 40℃, adjust the pH to neutral, and filter the material. Obtain the second polymer emulsion B1.

[0224] Preparation Example B2 to Preparation Example B14, Preparation Examples B2 to B14, based on Preparation Example B1, the monomer types and mass ratios were adjusted to obtain the second polymer emulsions B2 to B14.

[0225] Example 1

[0226] Preparation of binder

[0227] The first polymer emulsion A1 and the second polymer emulsion B2 were weighed according to a weight percentage of 1:1 between the first polymer and the second polymer, stirred and mixed evenly, and then subjected to a spray drying process to obtain a diaphragm adhesive. The conditions of the spray drying process were an inlet air temperature of 110°C, an outlet air temperature of 50°C, and an air pressure of 0.5 kPa.

[0228] In Examples 2 to 23, based on Example 1, the types, mass ratio and Dv50 of the first polymer emulsion and the second polymer emulsion are adjusted to obtain Examples 2 to 23.

[0229] Comparative Example 1 and Comparative Example 2

[0230] On the basis of Example 1, the types of the first polymer emulsion and the second polymer emulsion were adjusted to obtain Comparative Examples 1 and 2.

[0231] Comparative Example 3, on the basis of Example 1, only the second polymer emulsion was weighed, and under the same conditions, a separator binder comparative example 3 was prepared by a spray drying process.

[0232] Comparative Example 4, on the basis of Example 1, only the first polymer emulsion was weighed, and under the same conditions, a separator binder comparative example 4 was prepared by a spray drying process.

[0233] Preparation of diaphragm

[0234] A commercially available PE microporous film with a thickness of 7 μm and an average pore size of 80 nm (from Zhuogao Electronic Technology Co., Ltd.) was used as the substrate. The membrane binder prepared as described above was stirred and mixed evenly in deionized water to obtain a slurry (solid content of 20%). The slurry was sprayed on both surfaces of the substrate and dried to remove the solvent. The coating density of the coating composition on the substrate was 1.5 g / m 2 , and obtain the diaphragm.

[0235] Preparation of positive electrode

[0236] Polyvinylidene fluoride (PVDF), lithium iron phosphate (LFP), conductive agent carbon black, and N-methylpyrrolidone (NMP) were mixed in a mass ratio of 1.2:58.38:0.42:40, and then stirred and mixed to prepare a positive electrode slurry. 2The loading amount is evenly coated on the positive electrode current collector aluminum foil, and then dried, cold pressed and cut to obtain the positive electrode sheet.

[0237] Preparation of negative electrode

[0238] Artificial graphite, conductive agent acetylene black, binder styrene butadiene rubber (SBR), thickener sodium carboxymethyl cellulose (CMC-Na) were added into deionized water in a mass ratio of 96.2:1.0:1.6:1.2, and stirred and mixed thoroughly to prepare negative electrode slurry (solid content 63%). 2 The loading amount is coated on the negative electrode collector copper foil, and then dried, cold pressed and cut to obtain the negative electrode sheet.

[0239] Preparation of electrolyte

[0240] At 25°C, ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain a mixed solvent, and then LiPF6 is dissolved in the mixed solvent to obtain an electrolyte, in which the concentration of LiPF6 is 1 mol / L.

[0241] Preparation of secondary batteries

[0242] The positive electrode sheets, separators and negative electrode sheets are stacked and wound in order, and cold-pressed (during which the separators and the electrode sheets are bonded) to obtain a battery cell; the battery cell is placed in an outer package, and the prepared electrolyte is added, and after packaging, standing, formation, aging and other processes, a secondary battery is obtained.

[0243] Performance Testing

[0244] (1) Glass transition temperature test

[0245] Weigh 6±0.05 mg of sample into an Al crucible, shake it flat and cover it with a lid, and use the measuring instrument Netzsch DSC3500Sirius for testing; nitrogen atmosphere, purge gas rate is 50 mL / min, and protective gas rate is 100 mL / min; heating conditions: heating rate is 10℃ / min, and the temperature range is -70~200℃.

[0246] (2) Particle size test

[0247] Use a laser particle size analyzer (Malvern 3000, MasterSizer3000) for testing, and use a helium-neon red light source as the main light source. Take a clean small beaker and add 1g of the sample to be tested, add a drop of surfactant, add 20ml of deionized water, and ultrasonicate at 53KHz / 120W for 5min to ensure that the sample is completely dispersed. Turn on the laser particle size analyzer, clean the optical path system, and automatically test the background. Stir the ultrasonicated solution to be tested to make it evenly dispersed, put it into the sample pool as required, and start measuring the particle size. The measurement results can be read from the instrument.

[0248] (3) Cold press bonding test steps

[0249] The negative electrode of the battery is overlapped with the separator, and placed on a hot press. The parameters of the hot press are set as follows: temperature of 25°C, pressure of 7t, time of 15s, and pressing to obtain a bonded separator / negative electrode sample; the separator / electrode sample is cut into a rectangular strip of 150mm×20mm. The electrode side of the rectangular strip is pasted on the steel plate with double-sided tape, and the separator and the electrode are separated by 2cm in the length direction at one end of the rectangular strip to obtain a test sample.

[0250] The steel plate was kept horizontal and fixed with the lower clamp of the universal testing machine (Xieqiang Instrument Manufacturing (Shanghai) Co., Ltd., Model CTM2100). The peeled end of the diaphragm as described above was fixed with the upper clamp of the universal testing machine and connected to the tensile machine. The test conditions were set to a tensile rate of 20 mm / min and a horizontal pull of 10 cm. After the tension stabilized, the tension value was recorded, and the adhesion between the diaphragm and the electrode was obtained by the ratio of the tension value to the sample width.

[0251] (4) Battery cell hardness test steps

[0252] Place the battery cell on a table with both ends horizontal, fix the hollow part in the middle to be 12cm wide, let the battery cell lie flat naturally, and measure the deviation of the center of the battery cell from the horizontal reference line to evaluate the hardness of the battery cell. The greater the deviation of the center of the battery cell from the horizontal reference line, the poorer the hardness of the battery cell.

[0253] (5) Battery cycle performance test steps

[0254] At 25°C, the prepared battery was charged to 3.65V at 1 / 3C constant current, then charged to 0.05C at 3.65V constant voltage, left for 5 minutes, and then discharged to 2.5V at 1 / 3C. The obtained discharge capacity was recorded as the initial capacity C0. The above steps were repeated for the same battery, and the discharge capacity Cn of the battery after the nth cycle was recorded at the same time. The battery capacity retention rate after each cycle Pn = (Cn / C0) × 100%. The battery capacity retention rate at 500 cycles can be used to reflect the difference in cycle performance.

[0255] Table 1 Preparation parameters of the first polymer emulsion

[0256]

[0257] Table 2 Preparation parameters of the second polymer emulsion

[0258]

[0259]

[0260] Table 3 Preparation parameters of the diaphragm binder

[0261]

[0262] Table 4 Performance test parameters

[0263]

[0264] The first polymer and the second polymer are prepared by suitable monomers, the glass transition temperatures of the first polymer and the second polymer are regulated within a suitable range, and a binder is obtained by a spray drying process. The obtained binder has good bonding properties within a suitable range and is applied to a diaphragm, which is beneficial to improving the performance of the battery.

[0265] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the contents of the present invention's specification and drawings, or directly / indirectly applied in other related technical fields, are included in the patent protection scope of the present invention.

Claims

1. A binder for a secondary battery, characterized in that: The binder includes an organic polymer, and the organic polymer includes a first glass transition temperature and a second glass transition temperature, wherein the first glass transition temperature is less than or equal to 25°C, and the second glass transition temperature is greater than 25°C.

2. The binder for secondary batteries according to claim 1, wherein The first glass transition temperature ranges from -80°C to 25°C, preferably from -60°C to 25°C.

3. The binder for secondary batteries according to claim 1 or 2, characterized in that: The second glass transition temperature ranges from 26°C to 100°C, preferably from 26°C to 90°C.

4. The binder for secondary batteries according to any one of claims 1 to 3, characterized in that The organic polymer includes an acrylic ester copolymer, and / or the organic polymer includes at least one of an ester group, a carboxyl group, an acrylamide group, a carbonyl group, an amide group, and a nitrile group.

5. The secondary battery binder according to any one of claims 1 to 4, characterized in that The shape of the binder includes a spherical shape.

6. The binder for secondary batteries according to any one of claims 1 to 5, characterized in that The binder has a volume particle size distribution Dv50 of 1 μm to 15 μm, preferably 5 μm to 10 μm, and / or a number particle size distribution Dn10 of 1 μm to 5 μm, preferably 1 μm to 3 μm.

7. The binder for secondary batteries according to any one of claims 1 to 6, characterized in that The organic polymer includes a first polymer and a second polymer, and the first polymer and the second polymer include an acrylic copolymer.

8. The binder for secondary batteries according to claim 7, characterized in that The mass ratio of the first polymer to the second polymer is in the range of 1:(0.1-10), preferably 1:(0.5-3).

9. The binder for secondary batteries according to claim 7 or 8, characterized in that: The first polymer and / or the second polymer includes a first polymerized monomer, and the structure of the first polymerized monomer includes: Among them, R1 includes a hydrogen atom or an alkyl group of 1 to 12 carbon atoms, and R2 includes an alkyl group of 1 to 12 carbon atoms.

10. The binder for secondary batteries according to claim 9, characterized in that The first polymerizable monomer includes one or more of methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-propyl acrylate, cyclohexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate.

11. The binder for secondary batteries according to any one of claims 7 to 10, characterized in that The first polymer includes a second polymerized monomer, and the structure of the second polymerized monomer includes: Wherein, R3 includes a hydrogen atom, a substituted or unsubstituted alkyl group of 1 to 6 carbon atoms.

12. The binder for secondary batteries according to claim 11, wherein The second polymerizable monomer includes one or more of acrylic acid, methacrylic acid, butenoic acid, and heptenoic acid.

13. The binder for secondary batteries according to any one of claims 7 to 12, characterized in that: The first polymer and / or the second polymer includes a third polymerized monomer, and the structure of the third polymerized monomer includes: Among them, R4 includes a hydrogen atom or an alkyl group of 1 to 6 carbon atoms, and R5 includes a hydrogen atom, an alkyl group of 1 to 6 carbon atoms substituted with a hydroxyl group, or an alkoxy group of 1 to 6 carbon atoms.

14. The binder for secondary batteries according to claim 13, characterized in that The third polymerizable monomer includes one or more of acrylamide, N-hydroxymethyl acrylamide and N-butoxymethyl acrylamide.

15. The binder for secondary batteries according to any one of claims 7 to 14, characterized in that The second polymer includes a fourth polymerized monomer, and the structure of the fourth polymerized monomer includes: Here, R6 includes a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.

16. The binder for secondary batteries according to claim 15, characterized in that: The fourth polymerizable monomer includes one or more of acrylonitrile and methacrylonitrile.

17. The method for preparing a secondary battery binder according to any one of claims 1 to 16, characterized in that: include: Mixing water, an emulsifier, an initiator, and monomers constituting the first polymer, stirring, and heating for reaction to obtain a first polymer emulsion; Mixing water, an emulsifier, an initiator, and monomers constituting the second polymer, stirring, and heating for reaction to obtain a second polymer emulsion; The first polymer emulsion and the second polymer emulsion are mixed and stirred, and then spray-dried to obtain a binder.

18. A diaphragm, characterized in that: The separator includes the binder for a secondary battery according to any one of claims 1 to 16 or a binder prepared by the method for preparing a binder for a secondary battery according to claim 17 .

19. A battery cell, characterized in that: The battery cell includes the separator according to claim 18 .

20. A battery, characterized in that: The battery comprises the battery cell as claimed in claim 19.

21. An electrical device, characterized in that: The electrical device comprises the battery cell according to claim 19 or the battery according to claim 20.

Citation Information

Patent Citations

  • Porous membrane for secondary battery, and secondary battery

    CN102630353A

  • Adhesive resin composition for secondary battery

    CN103828115A

  • Separator for secondary cell

    CN104221184A

  • Separator for lithium secondary battery and lithium secondary battery comprising same

    CN111712943A

  • Diaphragm slurry, preparation method and application thereof

    CN112259913A

Cited By

  • Binder for secondary battery, preparation method therefor, separator, battery cell, battery and electrical apparatus

    EP4467623A1

  • Secondary battery cell and electric device

    WO2026148980A1