Foaming agent for shield, preparation method and application

By using a three-arm anionic sulfonate surfactant as a foaming agent, the foam agent produced solves the problem of existing foam agents being unfriendly to the environment and achieves efficient foaming power and stability without adding foam stabilizers. Agent and thickener, suitable for earth pressure balance shield tunneling construction.

CN118772890APending Publication Date: 2024-10-15SHANGHAI CIVIL ENG GRP CO LTD OF CREC +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410761500.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing foam agent used for earth pressure balance shields is not environmentally friendly due to the addition of foam stabilizers and thickeners.

Method used

Using a foaming agent consisting only of a three-arm anionic sulfonate surfactant as a blowing agent, trimethylolpropane tris(3-mercaptopropionate) and 2-acrylamido-2-methylpropanesulfonic acid The solution is mixed with a photoinitiator, and after being irradiated by ultraviolet light, an alkaline solution is added to generate a three-arm anionic sulfonate surfactant, which is dissolved in water to form a foaming agent.

Benefits of technology

It achieves excellent foaming power and foaming stability without adding foam stabilizers and thickeners. The foaming ratio is greater than 40, the foam half-life is greater than 60 minutes, and it is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772890A_ABST
    Figure CN118772890A_ABST
Patent Text Reader

Abstract

The invention discloses a foaming agent for shield tunneling, the foaming agent is only prepared from a foaming agent and water, and the foaming agent contains a three-arm anion sulfonate surfactant. The structural formula of the three-arm anionic sulfonate surfactant is as shown in formula I: # imgabs0 #. The three-arm anionic sulfonate surfactant provided by the invention can obviously reduce the surface tension of water and improve the foaming power and foaming stability of the foaming agent, so that the prepared foaming agent does not need to be added with a foam stabilizer and a thickening agent; the foaming agent has excellent foaming power and foaming stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of earth pressure balance shield, and in particular to a foaming agent used for earth pressure balance shield, a preparation method and application thereof. Background Art

[0002] In recent years, as the available space for urban transportation resources on the ground has become less and less, the development and construction of underground space has become increasingly important, and rail transit construction has become the focus of urban development. The earth pressure balance shield construction method has been widely used because it is not affected by terrain, landform, soil layer, etc., and has significant technical and economic advantages. During the construction of the earth pressure balance shield, it is necessary to inject foaming agent into the soil excavation surface through the shield machine to make the cut soil have good fluidity and plasticity, avoid soil blockage in the shield machine, and ensure the smooth progress of the shield excavation.

[0003] At present, in addition to the foaming agent used to produce foam, the foaming agent on the market also needs to add a foam stabilizer and a thickener to improve the stability and foaming ratio of the foam. However, such foaming agents with added foam stabilizers and thickeners are often not environmentally friendly. Summary of the invention

[0004] The purpose of the present invention is to solve the technical problem that the existing foaming agent is not environmentally friendly due to the addition of a foam stabilizer and a thickener, and to provide a foaming agent made only of a foaming agent.

[0005] In order to achieve the above object, the present invention provides a foaming agent for shield tunneling, which is composed of a foaming agent and water. The foaming agent includes: a three-arm anionic sulfonate surfactant, and the structural formula of the three-arm anionic sulfonate surfactant is shown in Formula I:

[0006]

[0007] Optionally, by weight percentage, the three-arm anionic sulfonate surfactant accounts for 2%-6% of the foaming agent, and the remainder is water.

[0008] Optionally, by weight percentage, the three-arm anionic sulfonate surfactant accounts for 3%-5% of the foaming agent, and the remainder is water.

[0009] The present invention also provides a method for preparing the foaming agent for shield tunneling, the method comprising the following steps:

[0010] Step S1, by weight, 138-140 parts of trimethylolpropane tris(3-mercaptopropionate) solution, 160-175 parts of 2-acrylamide-2-methylpropane sulfonic acid solution, and 0.2-1 parts of a photoinitiator are mixed evenly; after ultraviolet light irradiation, a three-arm anionic sulfonic acid is obtained;

[0011] Step S2, slowly adding the three-arm anionic sulfonic acid into an alkaline solution to obtain a three-arm anionic sulfonate surfactant;

[0012] Step S3, dissolving the three-arm anionic sulfonate surfactant in water to obtain the foaming agent for shield tunneling.

[0013] Optionally, in step S1, the molar ratio of trimethylolpropane tris(3-mercaptopropionate) to 2-acrylamido-2-methylpropanesulfonic acid is 1:3.

[0014] Optionally, in step S1, in the trimethylolpropane tris(3-mercaptopropionate) solution, the solute is trimethylolpropane tris(3-mercaptopropionate), and the solvent is a furan solvent; in the 2-acrylamide-2-methylpropane sulfonic acid solution, the solute is 2-acrylamide-2-methylpropane sulfonic acid, and the solvent is an amide solvent.

[0015] The furan solvent is tetrahydrofuran, and the amide solvent is dimethylamide.

[0016] Optionally, in step S1, the photoinitiator is benzoin dimethyl ether.

[0017] Optionally, in step S2, the alkaline solution is at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, and potassium carbonate solution.

[0018] The invention also provides application of the foaming agent in the shield construction process.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The foaming agent provided by the present invention is made of only a foaming agent and water, and does not need to add a foam stabilizer and a thickener, and has excellent foaming power (foaming ratio greater than 40) and foaming stability (half-life greater than 60 minutes).

[0021] The principle that the foaming agent provided by the present invention has excellent foaming power and foaming stability is as follows:

[0022] In the foaming agent provided by the present invention, a three-arm anionic sulfonate surfactant is used as a foaming agent, and the structure of the three-arm anionic sulfonate surfactant is shown in Formula I.

[0023]

[0024] As can be seen from Formula I, the three-arm anionic sulfonate surfactant of the present invention carries three sulfonate groups. Since the sulfonate groups can improve the foaming power and foaming stability of the foaming agent (the principle is described below), and the three-arm anionic sulfonate surfactant provided by the present invention carries three sulfonate groups, it can significantly reduce the surface tension of water and enhance the stability of the foam, so that the foaming agent of the present invention has excellent foaming power and foaming stability.

[0025] The principle that sulfonate groups can improve the foaming power of foaming agents is as follows:

[0026] Since the sulfonate group itself is a surfactant group, it can reduce the surface tension of water, making it easier for air to enter the water to form foam, thereby increasing the foaming power of the foaming agent.

[0027] The principle that sulfonate groups can improve the foaming stability of foaming agents is as follows:

[0028] When foam is formed (before the bubbles float on the liquid surface), a large amount of gas enters the water and forms bubbles in the water. At this time, since the outside of the bubbles is all water phase and the sulfonate groups have hydrophobic carbon chains, the sulfonate groups will arrange and adsorb inside the bubbles to form an inner molecular layer. The hydrophilic sulfonate ions face the surface of the bubble membrane, and the hydrophobic carbon chains face the gas phase inside the bubbles, arranging on the inner surface of the bubble membrane to form an inner molecular layer.

[0029] Subsequently, the bubbles float to the surface of the liquid due to buoyancy, and the sulfonate groups on the surface of the liquid are adsorbed on the outside of the bubble membrane to form an outer molecular layer. The hydrophilic sulfonate ions face the surface of the bubble membrane, and the hydrophobic carbon chains face the gas phase outside the bubble, arranging on the outer surface of the bubble membrane to form an outer molecular layer.

[0030] At this time, the inner molecular layer inside the bubble membrane and the outer molecular layer outside the bubble membrane form a double molecular layer to protect the bubble membrane of the bubble and enhance the stability of the bubble. DETAILED DESCRIPTION

[0031] The technical solution of the present invention is further described below in conjunction with embodiments.

[0032] Explanation of terms

[0033] Foaming ratio: refers to the ratio of the volume of foam produced by a certain volume of foam agent solution to the volume of the original foam agent solution, that is, the volume of foam produced by a unit volume of foam agent solution.

[0034] Foam half-life: The time required for the foam produced by the foaming agent to reduce to half of the liquid after reaching the maximum height.

[0035] The earth pressure balance shield construction method is an important method in urban tunnel construction projects. During the construction process, this method requires the injection of foaming agents into the soil excavation surface to make the cut soil have good fluidity and plasticity, avoid soil blockage in the shield machine, and ensure the smooth progress of shield excavation. At present, the foaming agents used on the market contain not only foaming agents for foam production, but also need to add foam stabilizers and thickeners to improve the stability and foaming ratio of the foam, but this foaming agent with added foam stabilizers and thickeners is often not environmentally friendly.

[0036] The inventors of the present application have synthesized a three-arm anionic sulfonate surfactant through a large number of experiments and explorations, and used it as a foaming agent to prepare the foaming agent for shield construction of the present invention, wherein the structural formula of the three-arm anionic sulfonate surfactant is shown in Formula I.

[0037]

[0038] As can be seen from Formula I, the three-arm anionic sulfonate surfactant of the present invention has three sulfonate groups. After the sulfonate groups are dissolved in water, the ends of the groups dissociate into Since anionic groups are formed, the three-arm anionic sulfonate surfactant prepared in the present invention is called an "anionic" sulfonate surfactant.

[0039] The sulfonate groups carried by the three-arm anionic sulfonate surfactant of the present invention can improve the foaming power and foaming stability of the foaming agent (the principle is described below), and the three-arm anionic sulfonate surfactant provided by the present invention has three sulfonate groups, which can significantly reduce the surface tension of water and enhance the stability of the foam, so that the foaming agent of the present invention has excellent foaming power and foaming stability.

[0040] The principle that sulfonate groups can improve the foaming power of foaming agents is as follows:

[0041] Since the sulfonate group itself is a surfactant group, it can reduce the surface tension of water, making it easier for air to enter the water to form foam, thereby increasing the foaming power of the foaming agent.

[0042] The principle that sulfonate groups can improve the foaming stability of foaming agents is as follows:

[0043] When foam is formed (before the bubbles float on the liquid surface), a large amount of gas enters the water and forms bubbles in the water. At this time, since the outside of the bubbles is all water phase and the sulfonate groups have hydrophobic carbon chains, the sulfonate groups will arrange and adsorb inside the bubbles to form an inner molecular layer. The hydrophilic sulfonate ions face the surface of the bubble membrane, and the hydrophobic carbon chains face the gas phase inside the bubbles, arranging on the inner surface of the bubble membrane to form an inner molecular layer.

[0044] Subsequently, the bubbles float to the surface of the liquid due to buoyancy, and the sulfonate groups on the surface of the liquid are adsorbed on the outside of the bubble membrane to form an outer molecular layer. The hydrophilic sulfonate ions face the surface of the bubble membrane, and the hydrophobic carbon chains face the gas phase outside the bubble, arranging on the outer surface of the bubble membrane to form an outer molecular layer.

[0045] At this time, the inner molecular layer inside the bubble membrane and the outer molecular layer outside the bubble membrane form a double molecular layer to protect the bubble membrane of the bubble and enhance the stability of the bubble.

[0046] In some embodiments, the three-arm anionic sulfonate surfactant accounts for 2wt%-6wt% of the entire foaming agent, and the rest is water. In this case, the foaming agent prepared can have a foaming ratio of 30 and a foam half-life of 30 minutes.

[0047] In some embodiments, the three-arm anionic sulfonate surfactant accounts for 3wt%-5wt% of the entire foaming agent, and the rest is water. In this case, the foaming agent prepared can have a foaming ratio of up to 40 and a foam half-life of up to 60 minutes.

[0048] The present invention also provides a method for preparing the foaming agent for shield tunneling, and the reaction process is as follows:

[0049]

[0050] Step S1, by weight, 138-140 parts of trimethylolpropane tris(3-mercaptopropionate) solution, 160-175 parts of 2-acrylamide-2-methylpropanesulfonic acid solution, and 0.2-1 parts of photoinitiator are mixed evenly, and then irradiated with ultraviolet light and impurities are removed to obtain a three-arm anionic sulfonic acid.

[0051] In some embodiments, the molar ratio of trimethylolpropane tris(3-mercaptopropionate) to 2-acrylamido-2-methylpropanesulfonic acid is 1:3 to generate a three-arm anionic sulfonic acid with three sulfonic acid groups.

[0052] In some embodiments, the photoinitiator is benzoin dimethyl ether.

[0053] Step S2, slowly adding the three-arm anionic sulfonic acid into an alkaline solution to obtain a three-arm anionic sulfonate surfactant.

[0054] In some embodiments, the alkaline solution may be at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, and potassium carbonate solution. Further, the alkaline solution may be a 30 wt % sodium hydroxide solution.

[0055] Step S3, dissolving the three-arm anionic sulfonate surfactant in water to obtain the foaming agent for shield tunneling of the present invention.

[0056] The following is a specific description with reference to embodiments.

[0057] Example 1

[0058] This embodiment provides a foaming agent for shield tunneling, and the preparation method thereof is as follows:

[0059] Step S1, weigh 139.86 parts of trimethylolpropane tris(3-mercaptopropionate) solution, 162.17 parts of 2-acrylamide-2-methylpropane sulfonic acid solution, and 0.5 parts of photoinitiator, mix them evenly, irradiate them under ultraviolet light for 20 minutes, and obtain 90 parts of three-arm anion sulfonic acid after removing impurities.

[0060] Step S2, dropping 90 parts of three-arm anionic sulfonic acid into 40 parts of 30 wt % sodium hydroxide aqueous solution to obtain a three-arm anionic sulfonate surfactant.

[0061] Step S3, adding a three-arm anionic sulfonate surfactant into 1670 parts of water to obtain the foaming agent for shield tunneling of this embodiment (5 wt% of a three-arm anionic sulfonate surfactant).

[0062] In this embodiment, the photoinitiator is benzoin dimethyl ether.

[0063] In this embodiment, 139.86 parts of trimethylolpropane tris(3-mercaptopropionate) solution is prepared by dissolving 39.86 parts of trimethylolpropane tris(3-mercaptopropionate) in 100 parts of a furan solvent, wherein the furan solvent is tetrahydrofuran.

[0064] In this embodiment, 162.17 parts of 2-acrylamide-2-methylpropanesulfonic acid solution is prepared by dissolving 62.17 parts of 2-acrylamide-2-methylpropanesulfonic acid in 100 parts of amide solvent, wherein the amide solvent is dimethylamide.

[0065] In this embodiment, the molar ratio of trimethylolpropane tris(3-mercaptopropionate) to 2-acrylamido-2-methylpropanesulfonic acid is 1:3.

[0066] In step S1 of this embodiment, the step of removing impurities includes: firstly removing furan solvents and amide solvents by vacuum rotary evaporation at 60°C, then dissolving the product with petroleum ether, filtering to remove excess photoinitiator, and rotary evaporating to remove petroleum ether and placing in a vacuum drying oven for 6 hours.

[0067] In the above impurity removal step, the furan solvent and amide solvent are removed first, and then the photoinitiator is removed for the following reasons:

[0068] Since the photoinitiator is soluble in furan solvents and amide solvents, if petroleum ether is added first, the petroleum ether cannot precipitate the photoinitiator because the photoinitiator has been dissolved by the furan solvents and amide solvents, and the photoinitiator cannot be filtered out. Therefore, the furan solvents and amide solvents should be removed by rotary evaporation first, and then the photoinitiator should be precipitated with petroleum ether. At this time, the photoinitiator can be removed by filtering.

[0069] Example 2

[0070] This embodiment provides a foaming agent for shield tunneling, in which the three-arm anionic sulfonate surfactant accounts for 4wt% of the foaming agent.

[0071] The difference between the preparation method of the foaming agent in this embodiment and that in Embodiment 1 is that in step S3, the mass fraction of water is 2120 parts.

[0072] Example 3

[0073] This embodiment provides a foaming agent for shield tunneling, in which the three-arm anionic sulfonate surfactant accounts for 3wt% of the foaming agent.

[0074] The difference between the preparation method of the foaming agent in this embodiment and that in Embodiment 1 is that in step S3, the mass fraction of water is 2870 parts.

[0075] Example 4

[0076] This embodiment provides a foaming agent for shield tunneling, in which the three-arm anionic sulfonate surfactant accounts for 2.5wt% of the foaming agent.

[0077] The difference between the preparation method of the foaming agent in this embodiment and that in Embodiment 1 is that in step S3, the mass fraction of water is 3470 parts.

[0078] Example 5

[0079] This embodiment provides a foaming agent for shield tunneling, in which the three-arm anionic sulfonate surfactant accounts for 5.5wt% of the foaming agent.

[0080] The difference between the preparation method of the foaming agent in this embodiment and that in Embodiment 1 is that in step S3, the mass fraction of water is 1506 parts.

[0081] Comparative Example 1

[0082] This comparative example is used for comparison with Example 2.

[0083] The difference between the preparation method of the foaming agent in this comparative example and that in Example 2 is that in step S1, natural light is used instead of ultraviolet light.

[0084] Comparative Example 2

[0085] This comparative example is used for comparison with Example 2.

[0086] The difference between the preparation method of the foaming agent in this comparative example and that in Example 2 is that no NaOH treatment is used (step S2 is omitted), and after 90 parts of three-arm anion sulfonic acid are generated in step S1, the three-arm anion sulfonic acid is directly added to 2160 parts of water.

[0087] Comparative Example 3

[0088] This comparative example is used for comparison with Example 2.

[0089] The difference between the preparation method of the foaming agent of this comparative example and that of Example 2 is that in step S1, the amount of 2-acrylamide-2-methylpropane sulfonic acid used is 41.45 parts by mass, and 70 parts by mass of three-arm anionic sulfonic acid are obtained.

[0090] This comparative example reduces the amount of 2-acrylamide-2-methylpropanesulfonic acid used, and the molar ratio of trimethylolpropane tris(3-mercaptopropionate) to 2-acrylamide-2-methylpropanesulfonic acid in Example 2 is reduced from 1:3 to 1:2.

[0091] In addition, in order to ensure that the mass percentage of the main components in the foaming agent of this comparative example is the same as that of Example 2 (both are 4wt%), the mass percentage of water in step S3 of this comparative example is 1640 parts.

[0092] Comparative Example 4

[0093] This comparative example is used for comparison with Example 2.

[0094] This comparative example uses a commercially available BASF foaming agent, which is diluted to 4 wt%.

[0095] Comparative Example 5

[0096] This comparative example is used for comparison with Example 2.

[0097] This comparative example uses commercially available CONDAT foaming agent, which is diluted to 4 wt %.

[0098] The foaming agents of each embodiment and comparative example were evaluated by the following method:

[0099] Foaming ratio: Add the foaming agent into the measuring cup and record the volume of the foaming agent. Use the indoor foaming device to foam the foaming agent and use the measuring cup to record the volume of bubbles.

[0100] Foaming ratio = bubble volume ÷ foaming agent volume

[0101] Foam half-life: Add the foaming agent into the measuring cup, use the measuring cup to record the initial volume of the bubbles, and start timing. When the foam volume drops to half of the initial volume, stop timing and record the time required, which is the foam half-life.

[0102] The properties of the foaming agents of various embodiments and comparative examples are shown in Table 1.

[0103] Table 1 Performance test results of Examples 1-5 and Comparative Examples 1-5

[0104]

[0105] The inventors of this application found through the above experiments:

[0106] It can be seen from Example 2 and Comparative Examples 1-5 in Table 1 that:

[0107] Compared with Example 2, Comparative Example 1 uses natural light as the reaction condition. In this case, trimethylolpropane tris(3-mercaptopropionate) and 2-acrylamido-2-methylpropane sulfonic acid do not undergo a click reaction between the thiol group and the double bond, and an anionic surfactant cannot be generated. The foaming ratio and half-life of the foaming agent of Comparative Example 1 are lower than those of Example 2.

[0108] Compared with Example 2, Comparative Example 2 did not add NaOH, and the reaction only generated three-arm anionic sulfonic acid, and no anionic surfactant was generated. The acidic substance could not produce stable micelles, and the foaming rate and half-life of the foaming agent in Comparative Example 2 were lower than those in Example 2.

[0109] Compared with Example 2, in Comparative Example 3, trimethylolpropane tris(3-mercaptopropionate) and 2-acrylamide-2-methylpropane sulfonic acid in a molar ratio of 1:2 are used to prepare the foaming agent. The surfactant generated by the reaction has only two sulfonate groups, and its foaming ratio and half-life are lower than those of the foaming agent in Example 2.

[0110] Comparative Examples 4 and 5 are commercially available BASF and CONDAT products, respectively. The foaming ratio and half-life of the foaming agent of the present invention are better than those of BASF and CONDAT products.

[0111] It can be seen from Examples 1-5 of Table 1 that:

[0112] As the concentration of the three-arm anionic sulfonate surfactant in the foaming agent increases from 5wt% to 2.5wt%, the foaming ratio of the foaming agent decreases and the half-life becomes shorter, indicating that the performance of the foaming agent is related to the concentration of the three-arm anionic sulfonate surfactant. The higher the concentration of the three-arm anionic sulfonate surfactant, the better the performance of the foaming agent.

[0113] When the concentration of the three-arm anionic sulfonate surfactant was further increased to 5.5wt%, the foaming ratio and half-life of the foaming agent did not change, indicating that the system had reached saturation and the performance of the foaming agent no longer changed with the concentration of the three-arm anionic sulfonate surfactant.

[0114] The above experiments show that in the foaming agent provided by the present invention, the concentration of the three-arm anionic sulfonate surfactant is preferably 3wt%-5wt%.

[0115] In summary, the present invention provides a foaming agent for shield tunneling, which is made of only a foaming agent and water, wherein the foaming agent contains a three-arm anionic sulfonate surfactant, which can significantly reduce the surface tension of water and improve the foaming power and foaming stability of the foaming agent. The foaming agent provided by the present invention does not need to add a foam stabilizer and a thickener, and has excellent foaming power (foaming ratio greater than 40) and foaming stability (half-life greater than 60min).

[0116] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.

Claims

1. A foaming agent for shield tunneling, It is characterized in that It is composed of a foaming agent and water; the foaming agent includes: a three-arm anionic sulfonate surfactant, and the structural formula of the three-arm anionic sulfonate surfactant is shown in Formula I:

2. The foaming agent for shield according to claim 1, It is characterized in that In terms of weight percentage, the three-arm anionic sulfonate surfactant accounts for 2%-6% of the foaming agent, and the remainder is water.

3. The foaming agent for shield according to claim 2, It is characterized in that In terms of weight percentage, the three-arm anionic sulfonate surfactant accounts for 3%-5% of the foaming agent, and the balance is water.

4. A method for preparing the foaming agent according to any one of claims 1 to 3, It is characterized in that The following steps are involved: Step S1, by weight, 138-140 parts of trimethylolpropane tris(3-mercaptopropionate) solution, 160-175 parts of 2-acrylamide-2-methylpropane sulfonic acid solution, and 0.2-1 parts of a photoinitiator are mixed evenly; after ultraviolet light irradiation, a three-arm anionic sulfonic acid is obtained; Step S2, slowly adding the three-arm anionic sulfonic acid into an alkaline solution to obtain a three-arm anionic sulfonate surfactant; Step S3, dissolving the three-arm anionic sulfonate surfactant in water to obtain the foaming agent for shield tunneling.

5. The method for preparing the foaming agent according to claim 4, It is characterized in that In step S1, the molar ratio of trimethylolpropane tris(3-mercaptopropionate) to 2-acrylamido-2-methylpropanesulfonic acid is 1:

3.

6. The method for preparing the foaming agent according to claim 4, It is characterized in that In step S1, in the trimethylolpropane tris(3-mercaptopropionate) solution, the solute is trimethylolpropane tris(3-mercaptopropionate), and the solvent is a furan solvent; in the 2-acrylamide-2-methylpropane sulfonic acid solution, the solute is 2-acrylamide-2-methylpropane sulfonic acid, and the solvent is an amide solvent.

7. The method for preparing the foaming agent according to claim 6, It is characterized in that The furan solvent is tetrahydrofuran, and the amide solvent is dimethylamide.

8. The method for preparing the foaming agent according to claim 4, It is characterized in that In step S1, the photoinitiator is benzoin dimethyl ether.

9. The method for preparing the foaming agent according to claim 4, It is characterized in that In step S2, the alkaline solution is at least one of sodium hydroxide, potassium hydroxide, sodium carbonate and potassium carbonate solution.

10. Use of the foaming agent according to any one of claims 1 to 3 in a shield construction process.