Preparation method of composite material with interface formed by reaction of metal melt and ceramic liquid phase
By making the ceramic liquid phase and the metal liquid phase form a continuous two-liquid phase coexistence state during the preparation of ceramic/metal composite materials, an interfacial reaction occurs and an interface layer is formed, which solves the problem of low bonding strength of ceramic/metal composite materials and significantly improves the Comprehensive properties and compressive strength of materials.
Patent Information
- Application Number
- CN202411266303.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the preparation process of ceramic/metal composite materials, the poor wettability between the metal melt and the ceramic phase leads to problems of low bonding strength and poor overall performance.
By mixing ceramic raw materials and metals in a certain proportion and heating, the liquid phase of the ceramic and the liquid metal phase form a continuous two-liquid phase coexistence state, and an interfacial reaction occurs to form an interface layer of intermetallic compounds, elemental substances and solid solutions, thereby realizing ceramic/metal composites. Tight combination of materials.
It significantly improves the interface bonding strength and comprehensive performance of ceramic/metal composite materials, enhances the material's load-bearing capacity and compressive strength, solves the pore problem caused by poor wettability, and achieves higher specific strength and energy absorption capacity.
Smart Images

Figure CN118773471A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of high temperature resistant structural composite materials, and in particular relates to a method for preparing a composite material with an interface formed by a metal melt and a ceramic liquid phase reaction. Background Art
[0002] Ceramic / metal composite materials have high specific strength, fracture toughness, corrosion resistance, low thermal expansion coefficient and good energy absorption performance. They have a wide range of applications, including aerospace, weapons and equipment, automobiles and ships, construction industry, entertainment facilities and other fields, and have broad application prospects. At present, the conventional preparation method is to prepare ceramics first and then composite with metals. Due to the poor wettability of molten metals and these ceramics, the degree of bonding between the two is low, thereby reducing the comprehensive mechanical properties of the material. Therefore, in the process of transferring loads, the ceramic phase will fall off and become unstable, which will affect the comprehensive performance of the composite material.
[0003] There are certain limitations in adjusting the wettability of the interface through surface treatment, such as chemical plating, ceramic interface corrosion, and changing the surface roughness. Not only does it have certain requirements on the physical properties of the ceramic phase, but the entire process preparation is also complicated.
[0004] The present invention starts from the bonding effect of the interface, and through component design, when the ceramic produces a liquid phase, it forms a continuous double liquid phase coexistence state with the metal liquid phase and reacts, and generates an interface layer mixed with a single substance, an intermetallic compound and a solid solution between the two phases, thereby obtaining a new process for obtaining a ceramic / metal composite material with good interface bonding strength. The problem of poor wettability of the two phases of the ceramic / metal composite material, low bonding strength and poor comprehensive performance is solved. Summary of the invention
[0005] The present invention provides a method for preparing a composite material in which a metal melt reacts with a ceramic liquid phase to form an interface. The technical problem to be solved is to make the metal melt react with the ceramic when a liquid phase is generated, and to form a tightly bonded interface reaction transition layer between the ceramic phase and the metal phase, so as to solve the technical problem of poor wettability and low comprehensive performance between the metal melt and the ceramic phase in the process of preparing the ceramic / metal composite material.
[0006] The technical solution of the present invention is: A method for preparing a composite material having an interface formed by a metal melt and a ceramic liquid phase reaction comprises the following steps: (1) The ceramic raw materials are mixed and mechanically formed to obtain a ceramic body; (2) The ceramic body and the metal are mixed in a certain proportion, placed in a container, heated to melt the metal into a liquid phase, and the ceramic body and the metal are tightly combined to obtain a preform; (3) When the ceramic in the preform produces a liquid phase at 800°C to 1300°C, it forms a continuous two-liquid phase coexistence state with the metal liquid phase and undergoes an interfacial reaction to form intermetallic compounds, single substances and solid solutions, thereby obtaining a ceramic / metal composite material with an interfacial reaction transition layer.
[0007] Furthermore, in the method for preparing the composite material having an interface formed by the reaction of the metal melt and the ceramic liquid phase, in step (1), the ceramic raw material includes one or more of SiO2, Al2O3, TiO2, Fe2O3, MnO2 and one or more of CaO, MgO, Na2O, K2O; the shape of the ceramic raw material body is not limited.
[0008] Furthermore, in the method for preparing the composite material in which the metal melt and the ceramic liquid phase react to form an interface, in step (2), the liquidus point of the ceramic body is higher than the melting point of the metal used. Furthermore, in the method for preparing the composite material in which the metal melt and the ceramic liquid phase react to form an interface, the physical form of the metal is solid metal, including but not limited to block and powder.
[0009] Furthermore, in the method for preparing the composite material having an interface formed by the reaction between the metal melt and the ceramic liquid phase, in the step (2), during the preparation of the preform, the metal and the ceramic body are placed in a container, the temperature is increased to melt the metal, and then the metal is infiltrated by pressurization or negative pressure.
[0010] Furthermore, in the method for preparing the composite material having an interface formed by the reaction of the metal melt and the ceramic liquid phase, in the step (2), the metal types include magnesium, aluminum and their alloys, and the volume fraction of the ceramic body is 10% to 90%.
[0011] Furthermore, in the method for preparing the composite material in which the metal melt reacts with the ceramic liquid phase to form an interface, in the step (3), the ceramic green body in the preform will produce a liquid phase at a sintering temperature of about 800°C to 1300°C; the metal used will react with the ceramic green body at a sintering temperature of about 800°C to 1300°C; and the temperature will be kept at the temperature at which the interface reaction occurs for 5 minutes to 120 minutes.
[0012] Furthermore, in the method for preparing the composite material in which the metal melt reacts with the ceramic liquid phase to form an interface, in the step (3), during the interfacial reaction, the reaction not only occurs at the interface between the two phases and forms an interfacial transition layer at the interface, but also the metal melt diffuses inward along the grain boundaries in the ceramic body to react with the liquid phase generated therein, and precipitates a single substance, a solid solution and an intermetallic compound inside the ceramic.
[0013] Advantages and beneficial effects of the present invention: 1. The present invention utilizes the characteristics of the ceramics forming a continuous double liquid phase coexistence state with the metal liquid phase and undergoing an interfacial reaction for the first time, and prepares a ceramic / metal composite material with an interfacial reaction transition layer through infiltration and chemical reaction. Its advantage is that the intermetallic compounds, simple substances and solid solutions precipitated by the interfacial reaction are distributed between the two phase interfaces and form an interfacial layer, which not only allows the interfacial layer to be fully combined with the ceramics and metals, making up for the pores left between the metal and the ceramics due to mechanical bonding, and greatly increases the contact area between the two, but also the ceramic phase and the metal phase can diffuse with the interfacial layer to improve the interfacial bonding force, thereby effectively promoting load transfer, and can maximize the role of the interfacial layer so that the composite material has a higher load-bearing capacity and the ability to resist deformation and other comprehensive properties. Moreover, in the process of the ceramics producing a liquid phase, the ceramic liquid phase will expand outward and squeeze the external metal liquid phase to promote the densification of the interface and the occurrence of interfacial reactions, thereby achieving a close combination of the interface layer.
[0014] 2. Since metals and ceramics are in a continuous dual-liquid coexistence state within a specific temperature range, matching metals and ceramics can be selected for compounding according to the actual service temperature conditions. Therefore, this technology has a wide range of applications.
[0015] 3. The ceramic / metal composite material provided by the present invention can achieve good wetting between the ceramic phase and the metal phase, solving the key problem of poor wettability of metal-ceramic composite materials, pores at the interface leading to residual stress concentration and interface cracking. A ceramic / metal composite material with high specific strength, high compressive strength and high energy absorption capacity can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 is a process flow chart of the present invention; Figure 2 This is a SEM view of the interface of the sample prepared in Example 1 of the present invention; Figure 3 This is the XRD analysis diagram of the sample prepared in Example 1 of the present invention; In the figure, Figure 2 It consists of Figure (a) and Figure (b), Figure (b) is a local enlarged SEM image of Figure (a), Figure 2 In the middle, 1-metal aluminum, 2-interface reaction transition layer, 3-ceramic, it can be seen that the interface bonding is good; Figure 3It consists of Figure (a) and Figure (b), where Figure (a) is the XRD phase composition of the preform, which is mainly composed of metal aluminum and silicon oxide, aluminum oxide, magnesium oxide, and calcium oxide in the ceramic. In addition, Figure (b) is the XRD phase composition of the sample after sintering, which is mainly composed of metal aluminum, elemental silicon and aluminum silicon compounds, indicating that the oxides in the ceramic reacted with the molten aluminum during the sintering process to form a new phase, thereby improving the bonding strength of the interface. The generated forsterite, spinel and calcium feldspar are mainly transformed from the oxides in the ceramic. DETAILED DESCRIPTION
[0017] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention but cannot be used to limit the scope of the present invention.
[0018] Example 1
[0019] The method for preparing the ceramic / metal composite material prepared in this embodiment comprises the following steps: The ceramic raw materials bauxite and asbestos tailings (Al2O3-SiO2 system) are mixed and then evenly mixed in a ball mill to obtain a mixed powder.
[0020] The mixed powder was put into a round pot granulator for ball making at a speed of 40 r / min for 1 h to obtain a spherical ceramic body with a ball diameter of 1 mm; the ceramic body was dried at a temperature of 80° C. for 4 h.
[0021] The ceramic green body and metal aluminum are placed in a crucible for pressure infiltration. The volume fraction of the ceramic green body is 10%, the infiltration temperature is 760°C, the infiltration pressure is 9.8N, the infiltration time is 1.5min, and the holding time is 0min. The ceramic green body and the molten aluminum are combined together, and a preform is obtained after cooling.
[0022] The preform is subjected to reaction sintering with a sintering temperature of 1100°C and a holding time of 5 minutes, so that the aluminum first melts at about 700°C, and then the ceramic produces a liquid phase and becomes a semi-liquid phase at about 1000°C. When the ceramic in the preform produces a liquid phase at 1000°C, it forms a continuous double liquid phase coexistence state with the metal liquid phase and an interface reaction occurs, thereby improving the bonding strength of the interface, and a ceramic / metal composite material is obtained as the furnace is cooled.
[0023] The preparation flow chart of this embodiment is as follows Figure 1 As shown, Figure 2 (a) is the interface SEM image of the sample, and (b) is a local enlarged image of (a). It can be seen that the white interface transition reaction layer is well bonded with the metal aluminum and ceramic. Figure 3XRD analysis of the preform and the sample. (a) is the phase composition of the preform, which is mainly composed of aluminum and oxides in the ceramic. In addition, (b) is the XRD phase composition of the sample, in which silicon and aluminum-silicon compounds are new phases formed by the reaction of aluminum melt and semi-liquid ceramics. Other compounds are transformed from oxides in the ceramic, including forsterite, spinel and calcium feldspar. The average density of the obtained ceramic / metal composite material is 2.2g / cm3, the porosity is 12.6%, and the compressive strength is 112MPa.
[0024] Example 2
[0025] The preparation method of the ceramic / metal composite material prepared in this embodiment comprises the following steps: The ceramic raw material Al2O3-SiO2 analytical pure powder, the foaming agent SiC, the auxiliary solvent MgO and NaO are mixed, and then mixed evenly by a ball mill to obtain a mixed powder.
[0026] The mixed powder was put into a round pot granulator for ball making at a speed of 60 r / min for 0.5 h to obtain a spherical ceramic body with a diameter of 2 mm; the ceramic body was dried at a temperature of 80° C. for 4 h.
[0027] The ceramic green body and metallic magnesium are placed in a crucible for pressure infiltration. The volume fraction of the ceramic green body is 20%, the infiltration temperature is 700°C, the infiltration pressure is 15.8N, the infiltration time is 0.5min, and the holding time is 1min. The ceramic green body and the molten magnesium are combined together, and a preform is obtained after cooling.
[0028] The preform is subjected to reaction sintering, the sintering temperature is 1000℃, the holding time is 15min, the metal magnesium is melted at about 700℃, and then the ceramic will produce liquid phase to become semi-liquid phase at about 900℃. When the ceramic in the preform produces liquid phase at 900℃, it forms a continuous double liquid phase coexistence state with the metal liquid phase and an interface reaction occurs to improve the bonding strength of the interface. Magnesium can reduce aluminum oxide and silicon oxide to generate elemental aluminum and elemental silicon and magnesium-aluminum, aluminum-silicon, magnesium-silicon and other compounds (such as Mg 17 Al 12 , Si9Al, Mg2Si, etc.), and then the ceramic / metal composite material is obtained by cooling in the furnace.
[0029] The average density of the ceramic / metal composite material prepared in this embodiment is 2.0 g / cm 3 , the porosity is 21.7% and the compressive strength is 132MPa.
[0030] Example 3
[0031] The preparation method of the ceramic / metal composite material prepared in this embodiment comprises the following steps: The ceramic raw materials diatomaceous earth, red mud and potassium feldspar (SiO2-Al2O3-K2O system) are mixed and then uniformly mixed by a ball mill to obtain a mixed powder.
[0032] The mixed powder was put into a star-shaped molding machine with a molding pressure of 5 MPa and maintained at pressure for 5 minutes to obtain a star-shaped ceramic body with a diagonal length of 5 mm and a thickness of 5 mm; the ceramic body was dried at a temperature of 80°C for 4 hours.
[0033] The ceramic green body and the aluminum-silicon alloy are placed in a crucible for pressure infiltration. The volume fraction of the ceramic green body is 30%, the infiltration temperature is 650°C, the infiltration pressure is 15.8N, the infiltration time is 0.5min, and the holding time is 1min. The ceramic green body and the aluminum-silicon alloy melt are combined together, and a preform is obtained after cooling.
[0034] The preform is subjected to reaction sintering with a sintering temperature of 1100°C and a holding time of 60 minutes, so that the aluminum-silicon alloy first melts at about 650°C, and then the ceramic produces a liquid phase and becomes a semi-liquid phase at about 1000°C. When the ceramic in the preform produces a liquid phase at 1000°C, it forms a continuous double liquid phase coexistence state with the metal liquid phase and undergoes an interface reaction, thereby improving the interface bonding strength. The aluminum in the aluminum-silicon alloy can reduce the silicon oxide in the ceramic to generate elemental silicon and generate aluminum-silicon compounds, and a ceramic / metal composite material is obtained as the furnace cools.
[0035] The average density of the ceramic / metal composite material prepared in this embodiment is 1.9 g / cm 3 , the porosity is 29.2% and the compressive strength is 125MPa.
[0036] Example 4
[0037] The method for preparing the ceramic / metal composite material prepared in this embodiment comprises the following steps: The analytically pure powders of ceramic raw materials SiO2-Al2O3-CaO-MgO-Na2O-K2O were mixed and uniformly mixed by a ball mill to obtain a mixed powder.
[0038] The mixed powder was put into a star-shaped molding machine with a molding pressure of 10 MPa and maintained at pressure for 2 minutes to obtain a star-shaped ceramic body with a diagonal length of 10 mm and a thickness of 10 mm; the ceramic body was dried at a temperature of 80°C for 4 hours.
[0039] The ceramic green body and the aluminum-magnesium alloy are placed in a crucible for pressure infiltration. The volume fraction of the ceramic green body is 40%, the infiltration temperature is 550°C, the infiltration pressure is 20.8N, the infiltration time is 2.5min, and the holding time is 1min. The ceramic green body and the molten aluminum-magnesium alloy are combined together, and a preform is obtained after cooling.
[0040] The preform is subjected to reaction sintering, the sintering temperature is 800℃, and the holding time is 120min, so that the aluminum-magnesium alloy is first melted at about 550℃, and then the ceramic will produce a liquid phase and become a semi-liquid phase at about 800℃. When the ceramic in the preform produces a liquid phase at 800℃, it forms a continuous double liquid phase coexistence state with the metal liquid phase and an interface reaction occurs, thereby improving the interface bonding strength. The aluminum-magnesium alloy can reduce the silicon oxide and aluminum oxide in the ceramic to generate single aluminum and silicon and aluminum-silicon, magnesium-silicon, aluminum-magnesium and other compounds (such as Si9Al, Mg2Si, Mg 17 Al 12 etc.) and then cooled in the furnace to obtain a ceramic / metal composite material.
[0041] The average density of the ceramic / metal composite material prepared in this embodiment is 1.8 g / cm 3 , the porosity is 34.5% and the compressive strength is 118MPa.
[0042] Example 5
[0043] The method for preparing the ceramic / metal composite material prepared in this embodiment comprises the following steps: The ceramic raw materials of coal gangue, iron tailings and albite (SiO2-Fe2O3-Na2O system) are mixed and then evenly mixed in a ball mill to obtain a mixed powder.
[0044] The mixed powder was put into a square pressing machine with a pressure of 5 MPa and the pressure was maintained for 0 min to obtain a square ceramic body with a side length of 10 mm; the ceramic body was dried at a temperature of 80°C for 4 h.
[0045] The ceramic green body and the aluminum-copper alloy are placed in a crucible for pressure infiltration. The volume fraction of the ceramic green body is 50%, the infiltration temperature is 740°C, the infiltration pressure is 9.8N, the infiltration time is 0.5min, and the holding time is 0min, so that the ceramic green body and the molten aluminum-copper alloy are combined together, and a preform is obtained after cooling.
[0046] The preform is subjected to reaction sintering, with a sintering temperature of 1300°C and a holding time of 5 minutes, so that the aluminum-copper alloy is first melted at about 740°C, and then the ceramic will produce a liquid phase and become a semi-liquid phase at about 1200°C. When the ceramic in the preform produces a liquid phase at 1300°C, it forms a continuous double liquid phase coexistence state with the metal liquid phase and an interface reaction occurs, thereby improving the interface bonding strength. The aluminum-copper alloy can reduce the silicon oxide and iron oxide in the ceramic to generate elemental silicon and iron and generate aluminum-silicon, silicon-iron and other compounds (such as Si9Al, FeSi, etc.), and obtain a ceramic / metal composite material with furnace cooling.
[0047] The average density of the ceramic / metal composite material prepared in this embodiment is 1.73 g / cm 3 , the porosity is 41.4% and the compressive strength is 152MPa.
[0048] Example 6
[0049] The method for preparing the ceramic / metal composite material prepared in this embodiment comprises the following steps: The ceramic raw materials yellow sand - red mud - rutile tailings - talc (SiO2-Al2O3-TiO2-MgO system) are mixed and then evenly mixed in a ball mill to obtain a mixed powder.
[0050] The mixed powder was put into a square pressing machine with a pressure of 5 MPa and maintained for 0 min to obtain a square ceramic body with a side length of 10 mm; the ceramic body was dried at a temperature of 100°C for 6 h.
[0051] The ceramic green body and the magnesium-aluminum alloy are placed in a crucible for pressure infiltration. The volume fraction of the ceramic green body is 60%, the infiltration temperature is 700°C, the infiltration pressure is 9.8N, the infiltration time is 2min, and the holding time is 0.5min. The ceramic green body and the molten magnesium-aluminum alloy are combined together, and a preform is obtained after cooling.
[0052] The preform is subjected to reaction sintering, with a sintering temperature of 1100°C and a holding time of 40 minutes, so that the magnesium-aluminum alloy is first melted at about 700°C, and then the ceramic will produce a liquid phase and become a semi-liquid phase state under the action of the auxiliary solvent MgO at about 1000°C. When the ceramic in the preform produces a liquid phase at 1000°C, it forms a continuous double liquid phase coexistence state with the metal liquid phase and an interface reaction occurs, thereby improving the bonding strength of the metal-ceramic interface. The magnesium-aluminum alloy can reduce silicon oxide, aluminum oxide, and titanium oxide in the ceramic to generate elemental silicon, elemental aluminum, and elemental titanium and generate magnesium-silicon, aluminum-silicon, aluminum-titanium and other compounds (such as Mg2Si, Si9Al, TiAl, etc.), and obtain a ceramic / metal composite material with furnace cooling.
[0053] The average density of the ceramic / metal composite material prepared in the embodiment is 1.6 g / cm 3 , the porosity is 46.2% and the compressive strength is 92MPa.
[0054] Example 7
[0055] The method for preparing the ceramic / metal composite material prepared in this embodiment comprises the following steps: The ceramic raw materials SiO2-Al2O3-TiO2-MgO-K2O are mixed and then uniformly mixed by a ball mill to obtain a mixed powder.
[0056] The mixed powder was put into a round pot granulator for ball making at a speed of 60 r / min for 0.5 h to obtain a spherical ceramic body with a diameter of 2 mm; the ceramic body was dried at a temperature of 100° C. for 8 h.
[0057] The ceramic green body and the aluminum-silicon-magnesium alloy are placed in a crucible for pressure infiltration. The volume fraction of the ceramic green body is 90%, the infiltration temperature is 680°C, the infiltration pressure is 9.8N, the infiltration time is 2min, and the holding time is 0.5min. The ceramic green body and the aluminum-silicon-magnesium alloy melt are combined together, and a preform is obtained after cooling.
[0058] The preform is subjected to reaction sintering at a sintering temperature of 1250°C and a holding time of 20 minutes, so that the aluminum-silicon-magnesium alloy is first melted at about 680°C, and then the ceramic will produce a liquid phase and become a semi-liquid phase at about 1150°C. When the ceramic in the preform produces a liquid phase at 1250°C, it forms a continuous double liquid phase coexistence state with the metal liquid phase and undergoes an interface reaction, thereby improving the interface bonding strength. The aluminum-silicon-magnesium alloy can reduce silicon oxide, aluminum oxide, and titanium oxide in the ceramic to generate elemental silicon, elemental aluminum, and elemental titanium, and generate aluminum-silicon, magnesium-silicon, aluminum-titanium and other compounds (such as Si9Al, Mg2Si, TiAl, etc.), and obtain a ceramic / metal composite material with furnace cooling.
[0059] The average density of the ceramic / metal composite material prepared in the embodiment is 1.5 g / cm 3 , the porosity is 62.3% and the compressive strength is 96MPa.
[0060] It is easy for those skilled in the art to understand that, under the premise of no conflict, the above-mentioned advantageous methods can be freely combined and superimposed.
[0061] The above are only preferred examples of the present application and are not intended to limit the present application. Any modifications, equivalent replacements and improvements made within the spirit and principles of the present application shall be included in the protection scope of the present application. The above are only preferred implementations of the present application. It should be pointed out that ordinary technicians in this technical field can make several improvements and variations without departing from the technical principles of the present application, and these improvements and variations should also be regarded as the protection scope of the present application.
Claims
1. A method for preparing a composite material having an interface formed by a metal melt and a ceramic liquid phase reaction, characterized in that: The following steps are involved: (1) The ceramic raw materials are mixed and mechanically formed to obtain a ceramic body; (2) The ceramic body and the metal are mixed in a certain proportion, placed in a container, heated to melt the metal into a liquid phase, and the ceramic body and the metal are tightly combined to obtain a preform; (3) When the ceramic in the preform produces a liquid phase at 800°C to 1300°C, it forms a continuous two-liquid phase coexistence state with the metal liquid phase and undergoes an interfacial reaction to form intermetallic compounds, single substances and solid solutions, thereby obtaining a ceramic / metal composite material with an interfacial reaction transition layer.
2. The method for preparing a composite material having an interface formed by a metal melt and a ceramic liquid phase reaction according to claim 1, characterized in that: In step (1), the ceramic raw material includes one or more of SiO2, Al2O3, TiO2, Fe2O3, MnO2 and one or more of CaO, MgO, Na2O, K2O; the shape of the ceramic raw material body is not limited.
3. The method for preparing a composite material having an interface formed by a metal melt and a ceramic liquid phase reaction according to claim 1, characterized in that: In step (2), the liquidus point of the ceramic body is higher than the melting point of the metal used.
4. The method for preparing a composite material having an interface formed by a metal melt and a ceramic liquid phase reaction according to claim 1, characterized in that: In the step (2), during the preparation of the preform, the metal and the ceramic body are placed in a container, heated to melt the metal, and then infiltrated by pressurization or negative pressure.
5. The method for preparing a composite material having an interface formed by a metal melt and a ceramic liquid phase reaction according to claim 1, characterized in that: In the step (2), the metal types include magnesium, aluminum and their alloys; and the volume fraction of the ceramic body is 10% to 90%.
6. The method for preparing a composite material having an interface formed by a metal melt and a ceramic liquid phase reaction according to claim 1, characterized in that: In the step (3), the ceramic green body in the preform will produce a liquid phase at a sintering temperature between 800°C and 1300°C; the metal used will react with the ceramic green body at a sintering temperature between 800°C and 1300°C; and the preform will be kept at a temperature at which an interfacial reaction occurs for 5 minutes to 120 minutes.
7. The method for preparing a composite material having an interface formed by a metal melt and a ceramic liquid phase reaction according to claim 1, characterized in that: In the step (3), during the interfacial reaction, the reaction will not only occur at the interface between the two phases and form an interfacial transition layer at the interface, but the metal melt will also diffuse inward along the grain boundaries in the ceramic body and react with the liquid phase generated therein, and precipitate a single substance, a solid solution and an intermetallic compound inside the ceramic.
Citation Information
Patent Citations
Ceramic particle enhanced magnesium-based composite material and preparation method thereof
CN103725947A
Preparation method for high-toughness abrasion-resistant metal ceramics
CN108277415A
Al2O3-base series composite materials and prepn. thereof
CN1145346A
Silver-metal oxide composite material and process for producing the same
US5286441A