Low-stress metallized plastic current collector and preparation method thereof

The film stress is reduced through infrared irradiation treatment technology, which solves the problem of reduced adhesion between the conductive layer and the substrate layer, and improves the cycle life of lithium-ion batteries and the performance of new energy batteries.

CN118782804APending Publication Date: 2024-10-15JIANGSU THREE LAYERS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410750252.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The film stress generated during the preparation process of traditional metallized plastic current collectors reduces the adhesion between the conductive layer and the substrate layer, affecting the cycle life and high-temperature storage performance of lithium-ion batteries.

Method used

Infrared irradiation treatment technology is used to heat treat the conductive layer to reduce the internal stress of the film and enhance the bonding force between the conductive layer and the substrate layer. The conductive layer is formed by argon ionization and magnetron sputtering in a vacuum chamber, and is passed Multi-layer superposition and infrared irradiation treatment obtain low-stress metallized plastic current collectors.

Benefits of technology

The adhesion between the conductive layer and the base material layer is improved, the electrolyte resistance of the metallized plastic current collector is enhanced, and the cycle life of the new energy battery is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782804A_ABST
    Figure CN118782804A_ABST
Patent Text Reader

Abstract

The invention relates to a low-stress metallized plastic current collector and a preparation method thereof. The preparation method comprises the following steps: S1, pretreating a base material layer; s2, forming a conductive layer on the pretreated base material layer; s3, performing infrared irradiation treatment on the conductive layer; and S4, repeating the steps S2-S3 for a plurality of times on the conductive layer subjected to infrared irradiation to obtain a base material layer on which a plurality of conductive layers are laminated, and performing the same process on the other side of the base material layer to obtain the low-stress metallized plastic current collector, the conductive layer is subjected to heat treatment through infrared radiation, atoms in the conductive layer exchange energy through lattice vibration, some dislocation is healed, and therefore the internal stress of the thin film is reduced; meanwhile, vacancies, gaps and other defects are eliminated when atoms in the conducting layer are diffused on the surface, so that the volume is shrunk to release residual internal stress in the conducting layer, finally, the binding force between the conducting layer and the base material layer is increased, the electrolyte resistance is enhanced, and the cycle life of the battery is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of batteries, and in particular to a low-stress metallized plastic current collector and a preparation method thereof. Background Art

[0002] With the continuous development and growth of the new energy industry, the current commercial lithium-ion batteries can no longer meet the growing demand for high safety, high energy density and power density. Among them, the current collector plays an extremely important role as an indispensable component in the battery, and its performance cannot be ignored in the overall battery performance. The traditional metal foil current collector affects the energy density of the battery due to the presence of a thicker metal layer. Compared with metal materials, polymer materials have lower density and higher mechanical strength. Therefore, the use of polymer materials is expected to make a breakthrough in the energy density of the battery.

[0003] However, since it is composed of pure metal and has the characteristics of brittleness and low toughness, it is prone to breakage and edge damage when used in the coating, rolling, drying, slicing and other processes of lithium-ion battery electrode materials under heat and tension during production. This can easily lead to material waste, poor product consistency, and reduced production efficiency. At the same time, pure metal current collectors are no longer the best application carriers due to many key factors such as cost, safety, and energy density. Therefore, many studies have begun to focus on replacing traditional metal current collectors with lightweight flexible metal / plastic composite film materials to achieve higher safety, higher volume energy density, and higher mass energy density for lithium batteries.

[0004] Metallized plastic current collectors are usually prepared by magnetron sputtering, evaporation plating, water electroplating and other processes when preparing the metal conductive layer, and the generation of film stress is a common phenomenon in the process of film deposition. The existence of film stress will affect the microstructure and properties of the film, such as the electrical and mechanical physical properties of the film, and also affect the bonding degree between the film and the base material and the basic properties of the base material.

[0005] This part of the film stress further leads to a decrease in the adhesion between the conductive layer and the polymer film. During the electrode processing and the life cycle of the lithium-ion battery, there are phenomena such as the peeling of the surface conductive layer of the metallized plastic current collector, which seriously affects the cycle life and high-temperature storage performance of the lithium-ion battery. Therefore, how to overcome the film stress generated during the preparation of the metal conductive layer is a technical problem that needs to be urgently solved in this field. Summary of the invention

[0006] The invention provides a low-stress metallized plastic current collector and a preparation method thereof, so as to solve the problem of the surface conductive layer of the metallized plastic current collector falling off due to film stress.

[0007] In order to solve the above technical problems, the present invention provides a method for preparing a low-stress metallized plastic current collector, comprising the following steps: step S1, pretreating a substrate layer; step S2, forming a conductive layer on the pretreated substrate layer; step S3, performing infrared radiation treatment on the conductive layer; step S4, repeating steps S2-S3 for several times on the infrared-irradiated conductive layer to obtain a substrate layer having several conductive layers stacked thereon, and performing the same process on the other side of the substrate layer to obtain a low-stress metallized plastic current collector.

[0008] Furthermore, the pre-treatment of the substrate layer in step S1 includes: introducing argon gas into the vacuum chamber, ionizing the argon gas by providing 800 W of power to the ion source, and then cleaning the surface of the substrate.

[0009] Furthermore, forming a conductive layer on the pretreated substrate layer in step S2 includes: introducing sputtering gas argon into a vacuum chamber to prepare the conductive layer by sputtering.

[0010] Furthermore, the amount of argon gas is 300-500 sccm, preferably 300, 400, 500 sccm, and the gas pressure of the vacuum chamber is 0.3-0.5 Pa, preferably 0.3, 0.4, 0.5 Pa.

[0011] Furthermore, the sputtering is dual rotating cathode, DC magnetron sputtering; the power is 1Kw to 15Kw, preferably 1, 3, 5, 8, 10, 12, 15Kw.

[0012] Furthermore, the infrared irradiation treatment of the conductive layer in step S3 includes: the power of the infrared irradiation is 3000-5800W, preferably 3000, 3500, 4000, 4500, 5000, 5500, 5800W, the radiation peak λmax is 0.9-1μm, the distance between the workpiece and the radiation source is 50-200mm, preferably 50, 100, 150, 200mm, and the radiation time is 5-200s, preferably 5, 10, 20, 50, 80, 100, 150, 200s.

[0013] Furthermore, in step S4, the number of the single-sided conductive layer is 1 to 20 layers, preferably 1, 2, 3, 5, 7, 9, 15, or 20 layers.

[0014] In another aspect, the present invention further provides a low-stress metallized plastic current collector prepared by the method described above, wherein the low-stress metallized plastic current collector comprises a substrate layer and a conductive layer irradiated by infrared disposed on at least one side.

[0015] Furthermore, the substrate layer is any one of biaxially oriented polypropylene film, cast polypropylene film, polyethylene terephthalate film, polyimide film, and polyethylene naphthalate film; the thickness of the substrate layer is 3 to 20 μm, preferably 3, 5, 7, 10, 15, or 20 μm.

[0016] Furthermore, the conductive layer is made of metal material, including any one or a combination of multiple materials selected from aluminum, copper, nickel, titanium, silver, gold, cobalt, chromium, molybdenum, tungsten, and stainless steel.

[0017] The beneficial effect of the present invention is that the low-stress metallized plastic current collector and the preparation method thereof utilize infrared radiation to perform heat treatment on the conductive layer, and the atoms in the conductive layer exchange energy through lattice vibration to heal some dislocations, thereby reducing the internal stress of the film; at the same time, when the atoms in the conductive layer diffuse on the surface, defects such as vacancies and gaps therein are eliminated, causing the volume to shrink to release the residual internal stress in the conductive layer, and ultimately increasing the bonding force between the conductive layer and the substrate layer, enhancing the electrolyte resistance of the metallized plastic current collector, and improving the cycle life of the new energy battery.

[0018] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention are realized and obtained by the structures particularly pointed out in the description and the drawings.

[0019] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 A schematic structural diagram of a low-stress metallized plastic current collector according to some embodiments is shown.

[0022] In the figure:

[0023] Base material layer 1, conductive layer 2. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] The preparation methods of the metallized plastic current collector conductive layer can be selected from evaporation, sputtering, water electroplating, etc., but the problem of stress generation is inevitable.

[0026] Preparation by evaporation plating process: During the formation of the metal conductive layer, the vaporized gas phase atoms deposited on the substrate have high kinetic energy, and the thermal radiation generated from the evaporation source causes the film temperature to rise. When the deposition process is completed and the film cools to the ambient temperature, the atoms gradually become immobile. The critical criterion for whether the atoms inside the film can move is the recrystallization temperature. Thermal contraction below the recrystallization temperature is the cause of stress. At the same time, when the film thickness continues to increase and crystallization occurs, the internal stress will also increase sharply.

[0027] Preparation by magnetron sputtering process: The sputtered ions sputtered onto the substrate during magnetron sputtering have a certain amount of energy, which is 1-2 orders of magnitude greater than the energy during vacuum evaporation. Therefore, more defects such as vacancies or interstitial atoms will be formed during film formation, increasing the volume of the film. In addition, the accelerated ions or accelerated neutral atoms during the sputtering process often impact the film with very high energy. In addition to being captured by the film as impurities, the atoms on the surface of the film also move inward, causing the volume of the film to increase, forming compressive stress in the film.

[0028] Preparation by water electroplating process: When the electrodeposited metal forms crystals, the grain aggregates or part of the grain aggregates grow laterally from different nucleation centers, which will generate internal stress. When the grain aggregation or other growth processes cause dislocations in the directional arrangement, the stress field around the dislocation increases, which will promote the increase of internal stress in some way. The nature of the stress depends on the orientation of the dislocation arrangement.

[0029] Specifically, if the stress in the film cannot be released through plastic deformation of the substrate or film, when it accumulates to a certain value, the film will crack or even peel off. In fact, it is often observed during the coating process that the peeled film curls or the oxide film peels off only in a micro-area, indicating that there is a stress gradient and micro-area stress concentration in the film.

[0030] In this embodiment, specifically, since the uniformity of the film formed by sputtering is better than that of the film formed by evaporation, water electroplating, etc., the sputtering method is preferred in this embodiment. At the same time, the sputtering method can adopt alternating current (AC) magnetron sputtering, direct current (DC) magnetron sputtering, and radio frequency (RF) magnetron sputtering. Since the conductive layer is a conductor, direct current (DC) magnetron sputtering is preferred.

[0031] Preliminary preparation: In the chamber of the winding magnetron sputtering coating machine, place the processed substrate layer on the unwinding roller of the unwinding chamber and wind it onto the winding roller; at the same time, place the required target materials Z1, Z2, Z3, Z4, Z5, etc. on the corresponding cathode target positions of chambers C1, C2, C3, C4, C5, etc. Chambers C1, C2, C3, C4, C5 are coating chambers, and there are corresponding infrared irradiation chambers in the middle of adjacent chambers. In addition, adjust the distance from the target to the substrate surface to 10 cm; close all chamber doors, turn on the front pump and molecular pump in turn, and wait until the vacuum degree of the chamber reaches 5×10 -4 When the pressure drops to 0.05 Pa, fill in process gas until the process vacuum is reached, open the cathode and drive roller to start coating, and control the winding speed at 5-12 m / min.

[0032] Step S1:

[0033] Argon gas is introduced into the vacuum chamber, and the argon gas is ionized by providing 800 W of power to the ion source, thereby cleaning the surface of the substrate;

[0034] Step S2:

[0035] A sputtering gas argon with a purity of not less than 99.99% is introduced into the chamber C1, the argon amount is 400 sccm, and the chamber pressure is stabilized at 0.3 Pa. A conductive layer A1 of a certain thickness is formed on the base film using the Z1 target material through a dual rotating cathode and DC magnetron sputtering method. The composition of A1 is the same as the structural material shown in the sputtering target Z1 target material; the dual rotating cathode and DC magnetron sputtering power is 1Kw~15Kw.

[0036] Step S3:

[0037] Near infrared irradiation uses a high-power halogen-filled tungsten emitter imported from Germany, a selected high-efficiency gold reflector, a power of 3000-5800W, a radiation peak λmax0.9-1μm, and a distance of 50-200mm between the workpiece and the radiation source. After the above infrared irradiation equipment is installed at the corresponding position of the film layer, infrared irradiation is carried out for 5s-200s.

[0038] Step S4:

[0039] Repeat steps S2-S3 several times for the infrared irradiated conductive layer to obtain a substrate layer with several conductive layers stacked thereon, and perform the same process on the other side of the substrate layer to obtain a low-stress metallized plastic current collector.

[0040] Film adhesion test method:

[0041] The detailed steps of the 180° peel test are as follows:

[0042] 1. Preparation: First, prepare the required test equipment and ensure that the test machine is in normal working condition. Select an appropriate peeling angle (180°) for the test. Cut a single-layer coated tape sample of appropriate size, ensuring that its adhesive surface and stretch surface correspond to the selected peeling angle.

[0043] 2. Bonding of tape to substrate: Prepare a long steel plate as the substrate for the tape. Make sure the surface of the steel plate is flat and clean. Bond the adhesive side of the single-layer coated tape to the surface of the steel plate. Use a 4.5lb roller to fully compact the tape to ensure good bonding. Leave the bonded tape and steel plate for a while to allow them to rest to ensure that the bond between the tape and the substrate is fully stable.

[0044] 3. Test machine settings: Clamp the two ends of the peeled portion of the label sample between the upper and lower clamps of the test machine, so that the longitudinal axis of the peeled portion of the sample coincides with the center line of the upper and lower clamps. Turn on the instrument, and the unpeeled portion is in a "T-shape" with the stretching direction.

[0045] 4. Define test conditions: Set test conditions such as peeling speed, peeling angle and test temperature according to test requirements to ensure that the test results accurately reflect the true performance of the material.

[0046] 5. Test: Click Test, and the system will automatically count the force required during the peeling process. Read data every 10 mm in the middle of the test strip, and read at least 5 data. Take the average value of the read data.

[0047] 6. Data analysis: After obtaining the peel force, ignore the value obtained when the first 25mm adhesive tape is mechanically peeled, and use the average force value obtained by the next 50mm adhesive tape as the peel force and convert it into peel strength. The number of samples in each group is not less than 3, and the test results are represented by the arithmetic mean of the peel strength in N / cm.

[0048] 7. Cleaning and preparation: Use a wiping material dipped in a cleaning agent to clean the test board, then wipe it dry with a clean absorbent gauze. Repeat this process for more than three times until the working surface of the board is clean after visual inspection. After cleaning, proceed to the next step.

[0049] Through the above steps, a 180° peel test can be completed to evaluate the adhesion strength of the material and its performance under different conditions.

[0050] Electrolyte immersion experiment: The metallized plastic current collector was immersed in an electrolyte containing 1000 ppm water for 120 hours and then the adhesion was tested.

[0051] In this embodiment, specifically, after adjusting and modifying the parameters, comparative examples and embodiments 1-6 were obtained, and film adhesion tests and electrolyte immersion experiments were performed. The results are shown in Table 1 below.

[0052] Table 1

[0053]

[0054]

[0055] In the present embodiment, specifically, it can be seen from Examples 1 to 5 that as the number of film layers increases and the infrared irradiation time increases, the adhesion between the conductive layer and the substrate is significantly improved; it can be seen from Example 6 that excessively long periods of infrared irradiation may cause fatigue aging of the film, and impurities remaining in the vacuum chamber may react with the film, thereby causing a decrease in adhesion.

[0056] Specifically, when an object that matches infrared rays is irradiated by infrared rays with continuously changing wavelengths, its molecules and atoms absorb radiation energy of certain wavelengths, and their vibrations and rotations accelerate, which not only causes energy level transitions from the ground state to the excited state, but also enhances the amplitude of various motions centered on the equilibrium position, increases the dipole moment (the product of the center distance of the positive and negative charges and the charge carried by the center of the charge), and increases the internal energy of the particles. The macroscopic reflection of the intensified motion of particles in the microscopic structure is the increase in the temperature of the object, so the object heats up quickly after absorbing infrared radiation energy. The energy of infrared rays is expressed in wave numbers, not wavelength or frequency. When cm is used as the unit of wavelength, the wave number is defined as the reciprocal of the wavelength. The wavelength of short-wave infrared is 0.78 to 2 μm (the wave number is 12820 to 5000 cm -1 ); mid-wave infrared wavelength 2~4μm (wave number 5000~2500cm -1 ); long-wave infrared wavelength 4 ~ 1000μm (wave number 2500 ~ 10cm -1 ). It can be seen that the shorter the wavelength, the greater its energy. Among the three types of infrared rays, the energy of the short wave is greater. The preferred short wave infrared wavelength is 0.78 to 2 μm.

[0057] like Figure 1 As shown, at least one embodiment provides a low-stress metallized plastic current collector, which is prepared by the method described above. The low-stress metallized plastic current collector includes a substrate layer and a conductive layer irradiated by infrared on at least one side.

[0058] Specifically, the substrate layer is any one of biaxially oriented polypropylene film (OPP), cast polypropylene film (CPP), polyethylene terephthalate film (PET), polyimide film (PI), and polyethylene naphthalate film (PEN); the thickness of the substrate layer is 3 to 20 μm.

[0059] Specifically, the conductive layer is made of metal material, including any one or a combination of multiple materials selected from aluminum, copper, nickel, titanium, silver, gold, cobalt, chromium, molybdenum, tungsten, and stainless steel.

[0060] In summary, the low-stress metallized plastic current collector and its preparation method of the present invention utilize infrared radiation to perform heat treatment on the conductive layer. The atoms in the conductive layer exchange energy through lattice vibration, heal some dislocations, and thus reduce the internal stress of the film. At the same time, when the atoms in the conductive layer diffuse on the surface, defects such as vacancies and gaps therein are eliminated, causing the volume to shrink to release the residual internal stress in the conductive layer, thereby ultimately increasing the bonding force between the conductive layer and the substrate layer, enhancing the electrolyte resistance of the metallized plastic current collector, and improving the cycle life of the new energy battery.

[0061] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.

[0062] In the several embodiments provided in this application, it should be understood that the disclosed systems, devices and methods can be implemented in other ways. The device embodiments described above are only schematic. For example, the division of the units is only a logical function division. There may be other division methods in actual implementation. For example, multiple units or components can be combined or integrated into another system, or some features can be ignored or not executed.

[0063] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing a low-stress metallized plastic current collector, It is characterized in that The steps include: Step S1, pre-treating the substrate layer; Step S2, forming a conductive layer on the pretreated substrate layer; Step S3, performing infrared radiation treatment on the conductive layer; Step S4, repeating steps S2-S3 for several times on the infrared irradiated conductive layer to obtain a substrate layer with several conductive layers stacked thereon, and performing the same process on the other side of the substrate layer to obtain a low-stress metallized plastic current collector.

2. The preparation method according to claim 1, It is characterized in that The pretreatment of the substrate layer in step S1 includes: introducing argon gas into the vacuum chamber, ionizing the argon gas by providing 800W of power to the ion source, and then cleaning the surface of the substrate.

3. The preparation method according to claim 1, It is characterized in that The step S2 of forming a conductive layer on the pretreated substrate layer includes: introducing a sputtering gas, argon, into a vacuum chamber to prepare the conductive layer by sputtering.

4. The preparation method according to claim 3, It is characterized in that The amount of argon gas is 300-500 sccm, and the gas pressure of the vacuum chamber is 0.3-0.5 Pa.

5. The preparation method according to claim 4, It is characterized in that The sputtering is double rotating cathode, DC magnetron sputtering; the power is 1Kw to 15Kw.

6. The preparation method according to claim 1, It is characterized in that The infrared irradiation treatment of the conductive layer in step S3 includes: the power of the infrared irradiation is 3000-5800W, the radiation peak λmax is 0.9-1μm, the distance between the workpiece and the radiation source is 50-200mm, and the irradiation time is 5-200s.

7. The preparation method according to claim 1, It is characterized in that In the step S4, the number of the single-side conductive layer is 1 to 20 layers, and the thickness of a single layer is 50 nm to 1 μm.

8. A low stress metallized plastic current collector, It is characterized in that The low-stress metallized plastic current collector is prepared by the method according to any one of claims 1 to 7, and comprises a substrate layer and a conductive layer irradiated by infrared radiation disposed on at least one side.

9. The low stress metallized plastic current collector according to claim 8, It is characterized in that The substrate layer is any one of a biaxially oriented polypropylene film, a cast polypropylene film, a polyethylene terephthalate film, a polyimide film, and a polyethylene naphthalate film; The thickness of the substrate layer is 3 to 20 μm.

10. The low stress metallized plastic current collector according to claim 8, It is characterized in that The conductive layer is made of metal material, including any one or a combination of multiple groups of aluminum, copper, nickel, titanium, silver, gold, cobalt, chromium, molybdenum, tungsten, and stainless steel.