Integrated light-assisted secondary battery
By adopting a layer-by-layer stacking structure of bifunctional electrode materials in light-assisted secondary batteries, the problems of low luminous efficiency and poor dynamic performance of photoinduced effects in the existing technology are solved, achieving efficient solar energy storage and conversion, and improving Battery performance and application value.
Patent Information
- Application Number
- CN202410753430.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-15
AI Technical Summary
Existing photo-assisted secondary batteries only have positive electrode materials, low photoluminescence efficiency, complex and high-cost preparation methods, and poor kinetic properties, resulting in low conversion efficiency, which limits their wide application and the development of integrated devices.
Bifunctional electrode materials are used, including electron transmission material layer, photosensitive material layer and energy storage active material layer. They are prepared by physical deposition and doctor blade coating methods to form a layer-by-layer stacking structure to realize the absorption, conversion and storage of solar energy, and improve the electron- Generation and transport of hole pairs.
It significantly improves the kinetic performance and cycle performance of the battery, increases the specific capacity and energy density, achieves excellent rate performance and stable operation, has low cost, flexible design, and has greater application value.
Smart Images

Figure CN118782871A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of optical energy storage, and specifically refers to an integrated optically assisted secondary battery, including optical storage sodium ion batteries and optical storage lithium ion batteries and other systems. Background Art
[0002] In this era of increasingly depleted fossil fuel resources, the use of solar energy as a renewable energy source has attracted great attention from many governments and industries. Solar energy is a huge resource - the earth's surface receives about 3×10 24 If only 0.1% of the Earth’s surface were covered by collectors that converted solar energy with 10% efficiency, then all of the world’s current annual energy needs (3×10 20 J / year) will be met. However, due to the intermittent nature of solar power generation, the excess energy can only be wasted and cannot be effectively stored. Therefore, we need to combine the electrochemical energy storage system with the photovoltaic system, integrate the design, store the energy converted by the photovoltaic system, promote the efficient application of clean new energy, and meet the energy use needs of building exterior walls, mobile transportation equipment, and various outdoor independent energy use scenarios.
[0003] When facing the demand for large-scale energy storage, secondary batteries have received widespread attention. For example, sodium-ion batteries have the advantages of abundant resources and low cost; lithium-ion batteries have the advantages of small size and high energy density. Therefore, combining them with photovoltaic systems to assemble integrated light-assisted secondary batteries will have great potential. Patent CN117174815A discloses a method for preparing a light-assisted lithium secondary battery MOF-loaded perovskite composite electrode material, and patent CN117174834A discloses a method for preparing a light-assisted lithium secondary battery positive electrode Co-CN@rGO composite material. Although the above two prior arts disclose light-assisted secondary batteries, they have certain defects. Specifically, on the one hand, the prepared materials are only positive electrode materials, and they are all used in lithium-ion batteries, which limits their wide application to a certain extent; on the other hand, the positive electrode materials of the photoinduced effect are all obtained by chemical compounding. The luminous efficiency of the photosensitive material after compounding is greatly reduced, and the preparation method is complicated and the synthesis cost is high. In addition, the photo-assisted secondary battery electrode materials in the above-mentioned prior art have poor kinetic performance (mainly manifested in low capacity improvement, large impedance, poor stability and poor rate performance), which leads to low conversion efficiency and seriously restricts the assembly and development of integrated devices. Summary of the invention
[0004] In order to solve the technical problems of intermittent solar power generation and orderly use, as well as the technical problems that the light-assisted secondary batteries assembled in the prior art are expensive, bulky and inflexible, cycle under light, have poor rate performance and low conversion efficiency, the present invention proposes an integrated light-assisted secondary battery.
[0005] To achieve the above object, the technical solution of the present invention is implemented as follows:
[0006] An integrated light-assisted secondary battery includes a bifunctional electrode material, a pole piece, an electrolyte and a separator. The bifunctional electrode material has a layer-by-layer stacked structure consisting of an electron transport material layer, a photosensitive material layer and an energy storage active material layer, wherein the photosensitive material is a middle layer structure.
[0007] The above-mentioned integrated light-assisted secondary battery is a dual-electrode system that can simultaneously realize the absorption, conversion and storage of solar energy.
[0008] The electron transport material layer is composed of any one or more of TiO2, ZnO, SnO2, fullerene and their derivatives.
[0009] The photosensitive material layer is composed of any one or more of photosensitive semiconductor and photosensitive polymer materials.
[0010] Furthermore, the photosensitive semiconductor is composed of any one or more of cadmium selenide, cadmium sulfide, perovskite and metal oxide; wherein, further preferably, the metal oxide is vanadium pentoxide (V2O5).
[0011] Furthermore, the photosensitive polymer material is any one or more of azobenzene and stilbene derivatives, N719 dye and anthocyanin fluorescent dye.
[0012] The bifunctional electrode material is a bifunctional positive electrode material or a bifunctional negative electrode material. When the bifunctional electrode material is a bifunctional positive electrode material, the energy storage active material layer is composed of any one or a combination of layered oxides, Prussian blue compounds and polyanion compounds (containing metal ion substances such as lithium, sodium, potassium, magnesium, etc.). At this time, the corresponding negative electrode plate is composed of any one or a combination of carbon-based negative electrodes, conversion negative electrodes, metal negative electrodes (lithium, sodium, potassium, magnesium, zinc, tin, etc.) and alloyed negative electrodes.
[0013] When the bifunctional electrode material is a bifunctional negative electrode material, the energy storage active material layer is composed of any one or a combination of carbon-based negative electrodes, conversion negative electrodes, metal negative electrodes (lithium, sodium, potassium, magnesium, zinc, tin, etc.) and alloyed negative electrodes. At this time, the corresponding positive electrode plate is composed of any one or a combination of layered oxides, Prussian blue compounds and polyanion compounds (containing metal ion substances such as lithium, sodium, potassium, magnesium, etc.).
[0014] Furthermore, the layered oxide is any one or more combinations of sodium nickel iron manganate, sodium nickel manganate and lithium nickel cobalt manganate; the Prussian blue compound is manganese iron-based Prussian blue; the polyanion compound is any one or more of lithium iron phosphate, sodium iron phosphate, sodium iron pyrophosphate, sodium vanadium phosphate, sodium fluorophosphate and sodium iron sulfate.
[0015] The above-mentioned carbon-based negative electrode is soft carbon, hard carbon or graphite carbon; the metal negative electrode is lithium, sodium, potassium, magnesium, zinc, tin metal sheet; the conversion negative electrode is FeS2 or FeS; the alloy negative electrode is Sn4P3, SnP 0.94 , SnP3 or Sn2S3.
[0016] The electrolyte is a soluble salt organic solution, and the diaphragm is polyethylene, polypropylene microporous membrane, glass fiber diaphragm, polyacrylonitrile diaphragm or a composite diaphragm thereof; or it is a gel or solid electrolyte with ion conductivity.
[0017] Furthermore, the diaphragm is a polypropylene microporous membrane or a glass fiber diaphragm.
[0018] The soluble salt organic solution is any one of a soluble sodium salt organic solution, a soluble lithium salt organic solution, a soluble zinc salt organic solution and a soluble aluminum salt organic solution.
[0019] Furthermore, the soluble salt organic solution is a soluble sodium salt organic solution or a soluble lithium salt organic solution.
[0020] Furthermore, the soluble lithium salt organic solution is LiPF6+EC / DMC or LiPF6+DMC / EC / EMC, and the soluble sodium salt organic solution is NaClO4+EC / PC / FEC, NaClO4+EC / DEC / FEC, NaFSI+EC / DEC, NaPF6+EC / DEC, NaPF6+EC / DMC or NaBF4+DGM.
[0021] The above-mentioned bifunctional electrode materials are prepared in a layered form by physical deposition and scraping, which is more conducive to the electron-hole pairs generated by the photosensitive material under the action of light to participate in the redox reaction of the energy storage active material. The bifunctional electrode material has the functions of absorbing and converting solar energy at the same time, and its layered structure can form a progressive energy level relationship, which is conducive to the generation and rapid transmission of electron-hole pairs under light.
[0022] The preparation method of the above-mentioned bifunctional electrode material comprises the following specific steps:
[0023] (1) Roll-coating the electron transport material solution onto the conductive glass, and then performing an annealing treatment;
[0024] (2) placing the photosensitive material in a solvent and fully dissolving it to obtain a solution;
[0025] (3) fully dipping, rolling or spin coating the solution obtained in step (2) on the conductive glass plate obtained in step (1), and drying;
[0026] (4) uniformly mixing the energy storage active material, the conductive agent, the binder and the dispersant to form a uniform slurry;
[0027] (5) Applying the slurry obtained in step (4) onto the conductive glass obtained in step (3) to obtain a bifunctional electrode material.
[0028] In the method for preparing the bifunctional electrode material, the annealing temperature in step (1) is 150-450° C., and the annealing time is 15-60 min.
[0029] In the preparation method of the bifunctional electrode material, the dipping temperature in step (3) is 25-35° C. and the time is 12-24 hours.
[0030] In the preparation method of the bifunctional electrode material, the conductive agent in step (4) is any one or more of acetylene black, Super P Li, Ketjen black or carbon nanotubes; the binder is any one or more of polyvinylidene fluoride, polyacrylic acid, hydroxymethyl cellulose, sericin, polyetherimide, polyimide, polylactic acid, polyethylene oxide; and the dispersant is any one or more of 1-methyl-2-pyrrolidone, dimethyl sulfoxide, NN-dimethylformamide, NN-dimethylacetamide, acetone, anhydrous ethanol and deionized water.
[0031] The beneficial effects produced by the present invention are:
[0032] (1) The present invention constructs an integrated light-storage system and integrates the design of an integrated light-assisted secondary battery device to achieve the collection and storage of solar energy. In the dark state, this system is a secondary battery in its original state; under light, due to the effect of the photosensitive material, the electron-hole pairs generated by absorbing sunlight can be separated and transferred to the greatest extent, thereby participating in the redox reaction of the energy storage active material, greatly improving the kinetic performance of the battery. During the illumination process, not only the specific capacity of the battery is effectively improved, but the battery can also operate stably under alternating darkness and light, with excellent cycle performance and rate performance. The integrated light-assisted secondary battery constructed by the present invention can effectively improve the energy density of the system under illumination. Taking a light-assisted sodium ion battery prepared with titanium dioxide / cadmium selenide / sodium iron pyrophosphate as a dual-functional positive electrode and metallic sodium as a negative electrode as an example, when illuminated, 1C (1C=119mAg -1 ) density, the discharge median voltage is 3.01 V and the specific capacity reaches 118.9 mAh g -1The battery discharge energy density reaches 344.1Wh / kg (1C = 119mA g -1 , the energy density is calculated based on the mass of the positive electrode active material); in the dark, 1C (1C = 119mA g -1 ) density, the discharge median voltage is 2.93 V and the specific capacity reaches 84.7 mAh g -1 The battery discharge energy density reaches 239.1Wh / kg (1C = 119mA g -1 The energy density is calculated based on the mass of the positive electrode active material). Compared with the dark state, the energy density is increased by 105Wh / kg. In addition, at 1, 2, 3, 5, and 8C rates, the light discharge specific capacity is 115.8, 106.1, 100.6, 89.2, and 75.4mAh g, respectively. -1 ; The dark discharge specific capacities are 93.2, 79.5, 70.1, 56.2, and 41.3 mAh g -1 ; After 240 cycles of alternating dark and light cycles at 5C, the light capacity increased by 30 mAh g compared to the dark capacity -1 It has excellent rate performance and cycle performance.
[0033] (2) The present invention achieves the highest overall system efficiency of 4.34% for integrated light-assisted secondary batteries reported so far. When converting the same amount of light energy, it can store and release the obtained energy to the maximum extent, and has greater application value in actual life scenarios.
[0034] (3) The integrated light-assisted secondary battery constructed by the present invention has the advantages of small size, high design flexibility, low cost, simple preparation, high specific capacity and good cycle performance. Under light, the dynamics of the battery are greatly improved, the specific capacity of the battery is increased, and the battery can be cycled stably. Under alternating darkness and light, the battery can also operate stably, with excellent cycle performance and rate performance, showing high technical application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0036] Figure 1 This is a comparison diagram of the dark illumination charge and discharge curves of the light-assisted sodium ion battery prepared in Example 1 of the present invention.
[0037] Figure 2This is a comparison chart of the dark illumination rate performance of the light-assisted sodium-ion battery prepared in Example 1 of the present invention.
[0038] Figure 3 This is a comparison chart of the dark-illumination cycle performance of the light-assisted sodium-ion battery prepared in Example 1 of the present invention.
[0039] Figure 4 It is the overall system efficiency of the integrated light-assisted secondary battery of the present invention.
[0040] Figure 5 This is a comparison diagram of the dark illumination charge and discharge curves of the light-assisted lithium-ion battery prepared in Example 2 of the present invention.
[0041] Figure 6 This is a comparison chart of the dark-light cycle performance of the light-assisted lithium-ion battery prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0042] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] Example 1
[0044] 1. The steps for preparing the titanium dioxide / cadmium selenide / sodium iron pyrophosphate bifunctional positive electrode material of this embodiment are as follows:
[0045] (1) Se powder (0.0256 g), tributylphosphine (0.58 mL) (TBP), and 1-octadecene (1.73 mL) (ODE) were mixed and placed in a sample tube for ultrasonic dissolution;
[0046] (2) CdO (0.0256 g), stearic acid (0.2275 g), and ODE (2.53 mL) were placed in a three-necked flask and heated at 220°C in an argon atmosphere to dissolve until a transparent yellow color was obtained, and then cooled to room temperature;
[0047] (3) octadecylamine (1.5 g) (ODA) and tri-n-octylphosphine oxide (0.5 g) (TOPO) were added to step (2) and heated to 280° C.;
[0048] (4) injecting step (1) into step (3) for 2 minutes, then cooling with cold water to 60° C. to obtain a crude CdSe product;
[0049] (5) Purifying the product of step (4) with anhydrous ethanol and chloroform, and finally dissolving CdSe with chloroform to form a CdSe solution with a concentration of 1 M;
[0050] (6) Dissolve TiO2 in acetic acid, and roll-coat the resulting 12.5 M TiO2 solution onto FTO, followed by annealing at 150°C for 15 min;
[0051] (7) soaking (6) in (5) for 12 h at a temperature of 25°C;
[0052] (8) Place (7) on a scraper, mix the energy storage active material sodium iron pyrophosphate, Super P Li, and polyvinylidene fluoride in a mass ratio of 80:10:10, use 1-methyl-2-pyrrolidone as a dispersant, mix the above mixture evenly into a slurry and apply it to TiO2 / CdSe, and after vacuum drying at 60°C, obtain a titanium dioxide / cadmium selenide / sodium iron pyrophosphate bifunctional positive electrode material with a side length of 1 cm.
[0053] 2. A method for preparing an integrated light-assisted secondary battery, the specific steps are as follows:
[0054] The bifunctional positive electrode material of titanium dioxide / cadmium selenide / sodium iron pyrophosphate is used as the positive electrode, the sodium metal sheet is used as the negative electrode (diameter is 16mm), the glass fiber membrane (Whatman GF / D) is used as the separator, and 1M NaClO4 dissolved in EC:PC (volume ratio is 1:1) (5wt.% FEC additive) is used as the electrolyte. It is packaged into a stacked battery with FTO as the shell.
[0055] The light-assisted sodium-ion battery assembled by the above process was charged and discharged at room temperature. Its charge and discharge curve, rate and cycle performance are shown in Figure 2. Figure 1-3 shown.
[0056] Figure 1 This is a comparison chart of the dark illumination charge and discharge curves of the light-assisted sodium ion battery prepared in Application Example 1 of the present invention. When illuminated, 1C (1C = 119mAg -1 ) density, the discharge median voltage is 3.01 V and the specific capacity reaches 118.9 mAh g -1 The battery discharge energy density reaches 344.1Wh / kg (1C = 119mAg -1 , the energy density is calculated based on the mass of the positive electrode active material); in the dark, 1C (1C = 119mAg -1 ) density, the discharge median voltage is 2.93 V and the specific capacity reaches 84.7 mAh g -1 The battery discharge energy density reaches 239.1Wh / kg (1C = 119mAg -1 , the energy density is calculated based on the mass of the positive electrode active material). Compared with the dark state, the energy density is increased by 105Wh / kg.
[0057] Figure 2 This is a comparison chart of the dark illumination rate performance of the light-assisted sodium ion prepared in Application Example 1 of the present invention. At 1, 2, 3, 5, and 8C rates, the illumination discharge specific capacities are 115.8, 106.1, 100.6, 89.2, and 75.4 mAh g, respectively. -1 ; The dark discharge specific capacities are 93.2, 79.5, 70.1, 56.2, and 41.3 mAh g -1 .
[0058] Figure 3 This is a comparison chart of the dark-light cycle performance of the light-assisted sodium ion battery prepared in Example 1 of the present invention. After 240 cycles of dark-light alternation at 5C, the light capacity increased by 30 mAh g compared with the dark capacity. -1 about.
[0059] The overall efficiency of the light-assisted sodium ion battery system prepared in Example 1 of this embodiment is calculated, and the result is as follows: Figure 4 The calculation formula is:
[0060] Where U is the battery voltage, t charge is the lighting time during light charging (h), A PV is the effective surface area of the photovoltaic device (cm -2 ), P in is the optical power density (mW cm -2 ) can be obtained by calculation, Figure 4 The overall efficiency is calculated at 1, 2, 3, 5, and 8C rates respectively, and the maximum overall efficiency is 4.34% at 8C.
[0061] Example 2
[0062] 1. The steps for preparing the titanium dioxide / cadmium selenide / lithium iron phosphate bifunctional positive electrode material of this embodiment are as follows:
[0063] (1) Se powder (0.0256 g), tributylphosphine (0.58 mL) (TBP), and 1-octadecene (1.73 mL) (ODE) were mixed and placed in a sample tube for ultrasonic dissolution;
[0064] (2) CdO (0.0256 g), stearic acid (0.2275 g), and ODE (2.53 mL) were placed in a three-necked flask and heated at 220°C in an argon atmosphere to dissolve until a transparent yellow color was obtained, and then cooled to room temperature;
[0065] (3) octadecylamine (1.5 g) (ODA) and tri-n-octylphosphine oxide (0.5 g) (TOPO) were added to step (2) and heated to 280° C.;
[0066] (4) injecting step (1) into step (3) for 2 minutes, then cooling with cold water to 60° C. to obtain a crude CdSe product;
[0067] (5) Purifying the product of step (4) with anhydrous ethanol and chloroform, and finally dissolving CdSe with chloroform to form a CdSe solution with a concentration of 1 M;
[0068] (6) Dissolve TiO2 in acetic acid, and roll-coat the resulting 12.5 M TiO2 solution onto FTO, followed by annealing at 150°C for 15 min;
[0069] (7) soaking (6) in (5) for 24 hours at a temperature of 25°C;
[0070] (8) Place (7) on a scraper, mix the energy storage active material lithium iron phosphate, Super P Li, and polyvinylidene fluoride in a mass ratio of 80:10:10, use 1-methyl-2-pyrrolidone as a dispersant, mix the above mixture evenly into a slurry and apply it to TiO2 / CdSe, and then vacuum dry at 60°C to obtain a titanium dioxide / cadmium selenide / lithium iron phosphate bifunctional positive electrode material with a side length of 1 cm.
[0071] 2. A method for preparing an integrated light-assisted secondary battery, the specific steps are as follows:
[0072] The positive electrode is made of titanium dioxide / cadmium selenide / lithium iron phosphate bifunctional positive electrode material, the negative electrode is made of lithium metal sheet (diameter 16mm), the glass fiber membrane (Whatman GF / D) is used as the separator, and 1M LiPF6 dissolved in DMC:EC:EMC (volume ratio 1:1:1) is used as the electrolyte. It is packaged into a stacked battery with FTO as the shell.
[0073] The light-assisted lithium-ion battery assembled by the above process was subjected to charge and discharge tests at room temperature. Its charge and discharge curves and cycle performance are shown in Figure 2. Figure 5-6 shown.
[0074] Figure 5 This is a comparison diagram of the dark illumination charge and discharge curves of the light-assisted lithium-ion battery prepared in Application Example 2 of the present invention. When illuminated, 3C (1C = 170mA g -1 ) density, the discharge median voltage is 3.14 V and the specific capacity reaches 171.4 mAh g -1 The battery discharge energy density reaches 535.9Wh / kg (1C = 119mA g -1 , the energy density is calculated based on the mass of the positive electrode active material); in the dark, 1C (1C = 119mA g -1 ) density, the discharge median voltage is 3.10V and the specific capacity reaches 95.6mAh g -1The battery discharge energy density reaches 295.3Wh / kg (1C = 170mAg -1 , the energy density is calculated based on the mass of the positive electrode active material). Compared with the dark state, the energy density is increased by 240.6Wh / kg.
[0075] Figure 6 This is a comparison chart of the dark-light cycle performance of the light-assisted lithium-ion battery prepared in Example 2 of the present invention. After 56 cycles of dark-light alternation at 3C, the light capacity increased by 75 mAh g compared with the dark capacity. -1 about.
[0076] Example 3
[0077] 1. The steps for preparing the titanium dioxide / vanadium pentoxide / hard carbon dual-function negative electrode material of this embodiment are as follows:
[0078] (1) Dissolve TiO2 in acetic acid, and roll-coat the resulting 12.5M TiO2 solution onto FTO, followed by annealing at 450°C for 60 min;
[0079] (2) dissolving V2O5 in acetic acid to form a 5.5 M V2O5 solution, then rolling the solution onto TiO2 and annealing the solution at 150°C for 30 min;
[0080] (3) Place (2) on a scraper, mix the energy storage active material hard carbon, Super P Li, and polyvinylidene fluoride in a mass ratio of 80:10:10, use 1-methyl-2-pyrrolidone as a dispersant, mix the above mixture evenly into a slurry and apply it to TiO2 / V2O5, and after vacuum drying at 60°C, obtain a titanium dioxide / vanadium pentoxide / hard carbon bifunctional negative electrode material with a side length of 1 cm.
[0081] 2. A method for preparing an integrated light-assisted secondary battery, the specific steps are as follows:
[0082] Titanium dioxide / vanadium pentoxide / hard carbon bifunctional negative electrode material is used as the negative electrode, glass fiber membrane (Whatman GF / D) is used as the separator, and 1M NaPF6 dissolved in EC:DEC (volume ratio of 1:1) is used as the electrolyte. It is assembled with the positive electrode material sodium iron pyrophosphate and encapsulated into a stacked battery with FTO as the shell.
[0083] Example 4
[0084] 1. The steps for preparing the titanium dioxide / cadmium selenide / hard carbon bifunctional negative electrode material of this embodiment are as follows:
[0085] (1) Se powder (0.0256 g), tributylphosphine (0.58 mL) (TBP), and 1-octadecene (1.73 mL) (ODE) were mixed and placed in a sample tube for ultrasonic dissolution;
[0086] (2) CdO (0.0256 g), stearic acid (0.2275 g), and ODE (2.53 mL) were placed in a three-necked flask and heated at 220°C in an argon atmosphere to dissolve until a transparent yellow color was obtained, and then cooled to room temperature;
[0087] (3) octadecylamine (1.5 g) (ODA) and tri-n-octylphosphine oxide (0.5 g) (TOPO) were added to step (2) and heated to 280° C.;
[0088] (4) injecting step (1) into step (3) for 2 minutes, then cooling with cold water to 60° C. to obtain a crude CdSe product;
[0089] (5) Purifying the product of step (4) with anhydrous ethanol and chloroform, and finally dissolving CdSe with chloroform to form a CdSe solution with a concentration of 1 M;
[0090] (6) Dissolve TiO2 in acetic acid, and roll-coat the resulting 12.5 M TiO2 solution onto FTO, followed by annealing at 150°C for 15 min;
[0091] (7) soaking (6) in (5) for 24 hours at a temperature of 35°C;
[0092] (8) Place (7) on a scraper, mix the energy storage active material hard carbon, Super P Li, and polyvinylidene fluoride in a mass ratio of 80:10:10, use 1-methyl-2-pyrrolidone as a dispersant, mix the above mixture evenly into a slurry and apply it to TiO2 / CdSe, and after vacuum drying at 60°C, obtain a titanium dioxide / cadmium selenide / hard carbon bifunctional negative electrode material with a side length of 1 cm.
[0093] 2. A method for preparing an integrated light-assisted secondary battery, the specific steps are as follows:
[0094] Titanium dioxide / cadmium selenide / hard carbon bifunctional negative electrode material is used as the negative electrode, glass fiber membrane (Whatman GF / D) is used as the separator, and 1M NaPF6 dissolved in DMC:EC:EMC (volume ratio of 1:1:1) is used as the electrolyte. It is assembled with the positive electrode material sodium iron pyrophosphate and encapsulated into a stacked battery with FTO as the shell.
[0095] Example 5
[0096] 1. The steps for preparing the tin dioxide / CsPbBr3 perovskite / sodium iron pyrophosphate bifunctional positive electrode material of this embodiment are as follows:
[0097] (1) PbBr2 (0.069 g), octadecene (5 mL), oleic acid (0.5 mL), and oleylamine (0.5 mL) were placed in a three-necked flask, degassed at 120 °C for 1 h, then introduced with argon and heated to 200 °C to dissolve PbBr2;
[0098] (2) Cesium carbonate (0.0814 g), octadecene (4 mL), and oleic acid (0.25 mL) were placed in a three-necked flask, degassed at 120 °C for 1 h, then switched to argon gas, and heated to 150 °C to dissolve until all cesium carbonate reacted with oleic acid;
[0099] (3) Lower the temperature of (1) to 100°C and quickly transfer 0.4 mL of cesium oleate solution in (2) to the first flask;
[0100] (4) After 10 seconds of reaction, place the flask in a water bath to stop the reaction;
[0101] (5) using tert-butyl alcohol and n-hexane in the flask after the reaction to precipitate and centrifuge, and finally using n-hexane as a dispersant to dissolve the CsPbBr3 perovskite;
[0102] (6) SnCl 2. 2H2O (1.0159 g) and thiourea (338 mg) were mixed and then added with 30 mL of deionized water, stirred at room temperature for 36 h, centrifuged at 9000 rpm for 5 min, and the SnO2 quantum dot solution obtained after filtration was spin-coated on FTO at 2000 rpm for 30 s, annealed at 200 °C for 60 min;
[0103] (7) soaking (6) in (5) for 24 hours at a temperature of 35°C;
[0104] (8) Place (7) on a scraper, mix sodium iron pyrophosphate with Super P Li and polyvinylidene fluoride in a mass ratio of 80:10:10, use 1-methyl-2-pyrrolidone as a dispersant, mix the above mixture evenly into a slurry, coat it on SnO2 / CsPbBr3 perovskite, and obtain a tin dioxide / CsPbBr3 perovskite / sodium iron pyrophosphate bifunctional positive electrode material with a side length of 1 cm after vacuum drying at 60°C.
[0105] 2. A method for preparing an integrated light-assisted secondary battery, the specific steps are as follows:
[0106] The tin dioxide / CsPbBr3 perovskite / sodium iron pyrophosphate bifunctional cathode material is used as the cathode, hard carbon is used as the anode, glass fiber membrane (Whatman GF / D) is used as the separator, and 1M NaClO4 dissolved in EC:PC (volume ratio of 1:1) (5wt.% FEC additive) is used as the electrolyte. It is packaged into a stacked battery with FTO as the shell.
[0107] Example 6
[0108] 1. The steps for preparing the tin dioxide / CsPbBr3 perovskite / sodium nickel iron manganese oxide bifunctional positive electrode material of this embodiment are as follows:
[0109] (1) SnCl 2. 2H2O (1.0159 g) and thiourea (338 mg) were mixed and then added with 30 mL of deionized water, stirred at room temperature for 36 h, centrifuged at 9000 rpm for 5 min, and the SnO2 quantum dot solution obtained after filtration was spin-coated on FTO at 2000 rpm for 30 s and annealed at 200 °C for 60 min.
[0110] (2) Spin-coat a 1 M PbBr2 solution in DMF onto a SnO2 substrate at 2000 rpm for 30 s and dry at 90 °C for 60 min;
[0111] (3) Spin-coat a 0.07 M CsBr solution in methanol onto the PbBr2 film in (2) at 2000 rpm for 30 s and heat at 250 °C for 5 min;
[0112] (4) Repeat step (3) 4 times to obtain a CsPbBr3 perovskite film;
[0113] (5) Place (4) on a scraper, mix sodium nickel iron manganese oxide with Super P Li and polyvinylidene fluoride in a mass ratio of 80:10:10, use 1-methyl-2-pyrrolidone as a dispersant, mix the above mixture evenly into a slurry and apply it to the tin dioxide / CsPbBr3 perovskite, and after vacuum drying at 60°C, obtain a tin dioxide / CsPbBr3 perovskite / sodium nickel iron manganese oxide bifunctional positive electrode material with a side length of 1 cm.
[0114] 2. A method for preparing an integrated light-assisted secondary battery, the specific steps are as follows:
[0115] The positive electrode is made of tin dioxide / CsPbBr3 perovskite / sodium nickel iron manganese oxide bifunctional positive electrode material, the negative electrode is made of sodium metal sheet (diameter 16mm), the glass fiber membrane (Whatman GF / D) is used as the separator, and 1M NaClO4 dissolved in EC:PC (volume ratio 1:1) (5wt.% FEC additive) is used as the electrolyte. It is packaged into a stacked battery with FTO as the shell.
[0116] Example 7
[0117] 1. The preparation steps of the PCBM / N719 dye / manganese iron-based Prussian blue dual-functional positive electrode material of this embodiment are as follows:
[0118] (1) PCBM solution (18 mg mL -1 in CB, the solvent was toluene) was spin-coated on FTO at 4000 rpm and annealed at 90 °C for 30 min;
[0119] (2) (1) was immersed in a 0.5 mM N719 dye solution (solvent: a mixture of acetonitrile and tert-butanol in a volume ratio of 1:1) for 24 h at a temperature of 35°C;
[0120] (3) Place (2) on a scraper, mix ferromanganese-based Prussian blue with Super P Li and polyvinylidene fluoride in a mass ratio of 80:10:10, use 1-methyl-2-pyrrolidone as a dispersant, mix the above mixture evenly into a slurry and apply it to fullerene / N719 dye, and then vacuum dry at 60°C to obtain a PCBM / N719 dye / ferromanganese-based Prussian blue bifunctional positive electrode material with a side length of 1 cm.
[0121] 2. A method for preparing an integrated light-assisted secondary battery, the specific steps are as follows:
[0122] PCBM / N719 dye / manganese iron-based Prussian blue bifunctional cathode material is used as the cathode, sodium metal sheet is used as the anode (diameter is 16mm), glass fiber membrane (Whatman GF / D) is used as the separator, and 1M NaClO4 dissolved in EC:PC (volume ratio is 1:1) (5wt.% FEC additive) is used as the electrolyte. It is packaged into a stacked battery with FTO as the shell.
[0123] Example 8
[0124] 1. The preparation steps of the PCBM / N719 dye / FeS2 dual-functional negative electrode material of this embodiment are as follows:
[0125] (1) PCBM solution (18 mg mL -1 in CB, the solvent was toluene) was spin-coated on FTO at 4000 rpm and annealed at 90 °C for 30 min;
[0126] (2) (1) was immersed in a 0.5 mM N719 dye solution (solvent: a mixture of acetonitrile and tert-butanol in a volume ratio of 1:1) for 24 h at a temperature of 35°C;
[0127] (3) Place (2) on a scraper, mix FeS2 with Super P Li and polyvinylidene fluoride in a mass ratio of 80:10:10, use 1-methyl-2-pyrrolidone as a dispersant, mix the above mixture evenly into a slurry and apply it to N719 dye, and after vacuum drying at 60°C, obtain a PCBM / N719 dye / FeS2 bifunctional negative electrode material with a side length of 1 cm.
[0128] 2. A method for preparing an integrated light-assisted secondary battery, the specific steps are as follows:
[0129] The PCBM / N719 dye / FeS2 bifunctional negative electrode material was used as the negative electrode, the glass fiber membrane (Whatman GF / D) was used as the separator, 1M NaClO4 dissolved in EC:PC (volume ratio of 1:1) (5wt.% FEC additive) was used as the electrolyte, and it was assembled with the positive electrode material sodium iron pyrophosphate and packaged into a stacked battery with FTO as the shell.
[0130] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An integrated light-assisted secondary battery, comprising a bifunctional electrode material, a pole piece, an electrolyte and a diaphragm, characterized in that: The bifunctional electrode material has a layer-by-layer stacking structure, consisting of an electron transport material layer, a photosensitive material layer and an energy storage active material layer, wherein the photosensitive material is a middle layer structure.
2. The integrated light-assisted secondary battery according to claim 1, characterized in that: The electron transport material layer is composed of any one or more of TiO2, ZnO, SnO2, fullerene and their derivatives.
3. The integrated light-assisted secondary battery according to claim 1, characterized in that: The photosensitive material layer is composed of any one or more of photosensitive semiconductor and photosensitive polymer materials.
4. The integrated light-assisted secondary battery according to claim 3, characterized in that: The photosensitive semiconductor is composed of any one or more of cadmium selenide, cadmium sulfide, perovskite and metal oxide; the photosensitive polymer material is composed of any one or more of azobenzene derivatives, stilbene derivatives, N719 dye and anthocyanin fluorescent dye.
5. The integrated light-assisted secondary battery according to any one of claims 1 to 3, characterized in that: When the bifunctional electrode material is a bifunctional positive electrode material, the energy storage active material layer is composed of any one or a combination of layered oxides, Prussian blue compounds and polyanion compounds. At this time, the corresponding negative electrode plate is composed of any one or a combination of carbon-based negative electrodes, conversion negative electrodes, metal negative electrodes and alloyed negative electrodes.
6. The integrated light-assisted secondary battery according to any one of claims 1 to 3, characterized in that: When the bifunctional electrode material is a bifunctional negative electrode material, the energy storage active material layer is composed of any one or a combination of carbon-based negative electrodes, conversion negative electrodes, metal negative electrodes and alloyed negative electrodes, and the corresponding positive electrode plate is composed of any one or a combination of layered oxides, Prussian blue compounds and polyanion compounds.
7. The integrated light-assisted secondary battery according to claim 1, characterized in that: The electrolyte is a soluble salt organic solution, and the diaphragm is polyethylene, polypropylene microporous membrane, glass fiber diaphragm, polyacrylonitrile diaphragm or a composite diaphragm thereof; or it is a gel or solid electrolyte with ion conductivity.
8. The integrated light-assisted secondary battery according to claim 1, characterized in that: The preparation method of the bifunctional electrode material comprises the following steps: (1) Roll-coating the electron transport material solution onto the conductive glass and then performing annealing treatment; (2) dissolving the photosensitive material in a solvent to obtain a solution; (3) dip coating, roll coating or spin coating the solution obtained in step (2) on the conductive glass plate obtained in step (1), and drying; (4) uniformly mixing the energy storage active material, the conductive agent, the binder and the dispersant to form a uniform slurry; (5) The slurry obtained in step (4) is coated on the conductive glass obtained in step (3) to obtain a bifunctional electrode material.
9. The integrated light-assisted secondary battery according to claim 8, characterized in that: In the method for preparing the bifunctional electrode material, the annealing temperature in step (1) is 150-450° C. and the annealing time is 15-60 min; and the dip coating temperature in step (3) is 25-35° C. and the time is 12-24 h.
10. The integrated light-assisted secondary battery according to claim 8, characterized in that: In the preparation method of the bifunctional electrode material, the conductive agent in step (4) is any one or more of acetylene black, Super P Li, Ketjen black or carbon nanotubes; the binder is any one or more of polyvinylidene fluoride, polyacrylic acid, hydroxymethyl cellulose, sericin, polyetherimide, polyimide, polylactic acid, polyethylene oxide; and the dispersant is any one or more of 1-methyl-2-pyrrolidone, dimethyl sulfoxide, NN-dimethylformamide, NN-dimethylacetamide, acetone, anhydrous ethanol and deionized water.
Citation Information
Patent Citations
Preparation method of photo-assisted lithium secondary battery MOF loaded perovskite composite electrode material
CN117174815A
Preparation method of photo-assisted lithium secondary battery positive electrode Co-CN (at) rGO composite material
CN117174834A
Cited By
Light-driven solid-state electrolyte membrane and integrated flexible light-assisted solid-state sodium metal battery based on light-driven solid-state electrolyte membrane
CN119833728A
A light-driven solid-state electrolyte membrane and integrated flexible light-assisted solid sodium metal battery based thereon
CN119833728B