Secondary battery and electronic device

By adjusting the composition of the positive electrode and electrolyte in the secondary battery, using combinations such as lithium iron phosphate, lithium manganate, boehmite, and lithium difluorophosphate, the problems of float safety and particle breakage change rate are solved, and a better battery life is achieved. High battery stability.

CN118782875AActive Publication Date: 2024-10-15NINGDE AMPEREX TECHNOLOGY LTD

Patent Information

Application Number
CN202411250462.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-10-15
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

Under the complicated application scenarios and performance improvement requirements of existing secondary batteries, it is difficult to simultaneously improve the safety of battery float charging and reduce the particle breakage change rate.

Method used

By adjusting the composition of the positive electrode and electrolyte in the secondary battery, using a combination including lithium iron phosphate, lithium manganate, boehmite and lithium difluorophosphate, and adjusting the proportions of zirconium, boron and antimony elements in the electrolyte, And using materials such as polyvinylidene fluoride and N-methylpyrrolidone to form special structural channels to improve battery stability.

Benefits of technology

It significantly improves the float charging safety of secondary batteries and reduces the particle breakage change rate, improving the overall stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to a secondary battery and an electronic device. Specifically, the secondary battery provided by the invention comprises a positive electrode, a negative electrode and an electrolyte, the positive electrode comprises a positive electrode current collector, and an insulating layer and a positive electrode material layer which are arranged on the positive electrode current collector; the insulating layer comprises boehmite, the positive electrode material layer comprises lithium iron phosphate and lithium manganate, the lithium iron phosphate comprises zirconium element and boron element, the lithium manganate comprises antimony element, and the electrolyte comprises lithium difluorophosphate. According to the invention, the floating charging safety of the secondary battery can be improved, and the particle breaking change rate can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of energy storage, and in particular to a secondary battery and an electronic device. Background Art

[0002] In the context of the rapid development of science and technology and the continuous improvement of the quality of life, secondary batteries have become the core power source in key areas such as portable electronic devices and electric vehicles due to their excellent high energy density characteristics and the convenience of cyclic charging and discharging, and their importance is becoming increasingly prominent. However, with the continuous expansion and complexity of application scenarios, more stringent requirements are placed on the comprehensive performance of secondary batteries. Summary of the invention

[0003] The embodiment of the present application further improves the comprehensive stability of the secondary battery by adjusting the composition of the positive electrode and the electrolyte in the secondary battery. The inventor of the present application found that the positive electrode includes a positive electrode current collector and an insulating layer and a positive electrode material layer arranged on the positive electrode current collector; the insulating layer includes boehmite, the positive electrode material layer includes lithium iron phosphate and lithium manganate, the lithium iron phosphate includes zirconium and boron elements, the lithium manganate includes antimony elements, and the electrolyte includes lithium difluorophosphate, which can not only improve the floating charge safety of the battery, but also reduce the particle breakage change rate, thereby completing the present application.

[0004] Optionally, based on the content of metal elements other than lithium in the positive electrode material layer, the mass content ratio of zirconium element, boron element and antimony element is 1:(0.1~0.9):(0.01~0.5).

[0005] Optionally, the amount of lithium difluorophosphate is 0.01 to 1 parts by mass relative to 100 parts by mass of the electrolyte.

[0006] Optionally, the amount of lithium difluorophosphate is 0.05 to 0.9 parts by mass relative to 100 parts by mass of the electrolyte.

[0007] Optionally, the amount of lithium difluorophosphate is 0.09 to 0.6 parts by mass relative to 100 parts by mass of the electrolyte.

[0008] Optionally, the insulating layer includes polyvinylidene fluoride and N-methylpyrrolidone.

[0009] Optionally, the electrolyte includes sodium dihydrogen phosphate, and the sodium dihydrogen phosphate is 0.03 parts by mass to 0.7 parts by mass relative to 100 parts by mass of the electrolyte.

[0010] Optionally, the electrolyte solution includes p-toluenesulfonyl isocyanate, and the p-toluenesulfonyl isocyanate is in an amount of 0.01 parts by mass to 3 parts by mass relative to 100 parts by mass of the electrolyte solution.

[0011] Optionally, the electrolyte includes sodium dihydrogen phosphate and p-toluenesulfonyl isocyanate, and relative to 100 parts by mass of the electrolyte, the sodium dihydrogen phosphate is a parts by mass, and the p-toluenesulfonyl isocyanate is b parts by mass, and 0.01≤a / b≤0.95.

[0012] In another aspect of the present application, the present application provides an electronic device, which includes the secondary battery described in the present application.

[0013] The present application not only improves the safety of battery floating charge but also reduces the particle breakage change rate by using a combination of a specific positive electrode and an electrolyte.

[0014] Additional aspects and advantages of the embodiments of the present application will be described, shown, or explained in part in the subsequent description through implementation of the embodiments of the present application. DETAILED DESCRIPTION

[0015] The embodiments of the present application will be described in detail below. The embodiments of the present application should not be interpreted as limiting the present application.

[0016] Unless expressly stated otherwise, the following terms used in this application have the meanings indicated below.

[0017] The present application not only improves the safety of battery floating charge but also reduces the particle breakage change rate by using a specific combination of positive electrode and electrolyte.

[0018] In one embodiment, the present application provides a secondary battery, which includes a positive electrode, a negative electrode, and an electrolyte as described below.

[0019] I. Positive electrode The present application relates to a secondary battery and an electronic device. Specifically, the present application provides a secondary battery, which includes: a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode includes a positive electrode current collector and an insulating layer and a positive electrode material layer disposed on the positive electrode current collector; the insulating layer includes boehmite, the positive electrode material layer includes lithium iron phosphate and lithium manganate, and the electrolyte includes lithium difluorophosphate. The present application can not only improve the floating charge safety of the battery, but also reduce the particle breakage change rate.

[0020] The positive electrode material layer includes lithium iron phosphate and lithium manganese oxide, and the positive electrode material layer can be one layer or multiple layers.

[0021] The inventors of the present application unexpectedly discovered in experiments that a positive electrode material layer comprising lithium iron phosphate and lithium manganese oxide and an insulating layer comprising boehmite can not only improve the floating charge safety of the battery but also reduce the particle breakage change rate in an electrolyte system containing lithium difluorophosphate.

[0022] The crystallographic information of boehmite, lithium iron phosphate, and lithium manganese oxide is quite different, but with the assistance of an electrolyte containing lithium difluorophosphate, the element sites in the three materials are in contact with lithium difluorophosphate. It is speculated that they form special structural channels in secondary batteries, which can not only improve the battery floating charge safety, but also reduce the particle breakage change rate.

[0023] Specifically, from the perspective of improving the safety of battery floating charge and reducing the rate of change of particle crushing, lithium iron phosphate includes zirconium and boron, and lithium manganate includes antimony. Among them, from the perspective of reducing the rate of change of particle crushing, the mass content ratio of zirconium, boron and antimony is 1: (0.1~0.9): (0.01~0.5), preferably 1: (0.16~0.6): (0.02~0.25), and more preferably 1: (0.2~0.5): (0.03~0.2). When the mass content ratio of zirconium, boron and antimony meets the above range, the safety of battery floating charge can be further improved and the rate of change of particle crushing can be reduced. When the above elements are introduced into the crystal structure of lithium iron phosphate and lithium manganate, the adaptability of the unit cell parameters between the two is further enhanced.

[0024] Specifically, from the perspective of improving the safety of battery floating charge and reducing the particle breakage change rate, in some embodiments, based on the content of metal elements other than lithium in the positive electrode material layer, the mass content of zirconium element is 1000ppm to 20000ppm, for example, 1000ppm, 2300ppm, 2600ppm, 5300ppm, 6300ppm, 7200ppm, 9500ppm, 10400ppm, 11700ppm, 13600ppm, 15000ppm, 15900ppm, 17900ppm, 19200ppm, 20000ppm or a value within the range composed of any two of them. In some embodiments, from the perspective of improving the floating charge safety of the battery and reducing the particle crushing change rate, based on the content of metal elements other than lithium in the positive electrode material layer, the mass content of the boron element is 500ppm to 3000ppm, for example, 500ppm, 700ppm, 1000ppm, 1200ppm, 1400ppm, 1500ppm, 1700ppm, 1900ppm, 2100ppm, 2200ppm, 2600ppm, 3000ppm or a value in the range of any two thereof. In some embodiments, from the perspective of improving the floating charge safety of the battery and reducing the particle crushing change rate, based on the content of metal elements other than lithium in the positive electrode material layer, the mass content of the antimony element is 100ppm to 1000ppm, for example, 100ppm, 200ppm, 300ppm, 400ppm, 500ppm, 600ppm, 700ppm, 800ppm, 900ppm, 1000ppm or a value in the range of any two thereof.

[0025] There is no limitation on the type of positive electrode conductive material, and any known conductive material can be used. Examples of positive electrode conductive materials may include, but are not limited to, carbon black such as acetylene black; carbon materials such as amorphous carbon such as needle coke; carbon nanotubes; graphene, etc. The above positive electrode conductive materials may be used alone or in any combination.

[0026] There is no limitation on the type of solvent used to form the positive electrode slurry, as long as it is a solvent that can dissolve or disperse the positive electrode material, the conductive material, and the positive electrode binder. Examples of solvents used to form the positive electrode slurry may include any of aqueous solvents and organic solvents. Examples of aqueous media may include, but are not limited to, water and mixed media consisting of alcohol and water. Examples of organic media may include, but are not limited to, aliphatic hydrocarbons such as hexane; aromatic hydrocarbons such as benzene, toluene, xylene, and methylnaphthalene; heterocyclic compounds such as quinoline and pyridine; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; esters such as methyl acetate and methyl acrylate; amines such as diethylenetriamine and N,N-dimethylaminopropylamine; ethers such as diethyl ether, propylene oxide, and tetrahydrofuran; amides such as N-methylpyrrolidone, dimethylformamide, and dimethylacetamide; non-protonic polar solvents such as hexamethylphosphoramide and dimethyl sulfoxide, etc.

[0027] The density of the active material layer of the positive electrode excluding the current collector is usually 3.5 g / cm 3 In order to further increase the capacity of the battery, it is preferably 4 g / cm 3 In addition, the upper limit is preferably 4.6 g / cm 3 the following.

[0028] The type of positive electrode current collector is not particularly limited, and it can be any material known to be suitable for use as a positive electrode current collector. Examples of positive electrode current collectors may include, but are not limited to, metal materials such as aluminum, stainless steel, nickel plating, titanium, tantalum, and carbon materials such as carbon cloth and carbon paper. In some embodiments, the positive electrode current collector is a metal material. In some embodiments, the positive electrode current collector is aluminum.

[0029] In order to reduce the electronic contact resistance between the positive electrode current collector and the positive electrode material layer, the surface of the positive electrode current collector may include a conductive additive or a conductive coating. Examples of conductive additives may include, but are not limited to, carbon and precious metals such as gold, platinum, and silver. Examples of conductive coatings may include a mixture layer containing an inorganic oxide, a conductive agent, and a binder.

[0030] From the viewpoint of improving the floating charge safety of the battery and reducing the particle breakage change rate, boehmite is contained in the insulating layer.

[0031] Specifically, from the viewpoint of improving the floating charge safety of the battery and reducing the particle crushing change rate, the insulating layer includes polyvinylidene fluoride and N-methylpyrrolidone.

[0032] The positive electrode is made as follows: Boehmite, polyvinylidene fluoride and N-methylpyrrolidone are mixed, and deionized water is added thereto and mixed evenly to prepare slurry 1.

[0033] The above-mentioned positive electrode material is mixed with a conductive agent such as acetylene black or carbon black, and a binder such as polyvinylidene fluoride or polyacrylonitrile, and a high boiling point solvent such as N-methylpyrrolidone is added thereto and kneaded to prepare a slurry 2 .

[0034] Slurry 1 and slurry 2 are applied in parallel on an aluminum foil or the like of a current collector, and then dried and pressed to form a positive electrode.

[0035] II. Electrolyte The electrolyte used in the secondary battery of the present application includes an electrolyte and a solvent for dissolving the electrolyte. In some embodiments, the electrolyte of the present application includes lithium difluorophosphate.

[0036] When lithium difluorophosphate is used in the secondary battery of the present application, the inventors found that the addition of lithium iron phosphate, lithium manganese oxide and boehmite to the positive electrode can not only improve the floating charge safety of the battery, but also reduce the particle breakage change rate.

[0037] Specifically, from the viewpoint of improving the floating charge safety of the battery and reducing the particle crushing change rate, the electrolyte includes lithium difluorophosphate, wherein relative to 100 parts by mass of the electrolyte, the lithium difluorophosphate is more than 0.01 parts by mass, preferably more than 0.05 parts by mass, more preferably more than 0.09 parts by mass, more preferably more than 0.15 parts by mass, and particularly preferably more than 0.18 parts by mass. In addition, as the upper limit of the content of lithium difluorophosphate, from the viewpoint of improving the floating charge safety of the battery and reducing the particle crushing change rate, lithium difluorophosphate is less than 1 part by mass, preferably less than 0.9 parts by mass, particularly preferably less than 0.8 parts by mass, more preferably less than 0.7 parts by mass, further preferably less than 0.6 parts by mass, and particularly preferably less than 0.5 parts by mass. When within the above range, it helps to further improve the floating charge safety of the secondary battery and reduce the particle crushing change rate.

[0038] Specifically, from the viewpoint of improving the floating charge safety of the secondary battery and reducing the particle crushing change rate, the electrolyte includes sodium dihydrogen phosphate. In some embodiments, relative to 100 parts by mass of the electrolyte, the sodium dihydrogen phosphate is a parts by mass, and the value range of a is 0.03 to 0.7, for example, a is 0.03, 0.05, 0.08, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7 or a value in the range composed of any two of them. When the mass fraction of sodium dihydrogen phosphate in the electrolyte is regulated to meet the above range, the floating charge safety of the secondary battery can be further improved and the particle crushing change rate can be reduced.

[0039] Specifically, from the perspective of improving the floating charge safety of the secondary battery and reducing the particle breakage change rate, the electrolyte includes p-toluenesulfonyl isocyanate. In some embodiments, relative to 100 parts by mass of the electrolyte, the p-toluenesulfonyl isocyanate is b parts by mass, and the value range of b is 0.01 to 3, for example, b is 0.01, 0.1, 0.2, 0.3, 0.7, 0.8, 1.1, 1.3, 1.6, 1.7, 2.0, 2.1, 2.4, 2.6, 3.0 or a value in the range composed of any two of them. When the mass fraction of p-toluenesulfonyl isocyanate in the electrolyte is regulated to meet the above range, the floating charge safety of the secondary battery can be further improved and the particle breakage change rate can be reduced.

[0040] Specifically, from the perspective of improving the floating charge safety of the secondary battery and reducing the particle breakage change rate, the electrolyte includes sodium dihydrogen phosphate and p-toluenesulfonyl isocyanate. In some embodiments, 0.01≤a / b≤0.95, for example, the value of a / b is 0.01, 0.06, 0.13, 0.19, 0.27, 0.37, 0.42, 0.46, 0.52, 0.63, 0.67, 0.75, 0.87, 0.88, 0.95 or a value in the range of any two thereof. When the mass fractions of sodium dihydrogen phosphate and p-toluenesulfonyl isocyanate in the electrolyte are regulated to meet the above relationship, the interaction and close cooperation between the two can be promoted, thereby better improving the floating charge safety of the secondary battery and reducing the particle breakage change rate.

[0041] In some embodiments, the additive in the electrolyte includes one or more of the following: ethylene glycol sulfate, 1,2-propylene glycol sulfate, 1,3-propylene glycol sulfate, 1,2-butylene glycol sulfate, 1,3-butylene glycol sulfate, 1,4-butylene glycol sulfate, 1,2-pentanediol sulfate, 1,3-pentanediol sulfate, 1,4-pentanediol sulfate, 1,5-pentanediol sulfate, dimethyl sulfate, ethyl methyl sulfate, sulfur diethyl sulfonate, methyl fluorosulfonate, ethyl trifluoromethanesulfonate, methyl methanesulfonate, ethyl methanesulfonate, butyl dimethanesulfonate, methyl 2-(methylsulfonyloxy)propionate, ethyl 2-(methylsulfonyloxy)propionate, 1-fluoro-1,3-propane sultone, 2-fluoro-1,3-propane sultone, 3-fluoro-1,3-propane sultone, 1-methyl-1,3-propane sultone, 2-methyl-1,3-propane sultone, 3-methyl-1, 3-propane sultone, 1-propylene-1,3-sultone, 2-propylene-1,3-sultone, 1-fluoro-1-propylene-1,3-sultone, 2-fluoro-1-propylene-1,3-sultone, 3-fluoro-1-propylene-1,3-sultone, 1-fluoro-2-propylene-1,3-sultone, 2-fluoro-2-propylene-1,3-sultone, 3-fluoro-2-propylene-1,3-sultone, 1-methyl-1-propylene-1,3-sultone, 2-methyl-1-propylene-1,3-sultone, 3-methyl-1-propylene-1,3-sultone, 1-methyl-2-propylene-1,3-sultone , 2-methyl-2-propylene-1,3-sultone, 3-methyl-2-propylene-1,3-sultone, 1,4-butane sultone, 1,5-pentane sultone, methylene methanedisulfonate, ethylene methanedisulfonate, dimethyl sulfite, ethyl methyl sulfite, diethyl sulfite, 1,2-ethylene glycol sulfite, 1,2-propylene glycol sulfite, 1,3-propylene glycol sulfite, 1,2-butylene glycol sulfite, 1,3-butylene glycol sulfite, 1,4-butylene glycol sulfite, 1,2-pentanediol sulfite, 1,3-pentanediol sulfite, 1,4-pentanediol sulfite, 1,5-pentanediol sulfite, etc. In some embodiments, the electrolyte further includes an ionizable lithium salt, and the ionizable lithium salt includes at least one of LiPF6, LiSbF6, LiAsF6, LiClO4, LiN(C2F5SO2)2, CF3SO3Li, LiC(CF3SO2)3 or LiC4BO8. For example, the lithium salt used in the electrolyte of the present application includes LiPF6, and the content of LiPF6 is 9-15% by mass, preferably 9-13% by mass, and more preferably 9-12% by mass based on the mass of the electrolyte. By setting the above content range, the effect of improving the floating charge safety of the secondary battery and reducing the particle breakage change rate can be more balanced.

[0042] In some embodiments, the electrolyte further includes at least one of lithium difluorophosphate (LiPO2F2), lithium difluorooxalatoborate (LiDFOB), lithium bis(oxalatoborate) (LiBOB), lithium tetrafluoroborate (LiBF4), lithium bis(trifluoromethanesulfonyl imide) (LiTFSI), and lithium bis(fluorosulfonyl imide) (LiFSI).

[0043] In some embodiments, the additive in the electrolyte further includes at least one of a fluoroether compound, a fluorocarbonate compound, and an ether nitrile compound, such as hydrofluoroether (HFE-458), fluoroethylene carbonate (FEC), and the like.

[0044] In some embodiments, the electrolyte may further include a non-aqueous solvent. The non-aqueous solvent may be selected from carbonate compounds, carboxylate compounds, ether compounds, phosphate compounds, other organic solvents, or combinations thereof.

[0045] Optionally, the carbonate compound may be a linear carbonate compound, a cyclic carbonate compound or a combination thereof. On the other hand, the carbonate compound may also be a fluorinated carbonate compound, a non-fluorinated carbonate compound or a combination thereof.

[0046] Specifically, examples of chain carbonate compounds are diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), methylethyl carbonate (MEC) and combinations thereof. Examples of cyclic carbonate compounds are ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylethylene carbonate (VEC) or combinations thereof. Examples of fluorinated carbonate compounds are fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate or combinations thereof.

[0047] Specifically, examples of the carboxylate compound are methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolide, valerolactone, mevalonolactone, caprolactone, methyl formate, or a combination thereof.

[0048] Specifically, examples of the ether compound are dibutyl ether, tetraglyme, diglyme, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, or a combination thereof.

[0049] Specifically, examples of the phosphate compound are trimethyl phosphate, triethyl phosphate, trioctyl phosphate, or a combination thereof.

[0050] Specifically, examples of other organic solvents are dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, N-methylpyrrolidone, formamide, dimethylformamide, acetonitrile, or a combination thereof.

[0051] III. Negative electrode The negative electrode includes a negative electrode current collector and a negative electrode material layer disposed on the surface of the negative electrode current collector, wherein the negative electrode material layer contains a negative electrode material. In some embodiments, the chargeable capacity of the negative electrode material is greater than the discharge capacity of the positive electrode material to prevent lithium metal from being accidentally precipitated on the negative electrode during charging.

[0052] The negative electrode material is not particularly limited, and examples thereof include carbon-based negative electrode materials, metal-based negative electrode materials, silicon-based negative electrode materials, and negative electrode materials in combination thereof.

[0053] Carbon-based negative electrode materials Here, the carbon-based negative electrode material refers to an active material having a carbon-based skeleton into which lithium can be inserted, and examples of the carbon-based negative electrode material include carbonaceous materials and graphite materials.

[0054] As carbonaceous materials, for example, graphitizable carbon, non-graphitizable carbon having a structure similar to an amorphous structure represented by glassy carbon, etc. can be cited. Here, as graphitizable carbon, for example, carbon materials obtained from petroleum or coal using tar pitch as a raw material can be cited. When giving specific examples, coke, mesocarbon microbeads (MCMB), mesophase pitch-based carbon fibers, and pyrolysis vapor-grown carbon fibers can be cited. In addition, as non-graphitizable carbon, for example, phenolic resin sintered bodies, polyacrylonitrile-based carbon fibers, quasi-isotropic carbon, furfuryl alcohol resin sintered bodies (PFA), hard carbon, etc. can be cited.

[0055] Furthermore, as graphite materials, for example, natural graphite, artificial graphite, etc. can be cited. Among them, as artificial graphite, for example: artificial graphite obtained by heat-treating carbon containing graphitized carbon mainly at 2800°C or above, graphite MCMB obtained by heat-treating MCMB at 2000°C or above, graphite mesophase pitch-based carbon fiber obtained by heat-treating mesophase pitch-based carbon fiber at 2000°C or above, etc. can be cited. In addition, in the present application, as a carbon-based negative electrode material, natural graphite (amorphous coated natural graphite) in which at least a portion of its surface is coated with amorphous carbon can be used.

[0056] In addition, the metal-based negative electrode material is an active material containing a metal, generally referring to an active material having an element capable of inserting lithium or alloying with lithium in the structure, an element capable of inserting lithium or alloying with lithium, and a theoretical current capacity of 500 mAh / g or more per unit mass. As a metal-based negative electrode material, for example, lithium metal, a single metal capable of forming a lithium alloy (such as Ag, Al, Ba, Bi, Cu, Ga, Ge, In, Ni, P, Pb, Sb, Si, Sn, Sr, Zn, Ti, etc.) and its alloy, and their oxides, sulfides, nitrides, silicides, carbides, phosphides, etc. can be used. Among them, as a metal-based negative electrode material, an active material (silicon-based negative electrode material) containing silicon is preferably used. This is because the use of a silicon-based negative electrode material can increase the capacity of a secondary battery.

[0057] Examples of silicon-based negative electrode materials include silicon (Si), alloys containing silicon, SiO, SiO 2 , and composites of silicon-containing materials and conductive carbon (silicon-carbon materials) in which a silicon-containing material is coated with conductive carbon or composited with conductive carbon.

[0058] From the viewpoint of improving battery capacity, a silicon-carbon material, for example, a porous carbon-supported silicon composite material is preferred.

[0059] The negative electrode material may be used alone or in combination of two or more at any ratio.

[0060] Here, the volume average particle size of the negative electrode material is preferably 1 μm or more, more preferably 5 μm or more, preferably 30 μm or less, and more preferably 20 μm or less. If the volume average particle size of the negative electrode material is above the above lower limit, the heat generation during the internal short circuit can be effectively suppressed. In addition, if the volume average particle size of the negative electrode material is below the above upper limit, the increase in the initial resistance of the obtained battery can be effectively suppressed.

[0061] The negative electrode material layer may further include a negative electrode binder. The negative electrode binder can improve the bonding between the negative electrode material particles and the bonding between the negative electrode material and the current collector. The type of negative electrode binder is not particularly limited, as long as it is a material that is stable to the solvent used in the electrolyte or electrode manufacturing. In some embodiments, the negative electrode binder includes a resin binder. Examples of resin binders include, but are not limited to, fluororesins, polyacrylonitrile (PAN), polyimide resins, acrylic resins, polyolefin resins, and the like. When an aqueous solvent is used to prepare the negative electrode mixture slurry, the negative electrode binder includes, but is not limited to, carboxymethyl cellulose (CMC) or its salt, styrene-butadiene rubber (SBR), polyacrylic acid (PAA) or its salt, polyvinyl alcohol, and the like.

[0062] As a current collector for holding the negative electrode material, any known current collector can be used. Examples of negative electrode current collectors include, but are not limited to, metal materials such as copper, nickel, stainless steel, and nickel-plated steel. In some embodiments, the negative electrode current collector is copper.

[0063] The negative electrode can be prepared by applying a negative electrode mixture slurry containing a negative electrode material, a resin binder, etc. on a negative electrode current collector, drying it, and then rolling it to form a negative electrode material layer on both sides of the negative electrode current collector, thereby obtaining a negative electrode.

[0064] IV. Isolation membrane In order to prevent short circuit, a separator is usually provided between the positive electrode and the negative electrode. In this case, the electrolyte of the present application is usually used by infiltrating the separator.

[0065] There is no particular restriction on the material and shape of the isolation membrane, as long as the effect of the present application is not significantly impaired. The isolation membrane may be a resin, glass fiber, inorganic substance, etc. formed of a material that is stable to the electrolyte of the present application. In some embodiments, the isolation membrane includes a porous sheet or a non-woven fabric-like material with excellent liquid retention. Examples of materials for resin or glass fiber isolation membranes may include, but are not limited to, polyolefins, aromatic polyamides, polytetrafluoroethylene, polyether sulfone, etc. In some embodiments, the polyolefin is polyethylene or polypropylene. In some embodiments, the polyolefin is polypropylene. The materials of the above isolation membranes may be used alone or in any combination.

[0066] The isolation film may also be a material formed by laminating the above materials, and examples thereof include, but are not limited to, a three-layer isolation film formed by laminating polypropylene, polyethylene, and polypropylene in this order.

[0067] Examples of inorganic materials may include, but are not limited to, oxides such as aluminum oxide and silicon dioxide, nitrides such as aluminum nitride and silicon nitride, and sulfates (eg, barium sulfate, calcium sulfate, etc.). The form of the inorganic material may include, but is not limited to, granular or fibrous.

[0068] The separator may be in the form of a thin film, examples of which include, but are not limited to, nonwoven fabrics, woven fabrics, microporous films, etc. In the thin film form, the separator has a pore size of 0.01 μm to 1 μm and a thickness of 5 μm to 50 μm. In addition to the above-mentioned independent thin film separators, the following separators can also be used: a separator formed by forming a composite porous layer containing the above-mentioned inorganic particles on the surface of the positive electrode and / or the negative electrode using a resin-based adhesive, for example, a separator formed by using a fluororesin as an adhesive to form a porous layer on both sides of the positive electrode with alumina particles having a particle size of 90% less than 1 μm.

[0069] The thickness of the isolation film is arbitrary. In some embodiments, the thickness of the isolation film is greater than 1 μm, greater than 5 μm, or greater than 8 μm. In some embodiments, the thickness of the isolation film is less than 50 μm, less than 40 μm, or less than 30 μm. When the thickness of the isolation film is within the above range, the insulation and mechanical strength can be ensured, and the DC resistance characteristics and energy density of the secondary battery can be ensured.

[0070] The present application further provides an electronic device, which includes the secondary battery described in the present application.

[0071] The use of the secondary battery of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. In some embodiments, the secondary battery of the present application can be used for, but not limited to, laptop computers, pen-input computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries and lithium-ion capacitors, etc.

[0072] Example Examples of the secondary battery of the present application are shown below, but the present application is not limited to these examples.

[0073] Preparation of secondary batteries Production of positive electrode: Boehmite and polyvinylidene fluoride were mixed in a mass ratio as shown in Table 1, dissolved in N-methylpyrrolidone, deionized water was added thereto and mixed evenly, to prepare a positive electrode slurry 1.

[0074] The positive electrode materials lithium iron phosphate (46wt%), lithium manganate (51wt%), and conductive carbon black (1wt%) in Table 1 were mixed, and polyvinylidene fluoride (2wt%) was dissolved in N-methylpyrrolidone to obtain a solution and mixed to prepare positive electrode slurry 2. Among them, slurry 1 was applied on the ear side, and slurry 1 and slurry 2 were applied on aluminum foil in parallel. The coated aluminum foil was dried, pressurized, and cut into a specified size to make a positive electrode.

[0075] Preparation of isolation membrane: A 12 μm thick polyethylene (PE) microporous membrane was selected as the isolation membrane.

[0076] Negative electrode production: The negative electrode material artificial graphite and SiO2 (mass ratio 90:10): 96wt%, styrene-butadiene rubber: 2wt% are mixed, added to a solution obtained by dissolving carboxymethyl cellulose lithium: 2wt% in deionized water in advance and mixed to prepare a negative electrode slurry. The negative electrode slurry is coated on one side of a copper foil, dried, pressurized, and then cut into a specified size to make a negative electrode.

[0077] Preparation of electrolyte: In an argon atmosphere glove box with a water content of less than 10 ppm, ethyl methyl carbonate, ethyl acetate, and diethyl carbonate are mixed in a mass ratio of 1:1:1 to obtain a basic solvent, and then lithium salt LiPF6 and the additives shown in Table 1 are added to the above-mentioned base solvent, and the electrolyte is obtained after uniform mixing, wherein the mass content of LiPF6 is 12% based on the mass of the electrolyte.

[0078] Battery production: The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, so that the separator is between the positive electrode sheet and the negative electrode sheet to play an isolating role, and the electrode assembly is wound, and the electrode assembly is placed in the outer packaging aluminum plastic film after welding the pole ear, and the water is removed at 80°C, and the above electrolyte is injected, and the lithium ion battery is obtained after vacuum packaging, standing, formation, shaping, capacity testing and other processes. The secondary battery is a bag-shaped battery with a width of 30mm, a height of 45mm, and a thickness of 5mm.

[0079] Table 1

[0080] Test Method Particle breakage rate Two secondary batteries (numbered as battery X and battery Y) were repeatedly charged and discharged by the following steps. The test method is as follows: First, in an environment of 25°C, the first charge and discharge were performed. First, constant current charging was performed at a current of 0.5C. After charging to 4.2V, constant voltage charging was performed. Then, constant current discharge was performed at a current of 1C to 2.8V. Then, battery X was charged and discharged 200 times, and battery Y was charged and discharged 400 times.

[0081] The battery after the above cycle was disassembled, and the positive electrode material layer was tested by cross-section polishing-scanning electron microscopy (CP-SEM) to obtain the particle crushing change rate = the first particle crushing percentage of battery X / the second particle crushing percentage of battery Y×100%. The evaluation was performed according to the following criteria: the smaller the particle crushing change rate, the higher the overall stability of the secondary battery in the present application.

[0082] A: The particle breakage change rate is less than 1.2.

[0083] B: The particle crushing change rate is 1.2 or more and less than 1.4.

[0084] C: The particle crushing change rate is 1.4 or more and less than 1.8.

[0085] D: The particle crushing change rate is 1.8 or more.

[0086] Float charge safety The test method is as follows: Place the prepared secondary battery in a 25℃ constant temperature box and let it stand for 30 minutes to allow the secondary battery to reach a constant temperature. Charge with a constant current of 1C to a voltage of 4.2V, charge with a constant voltage to a current of 0.05C, and then discharge with a constant current of 1C to a voltage of 2.8V. Then charge with a constant current of 0.5C to a voltage of 4.2V, charge with a constant voltage to a current of 0.05C, and use a micrometer to test and record the thickness of the secondary battery at this time as the initial thickness. Transfer the secondary battery to a 45℃ constant temperature box, and then charge with a constant voltage of 4.2V for 30 days. After 30 days, transfer the secondary battery to a 25℃ constant temperature box, let it stand for 60 minutes, and discharge with a constant current of 1C to a voltage of 2.8V. Then charge with a constant current of 1C to a voltage of 4.2V, charge with a constant voltage to a current of 0.05C, and then discharge with a constant current of 1C to 2.8V, and measure the thickness of the lithium-ion battery as the thickness after floating charge.

[0087] Float charge thickness change rate = (float charge thickness - initial thickness) / initial thickness × 100% The evaluation was performed according to the following criteria: the smaller the value of the floating charge thickness change rate, the higher the overall stability of the secondary battery in the present application.

[0088] A: The floating charge thickness change rate is less than 22%.

[0089] B: The floating thickness change rate is greater than 22% and less than 28%.

[0090] C: The floating thickness change rate is greater than 28% and less than 33%.

[0091] D: The floating thickness change rate is more than 33%.

[0092] Test Results In Table 1, “ / ” indicates that the substance was not added; It can be seen from Table 1 that the positive electrode of the present application includes a positive electrode collector and an insulating layer and a positive electrode material layer arranged on the positive electrode collector; the insulating layer includes boehmite, the positive electrode material layer includes lithium iron phosphate and lithium manganese oxide, and the electrolyte includes lithium difluorophosphate, which can not only improve the floating charge safety of the secondary battery, but also reduce the particle breakage change rate.

[0093] In particular, the present application dopes zirconium and boron into lithium iron phosphate and antimony into lithium manganese oxide, which can further improve the floating charge safety of the secondary battery and reduce the particle breakage change rate.

[0094] In particular, based on the content of metal elements other than lithium in the positive electrode material layer, the mass content ratio of zirconium, boron and antimony is 1:(0.1~0.9):(0.01~0.5), which can further improve the floating charge safety of the secondary battery and reduce the particle breakage change rate.

[0095] In particular, the amount of lithium difluorophosphate is 0.01 to 1 parts by mass relative to 100 parts by mass of the electrolyte, which can further improve the floating charge safety of the secondary battery and reduce the particle breakage change rate.

[0096] In particular, the amount of lithium difluorophosphate is more preferably 0.09 to 0.6 parts by mass relative to 100 parts by mass of the electrolyte, which can further improve the floating charge safety of the secondary battery and reduce the particle breakage change rate.

[0097] In particular, the insulating layer includes polyvinylidene fluoride and N-methylpyrrolidone, which can further improve the floating charge safety of the secondary battery and reduce the particle crushing change rate.

[0098] In particular, the electrolyte includes sodium dihydrogen phosphate, and the sodium dihydrogen phosphate is 0.03 to 0.7 parts by mass relative to 100 parts by mass of the electrolyte, which can further improve the floating charge safety of the secondary battery and reduce the particle breakage change rate.

[0099] In particular, the electrolyte includes p-toluenesulfonyl isocyanate, and the p-toluenesulfonyl isocyanate is 0.01 to 3 parts by mass relative to 100 parts by mass of the electrolyte, which can further improve the floating charge safety of the secondary battery and reduce the particle breakage change rate.

[0100] In particular, the electrolyte includes sodium dihydrogen phosphate and p-toluenesulfonyl isocyanate, relative to 100 parts by mass of the electrolyte, sodium dihydrogen phosphate is a parts by mass, p-toluenesulfonyl isocyanate is b parts by mass, 0.01≤a / b≤0.95 can further improve the floating charge safety of the secondary battery and reduce the particle breakage change rate.

[0101] References to "embodiments", "partial embodiments", "one embodiment", "another example", "example", "specific example" or "partial example" throughout the specification mean that at least one embodiment or example in the present application includes the specific features, structures, materials or characteristics described in the embodiment or example. Therefore, descriptions appearing in various places throughout the specification, such as: "in some embodiments", "in an embodiment", "in one embodiment", "in another example", "in an example", "in a specific example" or "example", do not necessarily refer to the same embodiment or example in the present application. In addition, the specific features, structures, materials or characteristics in the present application may be combined in one or more embodiments or examples in any suitable manner.

[0102] Although illustrative embodiments have been demonstrated and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions and modifications may be made to the embodiments without departing from the spirit, principles and scope of the present application.

Claims

1. A secondary battery, include: A positive electrode, a negative electrode and an electrolyte, characterized in that the positive electrode includes a positive electrode collector and an insulating layer and a positive electrode material layer arranged on the positive electrode collector; the insulating layer includes boehmite, the positive electrode material layer includes lithium iron phosphate and lithium manganate, the lithium iron phosphate includes zirconium and boron elements, the lithium manganate includes antimony elements, and the electrolyte includes lithium difluorophosphate.

2. The secondary battery according to claim 1, It is characterized in that Based on the content of metal elements other than lithium in the positive electrode material layer, the mass content ratio of the zirconium element, the boron element and the antimony element is 1:(0.1-0.9):(0.01-0.5).

3. The secondary battery according to claim 1 or 2, It is characterized in that The amount of the lithium difluorophosphate is 0.01 to 1 parts by mass relative to 100 parts by mass of the electrolyte.

4. The secondary battery according to claim 1 or 2, It is characterized in that The amount of the lithium difluorophosphate is 0.05 to 0.9 parts by mass relative to 100 parts by mass of the electrolyte.

5. The secondary battery according to claim 1 or 2, It is characterized in that The amount of the lithium difluorophosphate is 0.09 to 0.6 parts by mass relative to 100 parts by mass of the electrolyte.

6. The secondary battery according to claim 1 or 2, It is characterized in that The insulating layer comprises polyvinylidene fluoride and N-methylpyrrolidone.

7. The secondary battery according to claim 1 or 2, It is characterized in that wherein the electrolyte comprises sodium dihydrogen phosphate, and the amount of the sodium dihydrogen phosphate is 0.03 parts by mass to 0.7 parts by mass relative to 100 parts by mass of the electrolyte; or The electrolyte solution includes p-toluenesulfonyl isocyanate, and the p-toluenesulfonyl isocyanate is in an amount of 0.01 parts by mass to 3 parts by mass relative to 100 parts by mass of the electrolyte solution.

8. The secondary battery according to claim 1 or 2, It is characterized in that The electrolyte comprises sodium dihydrogen phosphate and p-toluenesulfonyl isocyanate. Relative to 100 parts by mass of the electrolyte, the sodium dihydrogen phosphate is a part by mass, the p-toluenesulfonyl isocyanate is b parts by mass, and 0.01≤a / b≤0.

95.

9. An electronic device, It is characterized in that It includes the secondary battery according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • High-capacity lithium-ion electrolyte, battery and preparation method of battery

    CN101771167A

  • Battery electrolyte and preparation method thereof, lithium sulfur secondary battery

    CN109167096A

  • Electrolyte adaptive to high-nickel ternary positive electrode material

    CN112599856A

  • Electrolyte, and electrochemical device and electronic device comprising same

    CN113767500A

  • Electrolyte, battery monomer, preparation method of battery monomer, battery and power utilization device

    CN117976970A

Cited By

  • Electrolyte and lithium ion battery

    CN119852521A

  • Secondary battery and electronic apparatus

    WO2026051628A1

  • Positive electrode material, secondary battery, and electronic device

    WO2026193917A1