Electrochemical device and electronic device
By using an electrolyte containing fluorinated ethylene carbonate and a compound of formula I in a lithium-ion battery, the problem of electrolyte consumption caused by the high reactivity of silicon-based materials after lithiation is solved, a stable interface film is formed, and the cycle stability of the battery is improved. properties and energy density.
Patent Information
- Application Number
- CN202410763763.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-15
AI Technical Summary
The lithium-silicon alloy formed after silicon-based materials are lithiated in lithium-ion batteries is highly reactive, leading to rapid electrolyte consumption and poor cycle stability of electrochemical devices.
An electrolyte containing fluoroethylene carbonate and a specific compound of formula I is used to protect the electrolyte through the interfacial film-forming properties of fluoroethylene carbonate, and the compound of formula I reduces the consumption rate of fluoroethylene carbonate to form a stable interfacial film. , improve cycle stability.
It effectively alleviates the rupture of the negative active material caused by the expansion of nano-silicon particles, improves the energy density and cycle performance of the electrochemical device, and extends the service life of the battery.
Smart Images

Figure CN118782877A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrochemical technology, and in particular to an electrochemical device and an electronic device. Background Art
[0002] With the rapid development of electronic products, electrochemical devices (such as lithium-ion batteries) are widely used in mobile phones, laptops, tablets, drones, electric vehicles, power tools, power storage systems, etc. due to their advantages such as high energy density, miniaturization and light weight. Especially in the field of 3C products, consumer users still have great demand for improving the battery life of electronic products, so higher requirements are put forward for the energy density of electrochemical devices.
[0003] In order to further improve the energy density of electrochemical devices, electrode materials with high specific capacity are needed. As a type of alloyed negative electrode material, silicon-based materials can provide ultra-high specific capacity of up to 4200mAh / g, so silicon-based materials are materials with great potential for improving energy density. However, after silicon-based materials are lithiated, lithium-silicon alloys will be formed. Lithium-silicon alloys are highly reactive and can easily attack solvent molecules in the electrolyte, resulting in rapid consumption of the electrolyte and loss of active lithium. Therefore, electrochemical devices will have poor cycle stability. Summary of the invention
[0004] The purpose of the present application is to provide an electrochemical device and an electronic device to improve the cycle stability of the electrochemical device.
[0005] A first aspect of the present application provides an electrochemical device, which includes a negative electrode sheet and an electrolyte, wherein;
[0006] The negative electrode plate includes a negative electrode material layer, the negative electrode material layer includes a silicon-based material, the silicon-based material includes silicon element, and based on the total mass of the negative electrode material layer, the mass percentage of silicon element is 30% to 60%;
[0007] The electrolyte comprises fluoroethylene carbonate and a compound of formula I:
[0008]
[0009] wherein R1 and R2 are each independently selected from a hydrogen atom, a fluorine atom, a substituted or unsubstituted C1 to C5 alkyl group, a substituted or unsubstituted C6 to C 10The present invention relates to an aryl group and a substituted or unsubstituted C2 to C6 carboxylate group, wherein the substituents in the carboxylate group, the alkyl group and the aryl group are fluorine atoms when substituted. The mass percentage of the silicon element mass is controlled within the above range, so that the electrochemical device can meet the space required for the expansion of the nano-silicon particles during the charging and discharging process, thereby effectively alleviating the phenomenon of the cracking of the negative electrode active material caused by the expansion of the nano-silicon particles, and improving the energy density and cycle performance of the electrochemical device. The compound of formula I is selected as a pre-film-forming additive to be combined with fluoroethylene carbonate. Through the interfacial film-forming characteristics of fluoroethylene carbonate, the electrolyte is protected from continuous decomposition at the interface to a certain extent, and the consumption rate of fluoroethylene carbonate is reduced by the compound of formula I, thereby improving the cycle stability of the electrochemical device.
[0010] In one embodiment of the present application, the compound of formula I comprises at least one of the following compounds:
[0011]
[0012]
[0013] In one embodiment of the present application, based on the total mass of the electrolyte, the mass percentage of fluoroethylene carbonate is 1% to 30%.
[0014] In one embodiment of the present application, the mass percentage of fluoroethylene carbonate is 10% to 30% based on the total mass of the electrolyte. By controlling the mass percentage of fluoroethylene carbonate within the above range, FEC can better meet the consumption of long-term cycles, thereby improving the cycle stability of the electrochemical device.
[0015] In one embodiment of the present application, the mass percentage of the compound of formula I is 0.01% to 5% based on the total mass of the electrolyte. By controlling the mass percentage of the compound of formula I within the above range, it is beneficial to improve the integrity of the interface film layer formed, and improve the problem of poor low temperature and rate discharge caused by the obstruction of interface ion transport in the electrochemical device, thereby improving the cycle stability of the electrochemical device.
[0016] In one embodiment of the present application, based on the total mass of the electrolyte, the mass percentage of the compound of formula I is 0.1% to 2%.
[0017] In one embodiment of the present application, the electrolyte further comprises a dinitrile compound, the dinitrile compound comprising at least one of succinonitrile, glutaronitrile, methylglutaronitrile, adiponitrile, pimelonitrile, suberonitrile, azelaic acid dinitrile or sebaconitrile; based on the total mass of the electrolyte, the mass percentage of the dinitrile compound is 0.1% to 3%. By controlling the mass percentage of the dinitrile compound within the above range, it is beneficial to improve the stability of the above SEI film, reduce the reactivity of the negative electrode active material, and thus improve the cycle stability of the electrochemical device.
[0018] In one embodiment of the present application, the electrolyte further comprises a cyclic compound containing a sulfur-oxygen double bond, the cyclic compound containing a sulfur-oxygen double bond comprises at least one of 1,3-propane sultone, 1,4-butane sultone or 2,4-butane sultone; based on the total mass of the electrolyte, the mass percentage of the cyclic compound containing a sulfur-oxygen double bond is 0.1% to 5%. By controlling the mass percentage of the cyclic compound containing a sulfur-oxygen double bond within the above range, the sulfur-oxygen double bond-containing compound and the compound of formula I can play a synergistic role in the film formation process, which is conducive to forming a more stable interface film on the surface of the silicon particles, so that the electrochemical device has good cycle stability.
[0019] In one embodiment of the present application, the silicon-based material includes at least one of a silicon-oxygen composite material or a silicon-carbon composite material, and an inorganic material exists on the surface of the silicon-oxygen composite material or the silicon-carbon composite material particles, and the inorganic material includes at least one of LiF, NaF, KF, MgF2, CaF2 or AlF3, and the mass percentage of the inorganic material is 0.5% to 2% based on the mass of the silicon-based material. By selecting the above-mentioned silicon-based material and inorganic material, and regulating the mass percentage of the inorganic material within the above-mentioned range, it is helpful to improve the stability of the negative electrode active particles, thereby improving the cycle performance of the electrochemical device.
[0020] In one embodiment of the present application, the electrolyte further comprises a first component, the first component comprising C2 to C 10 Linear carbonates or C2 to C 10 At least one of the linear carboxylates of C2 to C 10 The linear carbonate comprises at least one of dimethyl carbonate, diethyl carbonate or dipropyl carbonate, C2 to C 10The linear carboxylic acid ester includes at least one of propyl acetate, butyl acetate, ethyl propionate, propyl propionate, butyl propionate, ethyl butyrate, propyl butyrate, butyl butyrate, ethyl isobutyrate, propyl isobutyrate, butyl isobutyrate or isobutyl isobutyrate, and the mass percentage of the first component is 5% to 55% based on the total mass of the electrolyte. Linear carbonates and linear carboxylates have the characteristics of low viscosity. By adding them as co-solvents to the electrolyte, it is beneficial to improve the ionic conductivity of the overall electrolyte, so that the electrochemical device has good cycle stability.
[0021] The second aspect of the present application provides an electronic device, which includes the electrochemical device provided by the first aspect of the present application. Since the electrochemical device of the present application has good cycle stability, the electronic device of the present application has a long service life.
[0022] Beneficial effects of this application:
[0023] The present application provides an electrochemical device and an electronic device, wherein the electrochemical device comprises a negative electrode plate and an electrolyte, wherein the negative electrode plate comprises a negative electrode material layer, the negative electrode material layer comprises a silicon-based material, the silicon-based material comprises silicon element, and the mass percentage of silicon element is 30% to 60% based on the mass of the negative electrode material layer. The electrolyte comprises a compound of formula I and fluoroethylene carbonate (FEC), wherein R1 and R2 are each independently selected from a hydrogen atom, a fluorine atom, a substituted or unsubstituted C1 to C5 alkyl, a substituted or unsubstituted C6 to C 10 The compound of formula I includes NO2-R1-R2, which can form an interface film rich in inorganic substances such as Li3N and Li2O on the surface of silicon particles, and the compound of formula I has a preferential decomposition characteristic due to its decomposition potential earlier than FEC, thereby reducing the damage of the solid electrolyte interface film (SEI) film on the surface of silicon particles, thereby reducing the consumption rate of FEC, thereby improving the problem of poor cycle performance of the electrochemical device caused by excessive or insufficient FEC content in the electrochemical device containing negative electrode active materials of silicon element.
[0024] Of course, implementing any product or method of the present application does not necessarily require achieving all of the advantages described above at the same time. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.
[0026] It should be noted that in the specific implementation of the present application, lithium-ion batteries are used as an example of electrochemical devices to explain the present application, but the electrochemical devices of the present application are not limited to lithium-ion batteries. The specific technical solution is as follows:
[0027] The first aspect of the present application provides an electrochemical device, which includes a negative electrode plate and an electrolyte, wherein the negative electrode plate includes a negative electrode material layer, the negative electrode material layer includes a silicon-based material, the silicon-based material includes silicon element, and the mass percentage of silicon element is 30% to 60% based on the total mass of the negative electrode material layer; the electrolyte includes a compound of formula I and fluoroethylene carbonate:
[0028]
[0029] wherein R1 and R2 are each independently selected from a hydrogen atom, a fluorine atom, a substituted or unsubstituted C1 to C5 alkyl group, a substituted or unsubstituted C6 to C 10 The aryl group and the substituted or unsubstituted C2 to C6 carboxylate group, when substituted, the substituent in the carboxylate group, alkyl group and aryl group is a fluorine atom. The mass percentage of the silicon element mass is controlled within the above range, so that the electrochemical device can meet the space required for the expansion of the nano-silicon particles during the charging and discharging process, thereby effectively alleviating the phenomenon of the rupture of the negative electrode active material caused by the expansion of the nano-silicon particles, and improving the energy density and cycle performance of the electrochemical device. However, in the electrochemical device containing silicon-based materials, the lithium alloy formed after the silicon-based materials are lithiated has a highly active reactivity, resulting in rapid consumption of the electrolyte, thereby affecting the cycle performance of the electrochemical device. In order to alleviate the above problems, the inventors of the present application found that the compound of formula I is selected, and the compound of formula I includes NO2-R1-R2, which can form a Li3N, Li2O-rich electrolyte on the surface of the silicon particles. The compound of formula I contains an unsaturated bond, so its own decomposition potential is earlier than FEC and has a preferential decomposition characteristic, which reduces the damage of the SEI film on the surface of the silicon particles, thereby reducing the consumption rate of FEC. The compound of formula I also contains a carboxylate functional group, which has good ion conductivity and can ensure excellent ion transmission on the negative electrode side surface. Therefore, the compound of formula I is selected as a pre-film-forming additive to be combined with fluoroethylene carbonate. The interfacial film-forming characteristics of fluoroethylene carbonate can protect the electrolyte from continuous decomposition at the interface to a certain extent, and the consumption rate of fluoroethylene carbonate is reduced by the compound of formula I, thereby improving the cycle stability of the electrochemical device.
[0030] In one experimental scheme of the present application, the compound of formula I includes at least one of the following compounds:
[0031]
[0032]
[0033] By selecting the compound of formula I, the stability and flexibility of the formed interface film can be further enhanced, thereby further reducing the side reactions between the electrolyte and the negative electrode active material, thereby improving the cycle performance of the electrochemical device.
[0034] In one embodiment of the present application, based on the total mass of the electrolyte, the mass percentage of fluoroethylene carbonate is 1% to 30%. For example, the mass percentage of fluoroethylene carbonate can be 1%, 3%, 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30% or a range consisting of any two of the values. By controlling the mass percentage of fluoroethylene carbonate within the above range, FEC can better meet the use consumption of long-term cycles, thereby improving the cycle stability of the electrochemical device.
[0035] In one embodiment of the present application, the mass percentage of fluoroethylene carbonate is 10% to 30% based on the total mass of the electrolyte. For example, the mass percentage of fluoroethylene carbonate can be 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30% or a range consisting of any two of the values. By controlling the mass percentage of fluoroethylene carbonate within the above range, it is beneficial to make FEC better meet the long-term cycle consumption and further improve the cycle stability of the electrochemical device.
[0036] In one embodiment of the present application, based on the total mass of the electrolyte, the mass percentage of the compound of formula I is 0.01% to 5%. For example, the mass percentage of the compound of formula I can be 0.01%, 0.3%, 0.5%, 0.8%, 1%, 1.3%, 1.5%, 1.8%, 2%, 2.3%, 2.5%, 2.8%, 3%, 3.3%, 3.5%, 3.8%, 4%, 4.3%, 4.5%, 4.8%, 5% or a range consisting of any two of the values. By controlling the mass percentage of the compound of formula I within the above range, it is beneficial to improve the integrity of the interface film layer, and improve the problem of poor low temperature and rate discharge caused by the obstruction of interface ion transmission of the electrochemical device, thereby improving the cycle stability of the electrochemical device.
[0037] In one embodiment of the present application, based on the total mass of the electrolyte, the mass percentage of the compound of formula I is 0.1% to 2%. For example, the mass percentage of the compound of formula I can be 0.1%, 0.3%, 0.5%, 0.8%, 1%, 1.3%, 1.5%, 1.8%, 2% or a range consisting of any two of the values. By controlling the mass percentage of the compound of formula I within the above range, it is beneficial to better improve the integrity of the interface film layer, and better improve the problem of poor low temperature and rate discharge caused by the obstruction of interface ion transmission of the electrochemical device, thereby further improving the cycle stability of the electrochemical device.
[0038] In one embodiment of the present application, the electrolyte further includes a dinitrile compound, and the dinitrile compound includes at least one of succinonitrile, glutaronitrile, methylglutaronitrile, adiponitrile, pimelonitrile, suberonitrile, azelaic acid dinitrile or sebacate; based on the total mass of the electrolyte, the mass percentage of the dinitrile compound is 0.1% to 3%. For example, the mass percentage of the dinitrile compound can be 0.1%, 0.3%, 0.5%, 0.8%, 1%, 1.3%, 1.5%, 1.7%, 2%, 2.3%, 2.5%, 2.8%, 3% or a range consisting of any two of the values. By controlling the mass percentage of the dinitrile compound within the above range, it is beneficial to improve the stability of the above SEI film and reduce the reactivity of the negative electrode active material, thereby improving the problem of excessive consumption of the electrolyte, thereby improving the cycle stability of the electrochemical device.
[0039] In one embodiment of the present application, the electrolyte further comprises a cyclic compound containing a sulfur-oxygen double bond, and the cyclic compound containing a sulfur-oxygen double bond comprises at least one of 1,3-propane sultone, 1,4-butane sultone or 2,4-butane sultone; based on the total mass of the electrolyte, the mass percentage of the cyclic compound containing a sulfur-oxygen double bond is 0.1% to 5%. For example, the mass percentage of the cyclic compound containing a sulfur-oxygen double bond can be 0.1%, 0.3%, 0.5%, 0.8%, 1%, 1.3%, 1.5%, 1.7%, 2%, 2.3%, 2.5%, 2.8%, 3%, 3.3%, 3.5%, 3.8%, 4%, 4.3%, 4.5%, 4.8%, 5%, or a range consisting of any two of the values. By controlling the mass percentage of the cyclic compound containing sulfur-oxygen double bonds within the above range, the sulfur-oxygen double bond-containing compound and the compound of formula I can play a synergistic role in the film formation process, which is beneficial to forming a more stable interface film on the surface of silicon particles and reducing the side reactions between the silicon-based material and the electrolyte. Therefore, the electrochemical device has good cycle stability.
[0040] In one embodiment of the present application, the electrolyte further includes a first component, the first component including C2 to C 10Linear carbonates or C2 to C 10 At least one of the linear carboxylates of C2 to C 10 The linear carbonate comprises at least one of dimethyl carbonate, diethyl carbonate or dipropyl carbonate, C2 to C 10 The linear carboxylic acid ester includes at least one of propyl acetate, butyl acetate, ethyl propionate, propyl propionate, butyl propionate, ethyl butyrate, propyl butyrate, butyl butyrate, ethyl isobutyrate, propyl isobutyrate, butyl isobutyrate or isobutyl isobutyrate. Based on the total mass of the electrolyte, the mass percentage of the first component is 5% to 55%. For example, the mass percentage of the first component can be 5%, 7%, 10%, 13%, 15%, 17%, 20%, 23%, 25%, 27%, 30%, 33%, 35%, 37%, 40%, 43%, 45%, 47%, 50%, 53%, 55% or a range consisting of any two of the values. Linear carbonates and linear carboxylates have the characteristics of low viscosity. By adding them as co-solvents to the electrolyte, it is beneficial to improve the ionic conductivity of the overall electrolyte, so the electrochemical device has good cycle stability.
[0041] In one embodiment of the present application, the first component includes linear carbonate, and the mass percentage of the linear carbonate is 5% to 55% based on the total mass of the electrolyte. When the electrolyte includes the first compound, the electrochemical device has good cycle stability.
[0042] In one embodiment of the present application, the first component includes linear carboxylic acid ester, and the mass percentage of the linear carboxylic acid ester is 5% to 55% based on the total mass of the electrolyte. When the electrolyte includes the first compound, the electrochemical device has good cycle stability.
[0043] In one embodiment of the present application, the first component includes linear carbonate and linear carboxylate. In this case, there is no particular limitation on the mass percentage of each, as long as the total mass percentage of the first compounds meets the scope of the present application.
[0044] In the present application, the features of the different components contained in the above-mentioned electrolyte can be combined, and the implementation modes covered by the above-mentioned combination are all within the protection scope of the present application.
[0045] In the present application, the electrolyte also includes a lithium salt and a base solvent. The present application has no particular restrictions on the type of lithium salt, and lithium salts known in the art may be used. For example, the lithium salt may include but is not limited to at least one of LiBF4, LiPF6, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3 and LiPO2F2; the present application has no particular restrictions on the base solvent, as long as the purpose of the present application can be achieved. For example, the base solvent may include at least one of non-fluorinated cyclic carbonates, ether compounds, other linear carbonates, other linear carboxylates or other organic solvents; the ether compound may include but is not limited to at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran; the above-mentioned other linear carbonates include at least one of ethyl methyl carbonate, methyl propyl carbonate (MPC) or ethyl propyl carbonate (EPC). The above-mentioned non-fluorinated cyclic carbonates may include but are not limited to at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC) or vinyl ethylene carbonate (VEC). The above-mentioned other linear carboxylates include but are not limited to at least one of ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, methyl tert-butyrate, ethyl tert-butyrate, 2,2-difluoroethyl acetate, 2,2,2-trifluoroethyl acetate, hexafluoroisopropyl acetate, 2,2-difluoroethyl propionate, 2,2,2-trifluoroethyl propionate or hexafluoroisopropyl propionate. The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, cyclopentane, methyl cyclopentane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, trimethyl phosphate, triethyl phosphate, trioctyl phosphate or phosphate. The present application has no particular restrictions on the mass percentage of lithium salts and other basic solvents in the electrolyte, as long as the purpose of the present application can be achieved. For example, based on the mass of the electrolyte, the mass percentage of the lithium salt may be 8% to 20%, and the mass percentage of the base solvent may be 0% to 92%.
[0046] In one embodiment of the present application, the electrolyte may include a compound of formula I, FEC, a lithium salt, and a base solvent; the mass percentages of the compound of formula I, FEC, and the lithium salt are as described above, and the mass percentage of the base solvent is 45% to 91.89% based on the mass of the electrolyte. The electrochemical device including the above electrolyte also has good cycle stability.
[0047] In one embodiment of the present application, the electrolyte may include a compound of formula I, FEC, a lithium salt, a dinitrile compound, and a base solvent; the mass percentages of the compound of formula I, FEC, the lithium salt, and the dinitrile compound are as described above, and the mass percentage of the base solvent is 42% to 91.79% based on the mass of the electrolyte. The electrochemical device including the above electrolyte also has good cycle stability.
[0048] In one embodiment of the present application, the electrolyte may include a compound of formula I, FEC, a lithium salt, a cyclic compound containing a sulfur-oxygen double bond, and a base solvent; the mass percentages of the compound of formula I, FEC, the lithium salt, and the cyclic compound containing a sulfur-oxygen double bond are as described above, and the mass percentage of the base solvent is 40% to 91.79% based on the mass of the electrolyte. The electrochemical device including the above electrolyte also has good cycle stability.
[0049] In one embodiment of the present application, the electrolyte may include a compound of formula I, FEC, a lithium salt, a first component, and a base solvent; the mass percentages of the compound of formula I, FEC, the lithium salt, and the first component are as described above, and the mass percentage of the base solvent is 0% to 86.89% based on the mass of the electrolyte. The electrochemical device including the above electrolyte also has good cycle stability.
[0050] In one embodiment of the present application, the electrolyte may include a compound of formula I, FEC, a lithium salt, a dinitrile compound, a cyclic compound containing a sulfur-oxygen double bond, and a base solvent; the mass percentages of the compound of formula I, FEC, a lithium salt, a dinitrile compound, and a cyclic compound containing a sulfur-oxygen double bond are as described above, and the mass percentage of the base solvent is 37% to 91.69% based on the mass of the electrolyte. The electrochemical device including the above electrolyte also has good cycle stability.
[0051] In one embodiment of the present application, the electrolyte may include a compound of formula I, FEC, a lithium salt, a dinitrile compound, a first component, and a base solvent; the mass percentages of the compound of formula I, FEC, a lithium salt, a dinitrile compound, and the first component are as described above, and the mass percentage of the base solvent is 0% to 86.79% based on the mass of the electrolyte. The electrochemical device including the above electrolyte also has good cycle stability.
[0052] In one embodiment of the present application, the electrolyte may include a compound of formula I, FEC, a lithium salt, a dinitrile compound, a first component, and a base solvent; the mass percentages of the compound of formula I, FEC, a lithium salt, a dinitrile compound, and the first component are as described above, and the mass percentage of the base solvent is 0% to 86.79% based on the mass of the electrolyte. The electrochemical device including the above electrolyte also has good cycle stability.
[0053] In one embodiment of the present application, the electrolyte may include a compound of formula I, FEC, a lithium salt, a dinitrile compound, a cyclic compound containing a sulfur-oxygen double bond, a first component, and a base solvent; the mass percentages of the compound of formula I, FEC, a lithium salt, a dinitrile compound, a cyclic compound containing a sulfur-oxygen double bond, and the first component are as described above, and the mass percentage of the base solvent is 0% to 86.69% based on the mass of the electrolyte. The electrochemical device including the above electrolyte also has good cycle stability.
[0054] In the present application, the electrochemical device also includes a negative electrode plate, which includes a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector. The above-mentioned "negative electrode material layer disposed on at least one surface of the negative electrode current collector" means that the negative electrode material layer can be disposed on one surface of the negative electrode current collector along its own thickness direction, or on two surfaces of the negative electrode current collector along its own thickness direction. It should be noted that the "surface" here can be the entire area of the negative electrode current collector or a partial area of the negative electrode current collector. This application has no special restrictions, as long as the purpose of this application can be achieved.
[0055] In one embodiment of the present application, the silicon-based material includes at least one of a silicon-oxygen composite material or a silicon-carbon composite material, and the inorganic material present on the surface of the silicon-oxygen composite material or the silicon-carbon composite material particles includes at least one of LiF, NaF, KF, MgF2, CaF2 or AlF3, and the mass percentage of the inorganic material is 0.5% to 2% based on the mass of the silicon-based material. For example, the mass percentage of the inorganic material can be 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2% or a range consisting of any two of the values. By selecting the above-mentioned silicon-based materials and inorganic materials, and regulating the mass percentage of the inorganic materials within the above-mentioned range, it is helpful to improve the stability of the negative electrode active particles, thereby helping to further buffer the volume expansion of silicon during the electrochemical process, and further improving the cycle performance and high temperature storage performance of the electrochemical device.
[0056] The present application has no particular restrictions on the preparation method of silicon-based materials. Exemplarily, the preparation method of silicon-based materials may include but is not limited to the following steps: silicon-containing material and surface inorganic material are added to an organic solvent according to a certain mass ratio to form a suspension, mixed to obtain a mixture, filtered, dried, and a silicon-oxygen composite material or a silicon-carbon composite material is obtained. The present application has no particular restrictions on organic solvents, as long as the purpose of the present application can be achieved, for example, the organic solvent can be ethanol. The present application has no particular restrictions on silicon-containing material, as long as the purpose of the present application can be achieved, for example, silicon-containing material can be selected from at least one of microporous carbon material, silicon-carbon material, silicon-oxygen material, micron silicon, Si-Sn alloy, Si-Mg alloy, Si-Ge alloy or Si-Zn alloy loaded with nano-silicon.
[0057] The present application has no special restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the negative electrode current collector may include but is not limited to copper foil, aluminum foil, nickel foil or carbon-based current collector, for example, the thickness of the negative electrode current collector is 4μm to 12μm. The present application has no special restrictions on the thickness of the negative electrode material layer, as long as the purpose of the present application can be achieved, for example, the thickness of the single-sided negative electrode material layer is 30μm to 150μm. The present application has no special restrictions on the thickness of the negative electrode sheet, as long as the purpose of the present application can be achieved, for example, the thickness of the negative electrode sheet is 50μm to 350μm. The negative electrode material layer of the present application may also include a conductive agent and a binder.
[0058] The negative electrode active material of the present application may also include a carbon material, which may be selected from natural graphite, artificial graphite, mesophase microcarbon beads, hard carbon, soft carbon, silicon, silicon-carbon composites, Li-Sn alloys, Li-Sn-O alloys, Sn, SnO, SnO2, spinel-structured lithiated TiO2-Li4Ti5O 12 or at least one of Li-Al alloys. Based on the total mass of the negative electrode material layer, the mass percentage of the carbon material may be 10% to 70%.
[0059] The above-mentioned conductive agent and binder are not particularly limited, as long as the purpose of the present application can be achieved. For example, the conductive agent may include at least one of conductive carbon black, lamellar graphite, graphene, carbon nanotubes, carbon nanowires or carbon fibers. Conductive carbon black may include at least one of acetylene black and Ketjen black. The binder may include at least one of lithium polyacrylate, polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer, styrene-acrylate copolymer, styrene-butadiene copolymer, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylic acid salt, sodium carboxymethyl cellulose (CMC-Na), polyvinyl acetate, polyvinyl pyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, polyhexafluoropropylene, styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), polyaniline, polyimide, polyamide-imide, polysiloxane, epoxy resin, polyester resin, polyurethane resin or polyfluorene.
[0060] Optionally, the negative electrode plate may further include a conductive layer, which is located between the negative electrode current collector and the negative electrode material layer. The present application has no particular restrictions on the composition of the conductive layer, which may be a conductive layer commonly used in the art. The conductive layer includes a conductive agent and a binder. The present application has no particular restrictions on the conductive agent and the binder in the conductive layer, which may be at least one of the above conductive agent and the above binder. The present application has no particular restrictions on the mass ratio of the conductive agent and the binder in the conductive layer, and those skilled in the art may choose according to actual needs, as long as the purpose of the present application can be achieved. The present application has no particular restrictions on the thickness of the conductive layer, as long as the purpose of the present application can be achieved, for example, the thickness of the conductive layer is 1μm to 10μm. The electrochemical device of the present application also includes a positive electrode plate and a separator.
[0061] In the present application, the positive electrode plate includes a positive electrode current collector and a positive electrode material layer arranged on at least one surface of the positive electrode current collector. The above-mentioned "positive electrode material layer arranged on at least one surface of the positive electrode current collector" means that the positive electrode material layer can be arranged on one surface of the positive electrode current collector along its own thickness direction, or it can be arranged on two surfaces of the positive electrode current collector along its own thickness direction. It should be noted that the "surface" here can be the entire area of the positive electrode current collector or a partial area of the positive electrode current collector. This application has no special restrictions, as long as the purpose of this application can be achieved. This application has no special restrictions on the positive electrode current collector, as long as the purpose of this application can be achieved. For example, it can include aluminum foil, aluminum alloy foil or a composite current collector (such as an aluminum-carbon composite current collector).
[0062] The positive electrode material layer of the present application includes a positive electrode active material, and the positive electrode active material includes a substance that can reversibly embed and extract active ions such as lithium ions. The positive electrode material layer can be one or more layers, and each layer in the multilayer positive electrode material layer can contain the same or different positive electrode active materials. The present application has no particular restrictions on the positive electrode active material, as long as the purpose of the present application can be achieved. For example, the positive electrode active material may include but is not limited to lithium nickel cobalt manganese oxide (such as NCM811, NCM622, NCM523, NCM111), lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide (LiCoO2), lithium manganese oxide, lithium iron manganese phosphate or lithium titanate. At least one of the positive electrode material layer of the present application also includes a conductive agent and a binder. The present application has no particular restrictions on the conductive agent and the binder in the positive electrode material layer, as long as the purpose of the present application can be achieved. For example, the conductive agent may include but is not limited to at least one of conductive carbon black, carbon nanotubes (CNTs), carbon fibers, flake graphite, graphene, metal materials or conductive polymers. The above-mentioned conductive carbon black may include but is not limited to Super P, acetylene black or Ketjen black. The above-mentioned carbon nanotubes may include but are not limited to single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The above-mentioned carbon fibers may include but are not limited to vapor-grown carbon fibers (VGCF) and / or nanocarbon fibers. The above-mentioned metal materials may include but are not limited to metal powders and / or metal fibers, and specifically, the metal may include but is not limited to at least one of copper, nickel, aluminum or silver. The above-mentioned conductive polymers may include but are not limited to at least one of polyphenylene derivatives, polyaniline, polythiophene, polyacetylene or polypyrrole. The binder may include but is not limited to polyacrylate, polyimide, polyamide, polyamide-imide, polyvinylidene fluoride, polystyrene butadiene copolymer (styrene-butadiene rubber, SBR), sodium alginate, polyvinyl alcohol, polytetrafluoroethylene, polyacrylonitrile, sodium carboxymethyl cellulose (CMC-Na), potassium carboxymethyl cellulose, sodium hydroxymethyl cellulose or potassium hydroxymethyl cellulose. The present application does not particularly limit the mass ratio of the positive active material, the conductive agent and the binder in the positive electrode material layer, and those skilled in the art may select according to actual needs, as long as the purpose of the present application can be achieved.
[0063] The present application has no particular restrictions on the thickness of the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode current collector is 5 μm to 20 μm, preferably 6 μm to 18 μm. The present application has no particular restrictions on the thickness of the positive electrode material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the single-sided positive electrode material layer is 30 μm to 120 μm.
[0064] The present application has no particular restrictions on the isolation membrane, as long as the purpose of the present application can be achieved. For example, the isolation membrane may include at least one of polyethylene, polypropylene, polyvinylidene fluoride, polyethylene terephthalate, polyimide or aramid, etc., polyethylene and polypropylene can prevent short circuits, and can also improve the stability of electrochemical devices through the shutdown effect. For example, polyethylene can include at least one of high-density polyethylene, low-density polyethylene or ultra-high molecular weight polyethylene. The surface of the isolation membrane may include a porous layer, the porous layer is arranged on at least one surface of the isolation membrane, the porous layer may include at least one of inorganic particles or binders, and the porous layer can improve the heat resistance, oxidation resistance and electrolyte wetting performance of the isolation membrane, and enhance the adhesion between the isolation membrane and the pole piece. There is no particular restriction on the size of the pore size, as long as the purpose of the present application can be achieved, for example, the size of the pore size can be 0.01μm to 1μm. In the present application, the thickness of the isolation membrane can be 5μm to 30μm. The present application has no particular restrictions on the above-mentioned inorganic particles, as long as the purpose of the present application can be achieved. For example, the inorganic particles may include at least one of aluminum oxide (Al2O3), silicon oxide (SiO), magnesium oxide (MgO), titanium oxide (TiO2), hafnium dioxide (HfO2), tin oxide (SnO2), cerium dioxide (CeO2), nickel oxide (NiO), zinc oxide (ZnO), calcium oxide (CaO), zirconium oxide (ZrO2), yttrium oxide (Y2O3), silicon carbide (SiC), boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate, etc. For example, the binder of the porous layer may include at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, sodium carboxymethyl cellulose, polyvinyl pyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene or polyhexafluoropropylene, etc.
[0065] The preparation process of the electrochemical device is well known to those skilled in the art, and the present application has no particular limitation. For example, it may include but is not limited to the following steps: stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and winding, folding and other operations as needed to obtain an electrode assembly of a wound structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain an electrochemical device; or, stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and then fixing the four corners of the entire stacked structure with tape to obtain an electrode assembly of a stacked structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain an electrochemical device. In addition, overcurrent protection elements, guide plates, etc. may also be placed in the packaging bag as needed to prevent the pressure inside the electrochemical device from rising and overcharging and discharging. The present application does not limit the packaging bag, and those skilled in the art may select it according to actual needs, as long as the purpose of the present application can be achieved. For example, an aluminum-plastic film packaging bag may be used.
[0066] The second aspect of the present application provides an electronic device, which includes the electrochemical device provided by the first aspect of the present application. Since the electrochemical device of the present application has good cycle stability and high-temperature storage performance, the electronic device of the present application has a long service life.
[0067] The electronic device of the present application is not particularly limited, and it can be any electronic device known in the prior art. In some embodiments, the electronic device can include but is not limited to a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery or a lithium-ion capacitor, etc.
[0068] Example
[0069] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.
[0070] Test methods and equipment:
[0071] Cycle performance test:
[0072] Place the lithium-ion battery in a 25°C constant temperature test box and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature. Charge it to 4.45V at a constant current of 0.5C, then charge it to a current of 0.025C at a constant voltage of 4.45V, let it stand for 5 minutes, and discharge it to 3.0V at a constant current of 0.5C, and record it as the initial discharge capacity C1. Repeat this step for 200 cycles, record the discharge capacity C2 after 200 cycles, and calculate the cycle capacity retention rate of the lithium-ion battery. Cycle capacity retention rate (%) = C2 / C1×100%.
[0073] Cyclic thickness growth rate test:
[0074] Charge at a constant current of 0.5C to 4.45V, then charge at a constant voltage to a current of 0.025C, let stand for 5 minutes, measure the thickness, and count it as the thickness of the lithium-ion battery when it is fully charged for the first time; use the same charge and discharge process as in the above-mentioned cycle capacity retention test, cycle 500 times, measure the thickness, and count it as the thickness of the lithium-ion battery after the 500th cycle.
[0075] The difference between the thickness of the lithium-ion battery after the 500th cycle and the thickness of the lithium-ion battery when it is fully charged for the first time is divided by the thickness of the lithium-ion battery when it is fully charged for the first time. The thickness of the lithium-ion battery is measured with a micrometer, and 5 measurements are taken at 5 different positions to take the average value, which is the cycle thickness growth rate. The smaller the cycle thickness growth rate, the better.
[0076] Test of silicon mass percentage:
[0077] The lithium-ion battery discharged at 0.5C to 3.0V was disassembled, the negative electrode was removed, and it was soaked in dimethyl carbonate (DMC) for 20 minutes, and then rinsed with DMC and acetone in turn. Then the negative electrode was placed in an oven and baked at 80°C for 12 hours to obtain the negative electrode. The negative electrode was dried in a vacuum oven at 100°C for 24 hours, and 1g of the powdered sample of the negative electrode material layer on the negative electrode was scraped off with a blade, and then the mass percentage of silicon in the negative electrode material layer was tested using an inductively coupled plasma (ICP) analyzer.
[0078] Example 1-1
[0079] <Preparation of positive electrode sheet>
[0080] The positive electrode active material lithium cobalt oxide, conductive carbon black, and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 95:2.5:2.5, and then N-methylpyrrolidone (NMP) is added as a solvent to prepare a slurry with a solid content of 75%, and stirred evenly. The slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 10μm, and dried at 90°C to obtain a positive electrode sheet with a coating thickness of 110μm. After the above steps are completed, the single-sided coating of the positive electrode sheet is completed. After that, the above steps are repeated on the other surface of the positive electrode sheet to obtain a positive electrode sheet with double-sided coating of positive electrode active materials. After the coating is completed, cold pressing is then performed, and the positive electrode sheet is cut into a specification of 74mm×867mm and welded to the pole ear for standby use. The thickness of the single-sided positive electrode material layer after cold pressing is 75μm, and the compaction density of the positive electrode material layer is 4g / cm 3 .
[0081] <Preparation of Silicon-Based Materials>
[0082] The nano-silicon loaded microporous carbon material and the inorganic material LiF are added to an ethanol solution at a mass ratio of 99:1 to form a suspension, and ball milling is performed to mix and disperse uniformly to obtain a mixture, and after filtering and drying, a silicon-carbon composite material with the inorganic material LiF on the surface is obtained. Among them, the carbon content in the nano-silicon loaded microporous carbon material is 50%; based on the mass of the silicon-based material, the mass percentage of the inorganic material LiF is 1%.
[0083] <Preparation of negative electrode sheet>
[0084] The silicon-based material, artificial graphite, carbon nanotubes, and lithium polyacrylate prepared above are mixed in a mass ratio of 80:10:2:8, deionized water is added, and the mixture is mixed evenly under the action of a vacuum mixer to obtain a negative electrode slurry with a solid content of 30wt%. The negative electrode slurry is evenly coated on one side of a negative electrode current collector copper foil with a thickness of 12μm, and dried at 120°C to obtain a negative electrode sheet with a single-sided negative electrode active material layer coated with a coating thickness of 143μm, and then the above steps are repeated on the other side of the copper foil to obtain a negative electrode sheet with a double-sided negative electrode active material layer coated, and then cold pressed and cut to obtain a negative electrode sheet with a specification of 78mm×875mm. Among them, based on the mass of the negative electrode active material layer, the mass percentage of silicon element is 39.6%. The thickness of the single-sided negative electrode active material layer after cold pressing is 80μm, and the compaction density of the negative electrode material layer is 1g / cm 3 .
[0085] <Preparation of Electrolyte>
[0086] In an argon atmosphere glove box with a water content of less than 10ppm, ethylene carbonate, ethyl methyl carbonate, and ethyl acetate are mixed in a mass ratio of 3:3:4 to obtain a base solvent, and then lithium salt lithium hexafluorophosphate (LiPF6), fluoroethylene carbonate, and the compound of formula I-1 are added and mixed evenly to obtain an electrolyte. Wherein, based on the mass of the electrolyte, the mass percentage of lithium salt lithium hexafluorophosphate is 12.5%, the mass percentage of fluoroethylene carbonate is 20%, and the mass percentage of the compound of formula I-1 is 5%. The remainder is the base solvent.
[0087] <Preparation of Separator Film>
[0088] A polyethylene (PE) film with a thickness of 15 μm (provided by Celgard) was used.
[0089] <Preparation of lithium-ion batteries>
[0090] The positive electrode sheet, separator, and negative electrode sheet prepared above are stacked in order, so that the separator is located between the positive electrode and the negative electrode to play an isolating role, and then wound to obtain an electrode assembly. The electrode assembly is placed in an aluminum-plastic film packaging bag, and after drying, the electrolyte is injected, and a lithium-ion battery is obtained through vacuum packaging, standing, formation, degassing, trimming, and other processes.
[0091] Example 1-2 to Example 1-8
[0092] Except that the mass percentage of the compound of formula I-1 and fluoroethylene carbonate is adjusted according to Table 1 in <Preparation of electrolyte>, the mass percentage of the base solvent is changed accordingly, and the mass percentage of LiPF6 remains unchanged, the rest is the same as Example 1-1.
[0093] Example 1-9 to Example 1-11
[0094] Except for adjusting the type of compound of formula I according to Table 1 in <Preparation of electrolyte>, the rest is the same as Example 1-2.
[0095] Example 1-12 to Example 1-13
[0096] Except that the mass ratio parameters of silicon-based material and artificial graphite are adjusted in <Preparation of Negative Electrode Plate> so that the mass percentage of silicon element in the negative electrode material layer is as shown in Table 1, and the mass percentage of carbon nanotubes and lithium polyacrylate remain unchanged, the rest is the same as Example 1-2.
[0097] Example 1-14 to Example 1-17
[0098] Except that the mass percentage of the compound of formula I-1 and fluoroethylene carbonate is adjusted according to Table 1 in <Preparation of electrolyte>, the mass percentage of the base solvent is changed accordingly, and the mass percentage of LiPF6 remains unchanged, the rest is the same as Example 1-1.
[0099] Example 2-1 to Example 2-3
[0100] Except that the dinitrile compound is added according to Table 2 and its mass percentage is adjusted in <Preparation of Electrolyte>, the mass percentage of the base solvent changes accordingly, the mass ratio of each component of the base solvent remains unchanged, and the mass percentage of LiPF6 remains unchanged, the rest is the same as Example 1-2.
[0101] Example 3-1 to Example 3-3
[0102] Except that a cyclic compound containing a sulfur-oxygen double bond is added and its mass percentage is adjusted in accordance with Table 3 in <Preparation of Electrolyte>, the mass percentage of the base solvent changes accordingly, the mass ratio of each component of the base solvent remains unchanged, and the mass percentage of LiPF6 remains unchanged, the rest is the same as Example 1-2.
[0103] Example 4-1 to Example 4-6
[0104] The preparation of the electrolyte is the same as in Example 1-2 except that the cyclic compound and dinitrile compound containing a sulfur-oxygen double bond are added according to Table 4 and their mass percentages are adjusted, the mass percentage of the base solvent changes accordingly, the mass ratio of the components of the base solvent remains unchanged, and the mass percentage of LiPF6 remains unchanged.
[0105] Example 5-1 to Implementation 5-4
[0106] Except that the type of inorganic material on the surface of the silicon-based material particles and its mass percentage are adjusted according to Table 5 in <Preparation of Silicon-Based Material>, the rest is the same as Example 1-2.
[0107] Example 6-1 to Example 6-9
[0108] Except that the first component is added to <Preparation of Electrolyte> according to Table 6 and its mass percentage and type are adjusted, the mass percentage of the base solvent changes accordingly, the mass ratio of each component of the base solvent remains unchanged, and the mass percentage of the compound of formula I-1, FEC and LiPF6 remains unchanged, the rest is the same as Example 1-2.
[0109] Examples 6-10
[0110] Except that the dinitrile compound is added to <Preparation of Electrolyte> according to Table 6 and its mass percentage is adjusted, the mass percentage of the base solvent changes accordingly, the mass ratio of the components of the base solvent remains unchanged, the mass percentage of the compound of formula I-1, FEC and LiPF6 remains unchanged, and the mass percentage of the first component remains unchanged, the rest is the same as Example 6-8.
[0111] Embodiment 6-11
[0112] Except that a cyclic compound containing a sulfur-oxygen double bond is added to <Preparation of Electrolyte> according to Table 6 and its mass percentage is adjusted, the mass percentage of the base solvent changes accordingly, the mass ratio of the components of the base solvent remains unchanged, the mass percentage of the compound of Formula I-1, FEC and LiPF6 remains unchanged, and the mass percentage of the first component remains unchanged, the rest is the same as Example 6-8.
[0113] Examples 6-12
[0114] Except for adjusting the relevant parameters according to Table 6, the rest is the same as Example 6-10.
[0115] Comparative Example 1 to Comparative Example 2
[0116] Except that the relevant parameters of the mass percentage of the compound of formula I-1 and fluoroethylene carbonate are adjusted according to Table 1 in <Preparation of electrolyte>, the mass percentage of the base solvent changes accordingly, the mass ratio of the components of the base solvent remains unchanged, and the mass percentage of LiPF6 remains unchanged, the rest is the same as Example 1-1.
[0117] The preparation parameters and performance parameters of each embodiment and comparative example are shown in Tables 1 to 6.
[0118] Table 1
[0119]
[0120]
[0121] Note: (1) The “ / ” in Table 1 indicates that there is no corresponding preparation parameter, substance or performance parameter. (2) Taking Example 1-10 as an example, the “type of compound of formula I” is “formula I-14+formula I-18”, and the “mass percentage content of compound of formula I” is “1+2”, which means that the compound of formula I includes formula I-14 and formula I-18. Based on the total mass of the electrolyte, the mass percentage content of formula I-14 is 1%, and the mass percentage content of formula I-18 is 2%. The same applies to other examples.
[0122] From Example 1-1 to Example 1-17, Comparative Example 1 to Comparative Example 2, it can be seen that the present application selects an electrolyte including a compound of Formula I and fluoroethylene carbonate, and regulates the mass percentage of silicon in the negative electrode material layer within the scope of the present application. In the embodiments of the present application, the lithium ion battery has a higher capacity retention rate and / or a lower thickness growth rate, indicating that the lithium ion battery has good cycle stability. The electrolyte in Comparative Example 1 does not include fluoroethylene carbonate, and the electrolyte in Comparative Example 2 does not include a compound of Formula I. The obtained lithium ion battery has a lower capacity retention rate and / or a higher thickness growth rate, indicating that the cycle stability of the lithium ion battery is poor.
[0123] In the electrolyte, the type and mass percentage of the compound of formula I usually affect the cycle stability of the electrochemical device. From Examples 1-1 to 1-5, and Examples 1-10 to 1-17, it can be seen that when the mass percentage of the compound of formula I is adjusted within the scope of the present application, the lithium-ion battery has a higher capacity retention rate and a lower thickness growth rate, indicating that the lithium-ion battery has good cycle stability.
[0124] In the electrolyte, the mass percentage of FEC usually affects the cycle stability of the electrochemical device. From Examples 1-2, 1-6 to 1-8, and 1-14 to 1-17, it can be seen that when the mass percentage of FEC is adjusted within the scope of the present application, the lithium-ion battery has a higher capacity retention rate and a lower thickness growth rate, indicating that the lithium-ion battery has good cycle stability.
[0125] Table 2
[0126]
[0127] Note: (1) The “ / ” in Table 2 indicates that there is no corresponding preparation parameter, substance or performance parameter. (2) Taking Example 2-3 as an example, the “type of dinitrile compound” is “sebaconitrile + methylglutaronitrile” and the “mass percentage of dinitrile compound” is “1.5+1.5”, which means that the dinitrile compound includes sebaconitrile and methylglutaronitrile. Based on the total mass of the electrolyte, the mass percentage of sebaconitrile is 1.5%, and the mass percentage of methylglutaronitrile is 1.5%.
[0128] The type and mass percentage of dinitrile compounds usually affect the cycle stability of lithium-ion batteries. It can be seen from Examples 1-2 and 2-1 to 2-3 that when dinitrile compounds are further added to the electrolyte and the type and content of the dinitrile compounds are within the scope of this application, the obtained lithium-ion battery has a higher cycle capacity retention rate and a lower thickness growth rate, indicating that the lithium-ion battery has good cycle stability.
[0129] Table 3
[0130]
[0131] Note: (1) The “ / ” in Table 3 indicates that there is no corresponding preparation parameter, substance or performance parameter. Taking Example 3-3 as an example, the “type of cyclic compound containing sulfur-oxygen double bond” is “1,4-butane sultone + 2,4-butane sultone”, and the “mass percentage of cyclic compound containing sulfur-oxygen double bond” is “2+3”, which means that the cyclic compound containing sulfur-oxygen double bond includes 1,4-butane sultone and 2,4-butane sultone. Based on the total mass of the electrolyte, the mass percentage of 1,4-butane sultone is 2%, and the mass percentage of 2,4-butane sultone is 3%.
[0132] The type and mass percentage of the cyclic compound containing a sulfur-oxygen double bond usually affect the cycle stability of the lithium-ion battery. It can be seen from Examples 1-2 and 3-1 to 3-3 that when the electrolyte further adds a cyclic compound containing a sulfur-oxygen double bond, and the type and content of the cyclic compound containing a sulfur-oxygen double bond are within the scope of this application, the obtained lithium-ion battery has a higher cycle capacity retention rate and a lower thickness growth rate, indicating that the lithium-ion battery has good cycle stability.
[0133] Table 4
[0134]
[0135] Note: (1) The “ / ” in Table 4 indicates that there is no corresponding preparation parameter, substance or performance parameter. (2) Taking Example 4-5 as an example, the “type of cyclic compound containing sulfur-oxygen double bond” is “1,3-propane sultone + 2,4-butane sultone”, the “type of dinitrile compound” is “octanedinitrile + adiponitrile”, the “mass percentage of cyclic compound containing sulfur-oxygen double bond” is “1+1.5”, and the “mass percentage of dinitrile compound” is “0.5+1”, indicating that the cyclic compound containing sulfur-oxygen double bond includes 1,3-propane sultone and 2,4-butane sultone, and the dinitrile compound includes octanedinitrile and adiponitrile. Based on the total mass of the electrolyte, the mass percentage of 1,3-propane sultone is 1%, the mass percentage of 2,4-butane sultone is 1.5%, the mass percentage of octanedinitrile is 0.5%, and the mass percentage of adiponitrile is 1%. The same applies to other examples.
[0136] It can be seen from Examples 1-2, 2-2, 3-2, 4-1 to 4-6 that by simultaneously adding a dinitrile compound and a cyclic compound containing a sulfur-oxygen double bond into the electrolyte, and when their types and mass percentages are within the scope of the present application, the lithium-ion battery has a higher cycle capacity retention rate and a lower thickness growth rate, indicating that the lithium-ion battery has good cycle stability.
[0137] Table 5
[0138]
[0139]
[0140] Note: (1) Taking Example 5-2 as an example, the "type of inorganic material on the surface of silicon-based material particles" is "NaF+MgF2" and the "mass percentage of inorganic material on the surface of silicon-based material particles" is "1+0.5", which means that the inorganic material on the surface of silicon-based material particles includes NaF and MgF2. Based on the total mass of the silicon-based material, the mass percentage of NaF is 1%, and the mass percentage of MgF2 is 0.5%. The same applies to other examples.
[0141] The type of silicon-based material and the type and content of inorganic materials present on the particle surface usually affect the cycle stability of lithium-ion batteries. It can be concluded from Examples 1-2, 5-1 to 5-4 that, when inorganic materials are present on the surface of silicon-based materials and the type and content of inorganic materials are within the above range, lithium-ion batteries have a higher cycle capacity retention rate and a lower thickness growth rate, indicating that lithium-ion batteries have good cycle stability.
[0142] Table 6
[0143]
[0144]
[0145] “ / ” in Table 6 indicates that there is no corresponding preparation parameter, substance or performance parameter.
[0146] The type and content of the first component usually affect the cycle stability of the lithium-ion battery. It can be concluded from Examples 1-2, 6-1 to 6-9 that when the type and content of the first component are within the above range, the lithium-ion battery has a higher cycle capacity retention rate and a lower thickness growth rate, indicating that the lithium-ion battery has good cycle stability.
[0147] The composition of the electrolyte usually affects the cycle stability of the lithium-ion battery. It can be concluded from Examples 1-2, 2-2, 3-2, 6-10 to 6-12 that when a dinitrile compound or a cyclic compound containing a sulfur-oxygen double bond is added to the electrolyte comprising the first component, the composition of the electrolyte is still within the scope of the present application, and the lithium-ion battery has a higher cycle capacity retention rate and a lower thickness growth rate, indicating that the lithium-ion battery has good cycle stability.
[0148] The terms "comprises," "comprising," or any other variations thereof are intended to cover a non-exclusive inclusion such that a process, method, or article that comprises a list of elements includes not only those elements but also includes other elements not expressly listed or that are inherent to such process, method, or article.
[0149] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.
[0150] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. An electrochemical device comprising a negative electrode plate and an electrolyte, wherein; The negative electrode plate comprises a negative electrode material layer, the negative electrode material layer comprises a silicon-based material, the silicon-based material comprises silicon element, and based on the total mass of the negative electrode material layer, the mass percentage of the silicon element is 30% to 60%; The electrolyte comprises fluoroethylene carbonate and a compound of formula I: in, R1 and R2 are each independently selected from a hydrogen atom, a fluorine atom, a substituted or unsubstituted C1 to C5 alkyl group, a substituted or unsubstituted C6 to C 10 an aryl group and a substituted or unsubstituted C2 to C6 carboxylate group, and when substituted, the substituent in the carboxylate group, the alkyl group and the aryl group is a fluorine atom.
2. The electrochemical device according to claim 1, wherein: The compound of formula I comprises at least one of the following compounds:
3. The electrochemical device according to claim 1, wherein Based on the total mass of the electrolyte, the mass percentage of the fluoroethylene carbonate is 1% to 30%.
4. The electrochemical device according to claim 1, wherein Based on the total mass of the electrolyte, the mass percentage of the fluoroethylene carbonate is 10% to 30%.
5. The electrochemical device according to claim 1, wherein Based on the total mass of the electrolyte, the mass percentage of the compound of formula I is 0.01% to 5%.
6. The electrochemical device according to claim 1, wherein Based on the total mass of the electrolyte, the mass percentage of the compound of formula I is 0.1% to 2%.
7. The electrochemical device according to claim 1, wherein: The electrolyte further includes a dinitrile compound, wherein the dinitrile compound includes at least one of succinonitrile, glutaronitrile, methylglutaronitrile, adiponitrile, pimelonitrile, suberonitrile, azelaic acid dinitrile or sebacononitrile; Based on the total mass of the electrolyte, the mass percentage of the dinitrile compound is 0.1% to 3%.
8. The electrochemical device according to claim 1, wherein The electrolyte further comprises a cyclic compound containing a sulfur-oxygen double bond, wherein the cyclic compound containing a sulfur-oxygen double bond comprises at least one of 1,3-propane sultone, 1,4-butane sultone or 2,4-butane sultone; Based on the total mass of the electrolyte, the mass percentage of the cyclic compound containing sulfur-oxygen double bonds is 0.1% to 5%.
9. The electrochemical device according to claim 1, wherein: The silicon-based material includes at least one of a silicon-oxygen composite material or a silicon-carbon composite material, and inorganic materials exist on the surface of the silicon-oxygen composite material or silicon-carbon composite material particles, and the inorganic materials include at least one of LiF, NaF, KF, MgF2, CaF2 or AlF3; Based on the mass of the silicon-based material, the mass percentage of the inorganic material is 0.5% to 2%.
10. The electrochemical device according to claim 1, wherein The electrolyte also includes a first component, the first component includes C2 to C 10 Linear carbonates or C2 to C 10 At least one of the linear carboxylates of The C2 to C 10 The linear carbonate comprises at least one of dimethyl carbonate, diethyl carbonate or dipropyl carbonate; The C2 to C 10 The linear carboxylic acid ester comprises at least one of propyl acetate, butyl acetate, ethyl propionate, propyl propionate, butyl propionate, ethyl butyrate, propyl butyrate, butyl butyrate, ethyl isobutyrate, propyl isobutyrate, butyl isobutyrate or isobutyl isobutyrate; Based on the total mass of the electrolyte, the mass percentage of the first component is 5% to 55%.
11. An electronic device comprising the electrochemical device according to any one of claims 1 to 10.