Secondary battery and electric device

By arranging a coating in the negative electrode piece of the secondary battery and controlling its parameters, the problem of insufficient peeling force between the hard carbon material and the negative electrode current collector is solved, and the energy density and cycle performance of the secondary battery are improved.

CN118782883APending Publication Date: 2024-10-15SUNWODA MOBILITY ENERGY TECHNOLOGY CO LTD

Patent Information

Application Number
CN202410995615.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

When existing hard carbon materials are used as negative electrode materials for secondary batteries, the peeling force from the negative electrode current collector is low, resulting in poor cycle performance and stability of the secondary battery. In addition, in order to improve the adhesive force, a binder needs to be added, resulting in energy loss. Density decreases.

Method used

Set up a coating between the negative active material layer and the negative current collector, and reasonably control the roughness of the coating, the mass ratio of nanoparticles to conductive carbon materials, and the amount of binder used to ensure 2≤K≤80 and improve the negative electrode Peeling force and adhesive properties of the sheet.

Benefits of technology

It effectively improves the bonding performance between hard carbon materials and negative electrode current collectors, improves the energy density and cycle performance of secondary batteries, and ensures efficient battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782883A_ABST
    Figure CN118782883A_ABST
Patent Text Reader

Abstract

The invention provides a secondary battery and an electric device, and belongs to the technical field of batteries. According to the secondary battery provided by the invention, the coating is arranged between the negative electrode active material layer and the negative electrode current collector, and the roughness of the coating, the mass ratio of nanoparticles to the conductive carbon material in the coating and the mass percentage of the binder in the negative electrode active material layer are reasonably controlled; according to the present invention, the bonding performance of the hard carbon material in the negative electrode active material layer and the negative electrode current collector can be effectively improved, and the stripping force of the negative electrode current collector and the negative electrode active material layer in the negative electrode plate can be improved, such that the obtained secondary battery has characteristics of high energy density and excellent cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, in particular to a secondary battery and an electrical device. Background Art

[0002] Sodium-ion batteries have low cost, long life, high rate and excellent low-temperature performance, and have very good development prospects. At present, the main material of the negative electrode of commercial sodium-ion batteries is carbon-based material. Among them, hard carbon has a higher theoretical specific capacity and a lower voltage platform, and is a suitable negative electrode material. However, hard carbon materials are loose and porous, with a large specific surface area. During the coating process, the adhesion with the foil is low, resulting in low negative electrode peeling force, which poses a great challenge to negative electrode processing. In addition, due to the low peeling force between the hard carbon material and the negative electrode current collector, the cycle performance and stability of the secondary battery obtained are poor. Summary of the invention

[0003] The purpose of the present application is to solve the problem that when existing hard carbon materials are used as negative electrode materials of secondary batteries, the cycle performance of the secondary batteries is poor due to the low peeling force between the hard carbon materials and the negative electrode current collector, or the energy density of the secondary batteries is low due to increasing the amount of binder used in order to meet the peeling force between the hard carbon materials and the negative electrode current collector, and to provide a secondary battery and an electrical device with excellent cycle performance and high energy density.

[0004] To achieve the above-mentioned object, the first aspect of the present application provides a secondary battery, comprising a positive electrode sheet and a negative electrode sheet, wherein the negative electrode sheet comprises a negative electrode current collector, a negative electrode active material layer and a coating layer disposed between the negative electrode current collector and the negative electrode active material layer; the negative electrode active material layer comprises a negative electrode active material, and the negative electrode active material comprises hard carbon;

[0005] The coating layer includes nanoparticles and conductive carbon material, and the negative electrode active material layer includes a binder;

[0006] The negative electrode plate satisfies: 2≤K≤80;

[0007] Where, K = βm / c,

[0008] βμm is the roughness of the coating;

[0009] m is the mass ratio of nanoparticles to conductive carbon material;

[0010] c% is the mass percentage of the binder in the negative electrode active material layer.

[0011] As an embodiment of the present application, the roughness βμm of the coating is 1 to 15 μm.

[0012] As an embodiment of the present application, the mass ratio m of the nanoparticles to the conductive carbon material is 5-8.

[0013] As an embodiment of the present application, the binder accounts for 1 to 5% by mass of the negative electrode active material layer.

[0014] As an embodiment of the present application, the average particle size of the nanoparticles is 1 to 15 nm.

[0015] As an embodiment of the present application, the sphericity of the nanoparticles is 0.7 to 0.9.

[0016] As an embodiment of the present application, the average particle size of the conductive carbon material is 30 to 60 nm.

[0017] As an embodiment of the present application, the specific surface area of ​​the conductive carbon material is 100 to 150 m 2 / g.

[0018] As an embodiment of the present application, the thickness of the coating layer is 5 to 20 μm.

[0019] As an implementation scheme of the present application, the thickness of the negative electrode plate is 100 to 200 mm.

[0020] As an embodiment of the present application, the nanoparticles include at least one of metal materials, semiconductor materials, ferromagnetic materials, and ceramic materials.

[0021] As an embodiment of the present application, the metal material includes at least one of transition metals with atomic numbers of 21 to 32, 39 to 51, 57 to 80, magnesium, calcium, strontium, barium, and aluminum.

[0022] As an embodiment of the present application, the semiconductor material includes at least one of silicon, gallium nitride, silicon carbide, zinc oxide, aluminum oxide, cadmium sulfide, cadmium selenide, gallium arsenide, indium phosphide, and gallium borophosphide.

[0023] As an embodiment of the present application, the ferromagnetic material includes at least one of iron-nickel alloy, iron-cobalt alloy, ferrite, neodymium-iron-boron, samarium-cobalt, iron-chromium, and iron-silicon.

[0024] As an embodiment of the present application, the ceramic material includes at least one of aluminum oxide, silicon nitride, zirconium oxide, strontium titanate, magnesium oxide, iron oxide, zinc oxide, titanium oxide, indium tin oxide, lanthanum oxide, and yttrium oxide.

[0025] As an embodiment of the present application, the conductive carbon material includes at least one of graphite, graphene, soft carbon, hard carbon, carbon nanotubes, carbon fibers, activated carbon, carbon black, and carbon nanofibers.

[0026] As an embodiment of the present application, the binder includes at least one of styrene rubber latex and sodium carboxymethyl cellulose.

[0027] In a second aspect of the present application, an electrical device is provided, comprising the secondary battery described above.

[0028] Compared with the prior art, the beneficial effects of this application are:

[0029] In the secondary battery provided by the present application, by arranging a coating between the negative electrode active material layer and the negative electrode current collector, and by reasonably controlling the roughness of the coating, the mass ratio of nanoparticles to conductive carbon material in the coating, and the mass percentage of the binder in the negative electrode active material layer, the negative electrode pole piece satisfies a specific relationship: 2≤βm / c≤80, which can effectively improve the bonding performance between the hard carbon material in the negative electrode active material layer and the negative electrode current collector, and improve the peeling force between the negative electrode current collector and the negative electrode active material layer in the negative electrode pole piece, so that the obtained secondary battery can have not only a higher energy density, but also excellent cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a schematic diagram of the layered structure of the negative electrode sheet in Example 1 of the present application:

[0031] 1-negative electrode current collector, 2-coating layer, 3-negative electrode active material layer. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0033] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0034] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0035] The reagents or instruments used in this application without indicating the manufacturer are all conventional products that can be obtained through commercial purchase.

[0036] In one embodiment of the present application, the present application proposes a secondary battery, comprising a positive electrode sheet and a negative electrode sheet, wherein the negative electrode sheet comprises a negative electrode current collector, a negative electrode active material layer and a coating disposed between the negative electrode current collector and the negative electrode active material layer; the negative electrode active material layer comprises a negative electrode active material, and the negative electrode active material comprises hard carbon;

[0037] The coating layer includes nanoparticles and conductive carbon material, and the negative electrode active material layer includes a binder;

[0038] The negative electrode plate satisfies: 2≤K≤80;

[0039] Where, K = βm / c,

[0040] βμm is the roughness of the coating;

[0041] m is the mass ratio of nanoparticles to conductive carbon material;

[0042] c% is the mass percentage of the binder in the negative electrode active material layer.

[0043] The research of the present application found that the bonding force between the negative electrode active material layer and the negative electrode collector in the negative electrode pole piece will not only affect the cycle performance and service life of the secondary battery, but also affect the energy density of the secondary battery; the secondary battery provided by the present application sets a coating between the negative electrode active material layer and the negative electrode collector, and reasonably controls the roughness of the coating, the mass ratio of nanoparticles to conductive carbon material in the coating, and the mass percentage of the binder in the negative electrode active material layer, so that the negative electrode pole piece satisfies: 2≤βm / c≤80, which can effectively improve the bonding performance between the hard carbon material in the negative electrode active material layer and the negative electrode collector, and improve the peeling force between the negative electrode collector and the negative electrode active material layer in the negative electrode pole piece; thereby, the obtained secondary battery has a higher energy density and excellent cycle performance.

[0044] Exemplarily, the negative electrode plate satisfies 2≤K≤80, wherein K may be any point value or any two point range values ​​within the range of 2≤K≤80, for example, it may be 2, 5, 8, 10, 12, 15, 18, 20, 22, 25, 28, 30, 32, 35, 38, 40, 42, 45, 48, 50, 52, 55, 58, 60, 62, 65, 68, 70, 72, 75, 78, 80, or any two range values; when the K value of the negative electrode plate is within the above range, the peeling force between the negative electrode active material layer and the negative electrode current collector in the obtained negative electrode plate is high, and the obtained secondary battery has excellent cycle performance and high energy density.

[0045] In one embodiment, the negative electrode sheet satisfies 16≤K≤32. For example, K may be a range value of one or any two of 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32. The present application has found that when the negative electrode material is further selected to satisfy 16≤K≤32, the peeling force between the negative active material layer and the negative current collector in the obtained negative electrode sheet is higher, and the comprehensive performance of the obtained secondary battery is better.

[0046] In one embodiment, the roughness β μm of the coating is 1-15 μm.

[0047] It should be noted that the roughness of the coating is tested by a stylus-type surface roughness measuring instrument. Specifically, a diamond stylus with a tip curvature radius of about 2 microns is slowly slid along the surface to be tested. The up and down displacement of the diamond stylus is converted into an electrical signal by an electrical length sensor, and the surface roughness value is indicated by the display instrument after amplification, filtering and calculation.

[0048] The present application study found that the roughness of the coating affects the bonding force between the negative electrode active material layer and the negative electrode current collector. When the roughness of the coating is further selected to be 1 to 15 μm, the peeling force between the negative electrode active material layer and the negative electrode current collector can be effectively enhanced, thereby avoiding the problem of the negative electrode active material layer falling off on the negative electrode current collector due to volume expansion during the charge and discharge process of the secondary battery, resulting in increased internal resistance of the secondary battery, increased polarization and rapid capacity decay, thereby making the obtained secondary battery have excellent cycle performance.

[0049] Exemplarily, the β may be any point value or any two point range values ​​between 1 and 15, for example, it may be one or any two range values ​​of 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15.

[0050] In one embodiment, the roughness βμm of the coating is 5 to 12μm. For example, it can be a range of one or any two of 5, 5.5, 6.5, 7.5, 8.5, 9.5, 10.5, 11.5, 12. The present application has found that when the roughness βμm of the coating is further selected to be 5 to 12μm, the peeling force between the negative electrode active material layer and the negative electrode current collector in the obtained negative electrode sheet is higher, and the cycle performance of the secondary battery is better.

[0051] In one embodiment, the mass ratio m of the nanoparticles to the conductive carbon material is 5-8.

[0052] The present application study found that the mass ratio of nanoparticles and conductive carbon materials in the coating will affect the conductive properties of the coating to a certain extent, and will also affect the peeling force between the negative electrode active material layer and the negative electrode current collector; when the mass ratio m of the nanoparticles and the conductive carbon material is further selected to be 5 to 8, the obtained coating can achieve a good balance between conductive properties and enhanced peeling force between the negative electrode active material layer and the conductive carbon material, thereby improving the cycle performance of the secondary battery.

[0053] Exemplarily, the mass ratio m of the nanoparticles to the conductive carbon material can be any point value or any two point range values ​​between 5 and 8, for example, it can be one of 5.0, 5.2, 5.4, 5.6, 5.8, 6.0, 6.2, 6.4, 6.6, 6.8, 7.0, 7.2, 7.4, 7.6, 7.8, 8.0 or any two range values.

[0054] In one embodiment, the mass ratio m of the nanoparticles to the conductive carbon material is 6.5 to 7. For example, it can be 6.50, 6.52, 6.54, 6.56, 6.58, 6.60, 6.62, 6.64, 6.66, 6.68, 6.70, 6.72, 6.74, 6.76, 6.78, 6.80, 6.82, 6.84, 6.86, 6.88, 6.90, 6.92, 6.94, 6.96, 6.98, 7.00, or any two of the range values. The present application has found that when the mass ratio m of the nanoparticles to the conductive carbon material is further selected to be 6.5 to 7, the cycle performance of the secondary battery obtained is better.

[0055] In one embodiment, the mass percentage c% of the binder in the negative electrode active material layer is 1-5%.

[0056] The amount of binder in the negative electrode active material layer will affect the bonding performance between the negative electrode active material layer and the negative electrode current collector, but it will also affect the energy density of the secondary battery. The present application study found that when the mass percentage c% of the binder in the negative electrode active material layer is further selected to be 1-5%, the amount of binder added can be reduced as much as possible on the basis of ensuring the excellent bonding performance between the negative electrode active material layer and the negative electrode current collector, thereby increasing the amount of conductive material added, thereby improving the energy density of the secondary battery.

[0057] Exemplarily, the mass percentage c% of the binder in the negative electrode active material layer can be any point value or any two point range values ​​between 1 and 5%, for example, it can be one of 1, 1.2, 1.4, 1.6, 1.8, 2.0, 2.2, 2.4, 2.6, 2.8, 3.0, 3.2, 3.4, 3.6, 3.8, 4.0, 4.2, 4.4, 4.6, 4.8, 5.0 or any two of the range values.

[0058] In one embodiment, the mass percentage c% of the binder in the negative electrode active material layer is 2.5-4%. For example, it can be 2.50, 2.55, 2.65, 2.75, 2.85, 2.95, 3.05, 3.15, 3.25, 3.35, 3.45, 3.55, 3.65, 3.75, 3.85, 3.95, 4.00 or any two of them. The present application has found that when the mass percentage c% of the binder in the negative electrode active material layer is further selected to be 2.5-4%, the comprehensive performance of the secondary battery obtained is better.

[0059] In one embodiment, the average particle size of the nanoparticles is 1-15 nm.

[0060] It should be noted that the average particle size of the nanoparticles is obtained by testing with a laser particle size analyzer. Specifically, a narrow light beam from a He-Ne laser is expanded by a beam expansion system and then irradiated in parallel on a group of particles to be measured in a particle slot. The diffraction light generated by the particle group is converged by a focusing lens to form a diffraction pattern on its focal plane. A special annular photodetector located on the focal plane is used to perform photoelectric conversion of the signal. Then, the signal from the photodetector is amplified, A / D converted, and data is collected and sent to a computer. A pre-compiled optimization program is used to compare the calculated value with the measured value, so that the size distribution of the particle group can be quickly inferred.

[0061] The present application study found that the average particle size of the nanoparticles not only affects the roughness of the coating, but also affects the conductivity of the coating. Within a certain range, as the average particle size of the nanoparticles increases, when they are added to the coating, the roughness of the coating surface can be effectively increased, but the conductivity of the coating will decrease; when the average size of the nanoparticles is further selected to be 1 to 15 nm, the roughness range of the obtained coating is appropriate, thereby effectively improving the peeling force between the negative electrode active layer and the negative electrode current collector, and the conductivity of the coating is excellent; thereby, the overall performance of the prepared secondary battery is excellent.

[0062] Exemplarily, the average particle size of the nanoparticles may be any point value or any two point range values ​​between 1 and 15 nm, for example, it may be one or any two range values ​​of 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, and 15 nm.

[0063] In one embodiment, the sphericity of the nanoparticles is 0.7-0.9.

[0064] It should be noted that the sphericity of the nanoparticles is obtained by scanning electron microscopy testing, specifically by fixing the sample on a sample holder with conductive tape and then loading it into the sample chamber of the SEM. Adjust SEM parameters, such as accelerating voltage, working distance, etc., to obtain a clear image. Analyze the SEM image using image analysis software (such as ImageJ) to measure the size and shape parameters of the particles. Calculate the sphericity, which can be calculated by using the ratio of the volume and surface area of ​​the particles to an equal volume sphere.

[0065] The research in this application found that when the sphericity of the nanoparticles is further selected to be 0.7 to 0.9, on the one hand, the nanoparticles themselves have good geometric symmetry, which can help to achieve uniform charge distribution in the negative electrode sheet, thereby improving the electron transfer efficiency; on the other hand, the nanoparticles can be closely arranged, thereby effectively reducing the gaps between the coatings, thereby increasing the contact area between the negative electrode active material layer and the negative electrode current collector, and improving the conductivity of the negative electrode sheet; on the other hand, the friction and wear between the nanoparticles are also less, which can improve the processing mechanical stability and also help maintain the structural stability during the secondary battery cycle.

[0066] Exemplarily, the sphericity of the nanoparticles may be any point value or any two point range values ​​between 0.7 and 0.9, for example, it may be one of 0.70, 0.72, 0.74, 0.76, 0.78, 0.80, 0.82, 0.84, 0.86, 0.88, 0.90 or any two range values.

[0067] In one embodiment, the average particle size of the conductive carbon material is 30-60 nm.

[0068] It should be noted that the average particle size of the conductive carbon material is obtained by testing with a laser particle size analyzer, specifically, the dispersed sample is introduced into the measuring cell of the laser particle size analyzer, the measurement program is started, and the laser particle size analyzer irradiates the sample with a laser and analyzes the laser scattered by the sample. The instrument collects the scattered signal and converts it into an electrical signal, and performs data processing through the built-in software. The analysis software will provide a particle size distribution diagram and related statistical data, such as D10, D50, D90, etc., as well as the average particle size.

[0069] Specifically, the extraction steps of the conductive carbon sample are as follows: the conductive carbon and nanoparticles are separated by flotation method, and the mixture scraped from the negative electrode coating is ultrasonically dispersed for 30 minutes to fully disperse the conductive carbon and nanoparticles. The dispersed mixture is added to a stirring device with water, and the mass ratio of the mixture to water is 1:1.5. The mixture is fully stirred for 120 minutes to fully mix the mixture with water to form a slurry with uniform concentration, and then xanthate and cresol acid are added according to the mass ratio of mixture: xanthate: cresol acid = 1:0.2:0.01. The stirring is continued for 120 minutes to form a large number of bubbles in the slurry. The conductive carbon particles in the mixture are combined with the bubbles and float on the surface of the slurry to form a foam layer. The foam layer is collected with a scraper or other tools, and the collected foam is cleaned and dried to obtain a conductive carbon sample.

[0070] The research in this application found that the average particle size of the conductive carbon material will affect the roughness of the coating, and will also affect the conductivity of the coating. When the average particle size of the conductive carbon material is further selected to be 30 to 60 nm, the resulting negative electrode active material layer and negative electrode current collector have higher peeling force, and the overall performance of the secondary battery is better.

[0071] Exemplarily, the average particle size of the conductive carbon material may be any point value or any two point range values ​​between 30 and 60 nm, for example, it may be one or any two range values ​​of 30 nm, 32 nm, 35 nm, 38 nm, 40 nm, 42 nm, 45 nm, 48 nm, 50 nm, 52 nm, 55 nm, 58 nm, and 60 nm.

[0072] In one embodiment, the specific surface area of ​​the conductive carbon material is 100-150 m 2 / g.

[0073] It should be noted that the specific surface area of ​​the conductive carbon material is obtained by testing with a fully automatic physical adsorption instrument, specifically by drying and degassing the sample to be tested at high temperature to remove moisture and adsorbed gas in the pores of the sample. The pretreated sample is then placed in the sample cell of the instrument. The sample is vacuum degassed to remove the adsorbed gas on the surface and pores of the sample. At liquid nitrogen temperature, pure nitrogen is introduced into the sample tube for adsorption. After the adsorption is completed, the pressure of the nitrogen is gradually reduced and the desorption amount is recorded. The instrument automatically records the nitrogen adsorption and desorption amounts. Use BET (Brunol-Emmett-Teller) theory or other appropriate models to analyze the adsorption isotherm and calculate the specific surface area.

[0074] The present application found that the specific surface area of ​​the conductive carbon material affects the conductivity of the coating, and the size of the specific surface area also affects the peeling force of the negative electrode active material layer and the negative electrode current collector; when the specific surface area of ​​the conductive carbon material is further selected to be 100-150 m 2 / g, the comprehensive performance of the obtained secondary battery is better.

[0075] For example, the specific surface area of ​​the conductive carbon material may be 100 to 150 m 2 Any point value or any range value between two points, for example, 100m 2 / g、105m 2 / g, 110m 2 / g, 115m 2 / g, 120m 2 / g, 125m 2 / g, 130m 2 / g, 135m 2 / g, 140m 2 / g, 145m 2 / g, 150m 2 / g or both.

[0076] In one embodiment, the coating has a thickness of 5-20 μm.

[0077] The present application has found that when the coating thickness is selected to be 5 to 20 μm, a better peeling force range of the negative electrode active material layer and the negative electrode current collector can be achieved, thereby making the resulting secondary battery have better cycle performance and higher energy density.

[0078] Exemplarily, the thickness of the coating may be any point value or any two point range values ​​between 5 and 20 μm, such as 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm or any two range values.

[0079] In one embodiment, the thickness of the negative electrode plate is 100-200 mm.

[0080] Exemplarily, the thickness of the negative electrode plate may be any point value or any two point range values ​​between 100 and 200 mm, for example, it may be one or any two range values ​​of 100 mm, 110 mm, 120 mm, 130 mm, 140 mm, 150 mm, 160 mm, 170 mm, 180 mm, 190 mm, and 200 mm.

[0081] In one embodiment, the nanoparticles include at least one of metal materials, semiconductor materials, ferromagnetic materials, and ceramic materials.

[0082] In one embodiment, the metal material includes at least one of transition metals with atomic numbers of 21-32, 39-51, 57-80, magnesium, calcium, strontium, barium, and aluminum.

[0083] In one embodiment, the semiconductor material includes at least one of silicon, gallium nitride, silicon carbide, zinc oxide, aluminum oxide, cadmium sulfide, cadmium selenide, gallium arsenide, indium phosphide, and gallium borophosphide.

[0084] In one embodiment, the ferromagnetic material includes at least one of iron-nickel alloy, iron-cobalt alloy, ferrite, neodymium-iron-boron, samarium-cobalt, iron-chromium, and iron-silicon.

[0085] In one embodiment, the ceramic material includes at least one of aluminum oxide, silicon nitride, zirconium oxide, strontium titanate, magnesium oxide, iron oxide, zinc oxide, titanium oxide, indium tin oxide, lanthanum oxide, and yttrium oxide.

[0086] In one embodiment, the conductive carbon material includes at least one of graphite, graphene, soft carbon, hard carbon, carbon nanotubes, carbon fibers, activated carbon, carbon black, and carbon nanofibers.

[0087] In one embodiment, the binder includes at least one of styrene rubber latex and sodium carboxymethyl cellulose.

[0088] In one embodiment, the coating is prepared by vapor deposition technology.

[0089] Exemplarily, the vapor deposition technology includes at least one of magnetron sputtering, atomic layer deposition, electron beam evaporation, laser evaporation, and chemical vapor deposition.

[0090] The present invention has found that when vapor deposition technology is selected for the preparation of the coating, on the one hand, the coating can be directly deposited on the negative electrode current collector without the introduction of additional binder, thereby ensuring the conductivity of the negative electrode current collector; on the other hand, the coating can be distributed more evenly, thereby improving the peeling force between the negative electrode active material layer and the negative electrode current collector.

[0091] In one embodiment, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector; the positive electrode active material layer includes a positive electrode active material. The present application has no limitation on the positive electrode active material, and any known positive electrode active material can be used.

[0092] Exemplarily, the positive electrode active material includes at least one of Prussian blue, polyanions, and layered oxides.

[0093] In one embodiment, the electrolyte includes an organic solvent, a sodium salt and an additive. The present application has no limitation on the organic solvent, sodium salt and additive in the electrolyte, and any known organic solvent, sodium salt and additive can be used.

[0094] Illustratively, the organic solvent includes at least one of ethylene carbonate, propylene carbonate, and diethyl carbonate; the lithium salt includes at least one of sodium hexafluorophosphate, sodium tetrafluoroborate, and sodium hexafluoroarsenic phosphate; and the additive includes at least one of a film-forming additive, a conductive additive, and a flame retardant additive.

[0095] In one embodiment, the separator of the secondary battery is disposed between the positive electrode and the negative electrode.

[0096] In one embodiment, the secondary battery is a sodium battery.

[0097] In one embodiment of the present application, the present application proposes an electrical device, and the electrical device includes the secondary battery described in the present application.

[0098] Exemplarily, the above-mentioned electrical devices may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0099] Example 1

[0100] The present invention provides a secondary battery, wherein a method for preparing the secondary battery comprises the following steps:

[0101] (1) Preparation of negative electrode sheet

[0102] 1) Nanoparticles (alumina, average particle size 8nm, sphericity 0.8) and conductive carbon materials (carbon black, average particle size 45μm, specific surface area 125m 2 / g) are mixed evenly in a mass ratio of 5:1 and then put into a vapor deposition device, a copper foil current collector is placed directly opposite to the target material, and the equipment parameters are adjusted to deposit the nanoparticles and the conductive carbon material on the copper foil to form a coating with a thickness of 13 μm and a roughness of 10 μm;

[0103] 2) The negative electrode active material (hard carbon), the binder (sodium carboxymethyl cellulose), and the conductive agent (acetylene black) are mixed in a mass ratio of 95:2.5:2.5, and then 40% of the total mass of the mixed material is added with deionized water to obtain a negative electrode slurry under the action of a vacuum mixer; the negative electrode slurry is evenly coated on the coating; the coated electrode sheet is transferred to an oven for drying, and then cold pressed and cut to obtain a negative electrode sheet with a thickness of 150 μm;

[0104] (2) Preparation of positive electrode sheet

[0105] The positive electrode active material sodium ternary NaNi 0.33 Fe 0.33 Mn 0.33O2, a binder (polyvinylidene fluoride), and a conductive agent (acetylene black) are mixed in a mass ratio of 95:2.5:2.5, and 40% of the total mass of the mixed substance is added with N-methylpyrrolidone, and a positive electrode slurry is obtained under the action of a vacuum mixer; the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil; the coated electrode sheet is transferred to an oven for drying, and then cold pressed and cut to obtain a positive electrode sheet;

[0106] (3) Preparation of secondary batteries

[0107] The positive electrode sheet, the isolation film (12 μm thick polypropylene isolation film), and the negative electrode sheet are placed in the winding device in order and wound into a square bare battery cell, so that the isolation film is between the positive and negative electrode sheets to play an isolating role. Then, they are loaded into an aluminum shell and baked at 80°C to remove water. Then, the corresponding non-aqueous electrolyte is injected (the electrolyte is a NaPF6 solution with a concentration of 1 mol / L, and the solvents ethylene carbonate, ethyl methyl carbonate and diethyl carbonate are mixed in a volume ratio of 1:1:1) and sealed. After standing, hot and cold pressing, formation (the formation voltage is set to 3.1V), capacity division (the battery cell is charged to 4V at a rate of 1C) and other processes, a secondary battery is obtained.

[0108] Embodiments 2 to 7

[0109] The embodiment of the present application provides a secondary battery. The difference between the secondary battery and the embodiment 1 is that the roughness of the coating is changed by adjusting the physical deposition time and the deposition rate, or by adjusting the parameters of the nanoparticles and the conductive carbon material at the same time.

[0110] Embodiments 8 to 12

[0111] The embodiment of the present application provides a secondary battery. The difference between the secondary battery and the embodiment 1 is that the amount of nanoparticles and conductive carbon materials added is adjusted to achieve a change in the mass ratio of the nanoparticles and the conductive carbon materials.

[0112] Embodiments 13 to 17

[0113] The embodiment of the present application provides a secondary battery. The difference between the secondary battery and the embodiment 1 is that the amount of binder added is adjusted to achieve a change in the mass percentage of the binder in the negative electrode active material layer.

[0114] Embodiment 18

[0115] The embodiment of the present application provides a secondary battery, which is different from the embodiment 1 in that the selection of nanoparticles is changed.

[0116] Embodiment 19

[0117] The embodiment of the present application provides a secondary battery, which is different from the embodiment 1 in that the selection of the conductive carbon material is changed.

[0118] Embodiment 20

[0119] The embodiment of the present application provides a secondary battery, which is different from the embodiment 1 in that the thickness of the coating layer is changed by controlling the parameters of the vapor deposition.

[0120] Comparative Example 1

[0121] The comparative example of the present application provides a secondary battery, which is different from the embodiment 1 in that the coating layer is not introduced.

[0122] Comparative Example 2

[0123] The comparative example of the present application provides a secondary battery, which is different from the embodiment 1 in that no nanoparticles are added to the coating.

[0124] Comparative Example 3

[0125] The comparative example of the present application provides a secondary battery, which is different from the embodiment 1 in that no conductive carbon material is added to the coating.

[0126] Comparative Examples 4-5

[0127] The comparative example of the present application provides a secondary battery, which is different from Example 1 in that the K value is changed by adjusting the roughness of the coating, the mass ratio of nanoparticles to conductive carbon material in the coating, and the mass percentage of the binder in the negative electrode active material layer.

[0128] The roughness β of the coating, the mass ratio m of the nanoparticles to the conductive carbon material in the coating, the mass percentage c of the binder in the negative electrode active material layer, the average particle size and sphericity of the nanoparticles, the average particle size and specific surface area of ​​the conductive carbon material, the thickness of the coating, and the thickness of the negative electrode sheet in the embodiments and comparative examples are shown in Table 1;

[0129] Table 1

[0130]

[0131]

[0132] The test methods for the peeling force of the negative electrode active material layer and the negative electrode current collector in the negative electrode sheets prepared in Examples 1 to 20 and Comparative Examples 1 to 5, and the energy density and cycle performance of the secondary battery include the following:

[0133] 1) Peeling force: The peeling test tape is pasted on the negative electrode sheet. The test tape usually has a certain degree of adhesion and can be firmly adhered to the surface of the negative electrode active material layer of the negative electrode sheet; the peeling force is applied by the peeling force test equipment to peel the test negative electrode active material layer from the current collector. The sensor can measure and record the force required for peeling;

[0134] 2) Energy density: Weigh the mass of the secondary battery (Kg), then place it in a 25℃ environment for 1h, charge it to 4V at a constant current and constant voltage of 0.33C, and the cut-off current is 0.05C; discharge it at a constant current of 0.33C, and the cut-off voltage is 1.5V. This is a complete charge and discharge cycle test. Repeat the charge and discharge cycle 3 times, and obtain the discharge energy (Wh) from the third discharge test. Energy density = discharge energy / battery mass;

[0135] 3) Cycle performance: The secondary battery is placed in a 25°C environment for 1 hour, and charged to 4V at a constant current and constant voltage of 1.0C, with a cut-off current of 0.05C; it is discharged at a constant current of 1C, with a cut-off voltage of 1.5V. This is a complete charge and discharge cycle test. Repeat the charge and discharge cycle 3 times, with the third cycle discharge capacity as the initial capacity. The number of cycles reaches 2000 at room temperature, and the capacity retention rate of the secondary battery is recorded;

[0136] The test results are shown in Table 2;

[0137] Table 2

[0138] Peel force (N / m) Energy density (Wh / Kg) Capacity retention rate (%) Example 1 20.5 152.3 84.75 Example 2 20.1 152.3 83.01 Example 3 20.5 152.3 84.10 Example 4 10.1 152.4 75.33 Example 5 25.8 152.2 81.54 Example 6 8.3 152.4 70.21 Example 7 25.9 152.0 79.32 Example 8 25.1 152.2 84.80 Example 9 12.1 152.4 80.10 Example 10 30.0 152.1 80.54 Embodiment 11 9.3 152.1 71.2 Example 12 25.6 152.2 78.27 Embodiment 13 28.4 150.1 80.1 Embodiment 14 11.1 154.1 74.71 Embodiment 15 30.2 147.1 81.3 Example 16 8.2 152.0 70.2 Embodiment 17 31.2 144.7 78.42 Embodiment 18 20.3 152.2 85.4 Embodiment 19 20.3 152.4 85.7 Embodiment 20 21.7 148.1 84.67 Comparative Example 1 5.1 152.0 60.43 Comparative Example 2 6.2 152.1 63.54 Comparative Example 3 24.5 147.4 70.23 Comparative Example 4 10 152.4 68.24 Comparative Example 5 14.4 150.4 67.28

[0139] As can be seen from Table 2, in the present application, by controlling the negative electrode sheet to satisfy 2≤βm / c≤80, the peeling force between the negative electrode active material layer and the negative electrode current collector in the obtained negative electrode sheet is relatively high, above 8.2, and the obtained secondary battery has a high energy density and excellent cycle performance. Specifically, the energy density of the obtained secondary battery is above 147.1Wh / kg, and the cycle performance is above 70.20%;

[0140] The results of Examples 1 to 20 and Comparative Example 1 of the present application also show that when the coating is not introduced, the peeling force of the obtained secondary battery is low and the cycle stability is poor; the results of Examples 1 to 20 and Comparative Example 2 show that when no nanoparticles are added to the coating, the peeling force of the obtained secondary battery is low and the cycle stability is poor; the results of Examples 1 to 20 and Comparative Example 3 show that when no conductive carbon material is added, the energy density of the obtained secondary battery is low and the cycle stability is poor; Examples 1 to 20 and Comparative Examples 4 to 5 also show that when the K value is not within the range given in the present application, the cycle stability of the obtained secondary battery is poor.

Claims

1. A secondary battery, comprising a positive electrode sheet and a negative electrode sheet, characterized in that: The negative electrode sheet comprises a negative electrode current collector, a negative electrode active material layer and a coating disposed between the negative electrode current collector and the negative electrode active material layer; the negative electrode active material layer comprises a negative electrode active material, and the negative electrode active material comprises hard carbon; The coating layer includes nanoparticles and conductive carbon material, and the negative electrode active material layer includes a binder; The negative electrode plate satisfies: 2≤K≤80; Where, K = βm / c, βμm is the roughness of the coating; m is the mass ratio of nanoparticles to conductive carbon material; c% is the mass percentage of the binder in the negative electrode active material layer.

2. The secondary battery according to claim 1, characterized in that: Satisfy at least one of the following conditions: a. The roughness βμm of the coating is 1 to 15μm; b. The mass ratio m of the nanoparticles to the conductive carbon material is 5 to 8; c. The mass percentage c% of the binder in the negative electrode active material layer is 1 to 5%.

3. The secondary battery according to claim 1, characterized in that: Satisfy at least one of the following conditions: d. The average particle size of the nanoparticles is 1 to 15 nm; e. The sphericity of the nanoparticles is 0.7 to 0.

9.

4. The secondary battery according to claim 1, characterized in that: The average particle size of the conductive carbon material is 30 to 60 nm; And / or, the specific surface area of ​​the conductive carbon material is 100 to 150 m 2 / g.

5. The secondary battery according to claim 1, characterized in that: Satisfy at least one of the following conditions: f. The thickness of the coating is 5 to 20 μm; g. The thickness of the negative electrode plate is 100 to 200 mm.

6. The secondary battery according to claim 1, characterized in that: The nanoparticles include at least one of metal materials, semiconductor materials, ferromagnetic materials, and ceramic materials.

7. The secondary battery according to claim 6, characterized in that: Satisfy at least one of the following conditions: h. The metal material includes at least one of transition metals with atomic numbers of 21 to 32, 39 to 51, 57 to 80, magnesium, calcium, strontium, barium, and aluminum; i. The semiconductor material includes at least one of silicon, gallium nitride, silicon carbide, zinc oxide, aluminum oxide, cadmium sulfide, cadmium selenide, gallium arsenide, indium phosphide, and gallium borophosphide; j. The ferromagnetic material includes at least one of an iron-nickel alloy, an iron-cobalt alloy, a ferrite, a neodymium-iron-boron, a samarium-cobalt, an iron-chromium, and an iron-silicon; k. The ceramic material includes at least one of aluminum oxide, silicon nitride, zirconium oxide, strontium titanate, magnesium oxide, iron oxide, zinc oxide, titanium oxide, indium tin oxide, lanthanum oxide, and yttrium oxide.

8. The secondary battery according to claim 1, characterized in that: The conductive carbon material includes at least one of graphite, graphene, soft carbon, hard carbon, carbon nanotubes, carbon fibers, activated carbon, carbon black, and carbon nanofibers.

9. The secondary battery according to claim 1, characterized in that: The binder includes at least one of styrene rubber latex and sodium carboxymethyl cellulose.

10. An electrical device, characterized in that: A secondary battery comprising the secondary battery according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • CNT (Carbon Nano Tube) / SnO2 coaxial composite array lithium ion battery negative electrode material

    CN103647047A

  • Negative plate and preparation method thereof, lithium ion cell, lithium ion battery pack and application of lithium ion battery pack

    CN112271271A

  • Solid-state battery and method for improving rate capability and safety of solid-state battery

    CN112490433A

  • Secondary battery and device comprising same

    CN112909220A

  • Electrochemical device and electronic equipment

    CN114930600A

Cited By

  • Negative current collector, negative pole piece and lithium ion battery

    CN119674085A

  • Negative current collector, secondary battery and electronic equipment

    CN119812351A

  • Surface modification method of lithium metal negative electrode copper-based current collector

    CN120072952A