Antirust additive for alkaline manganese battery steel shell and application of antirust additive
By using Mg8Ba4Ca11O23/SiO2 anti-rust additive in alkaline manganese batteries, the anti-oxidation ability of the inner surface of the steel shell is improved, the problem of rust of the steel shell of alkaline manganese batteries is solved, and the discharge performance and storage stability of the battery are improved.
Patent Information
- Application Number
- CN202410760961.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-15
AI Technical Summary
The steel shell of alkaline manganese batteries is prone to rusting after long-term storage, leading to increased precipitation of impurities and increased gas evolution inside the battery, which in turn increases the risk of leakage and affects discharge performance.
Mg8Ba4Ca11O23/SiO2 is used as the anti-rust additive for the steel shell. MgO, BaO, CaO and SiO2 are mixed by heating to form a modified additive, which is used to improve the anti-oxidation ability of the inner surface of the steel shell and is used as part of the cathode material in alkaline manganese batteries. , used in combination with electrolyte and adhesive.
Significantly prolongs the rust time of the inner surface of the steel shell, improves the discharge performance of the battery after long storage, and ensures the stability and performance of the battery.
Smart Images

Figure BDA0004891056820000021 
Figure BDA0004891056820000022 
Figure BDA0004891056820000031
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alkaline manganese batteries, and in particular relates to the preparation of an alkaline manganese battery steel shell anti-rust additive and its application in the battery. Background Art
[0002] Alkaline manganese batteries are mainly composed of manganese dioxide positive electrode, zinc paste negative electrode, potassium hydroxide electrolyte, diaphragm and steel shell. Among them, the battery steel shell is not only a container for the alkaline manganese battery, but also a conductive part of the positive electrode current. Therefore, the quality of the steel shell not only affects the discharge performance of the battery, but also increases the impurity content due to the precipitation of Fe and Cu after long-term storage, and increases the amount of gas evolution inside the battery, thereby increasing the risk of leakage. Summary of the invention
[0003] In order to solve the above technical problems, the present invention discloses an alkaline manganese battery steel shell anti-rust additive, which aims to improve the antioxidant capacity of the inner surface of the steel shell, improve the strong oxidizing property of manganese dioxide by adding a modified additive, protect the stability of the inner surface properties of the steel shell, and improve the discharge performance of the battery after long-term storage.
[0004] In order to achieve the above technical purpose, the present invention adopts the following technical solutions:
[0005] An alkaline manganese battery steel shell rust-proof additive, characterized in that the steel shell rust-proof additive is Mg a Ba b Ca c O d / SiO2, the Mg a Ba b Ca c O d Preparation method of SiO2: First, a certain amount of MgO, BaO, CaO and SiO2 are mixed evenly, heated to 100 degrees and kept warm for 8 hours, then taken out and mixed evenly; then heated to 200 degrees and kept warm for 8 hours, then taken out and mixed evenly to obtain MgO / SiO2. a Ba b Ca c O d / SiO2 wherein a is 1-3, b is 2-6, and c is 5-10.
[0006] Furthermore, the mass ratio of MgO, BaO, CaO and SiO2 is 1-3:2-5:2-5:10-20.
[0007] An application of an alkaline manganese battery steel shell rust-proof additive, characterized in that the steel shell rust-proof additive is used to prepare an alkaline manganese battery positive electrode, and the formula is as follows: 100 parts of electrolytic manganese dioxide, 0.05-0.3 parts of homemade synthetic Mg a Ba b Cac O d Additives, 2-7 parts electrolyte, 0.1-1 parts binder, 0.1-1 parts zinc stearate;
[0008] Furthermore, the adhesive is carbomer sodium polyacrylate.
[0009] Furthermore, the electrolyte is a 25%-40% KOH solution.
[0010] The preparation method of the steel shell antirust additive alkaline manganese battery of the present invention is the same as that of the manganese dioxide alkaline manganese battery.
[0011] Beneficial effects of the present invention:
[0012] The alkaline manganese battery prepared by adding the steel shell anti-rust additive of the present invention has a significantly prolonged rust time on the inner surface of the steel shell when stored at 70 degrees. DETAILED DESCRIPTION
[0013] In order to deepen the understanding of the present invention by those skilled in the art, the present invention will be further described below in conjunction with specific embodiments.
[0014] Steel shell anti-rust additive Mg a Ba b Ca c O d Preparation method of SiO2: First, mix 1 part of MgO, 2 parts of BaO, 2 parts of CaO and 10 parts of SiO2 evenly, heat to 100 degrees and keep warm for 8 hours, take out and mix evenly. Then heat to 200 degrees and keep warm for 8 hours, take out and mix evenly to obtain Mg8Ba4Ca 11 O 23 / SiO2.
[0015] Example 1
[0016] Alkali manganese positive electrode material with steel shell anti-rust additive: 100 parts electrolytic manganese dioxide, 0.03 parts homemade synthetic Mg8Ba4Ca 11 O 23 / SiO2 additive, 6 parts of electrolyte, 0.5 parts of carbomer sodium polyacrylate, 0.2 parts of zinc stearate;
[0017] Alkali manganese negative electrode material with steel shell anti-rust additive: taken from the workshop.
[0018] The preparation method of the alkaline manganese battery with added steel shell antirust additive is consistent with the preparation method of the alkaline manganese battery without added steel shell antirust additive, both of which use the company's existing production line, and the prepared alkaline manganese battery is battery 1-1.
[0019] Control group 1:
[0020] Except that no rust inhibitor was added to the steel shell, the other formulas and preparation methods of Battery 1 were the same. The alkaline manganese battery prepared in the control group was Battery 1-0.
[0021] Compare the difference between battery 1-0 and battery 1-1 in 1.5w / 0.65w, 1000mA, 3.9Ω continuous discharge. 11 O 23 / SiO2 content was taken as the experimental variable, and 3 groups of experiments were controlled, and their new electricity is shown in Tables 1-2 below.
[0022] Table 1. Comparison of discharge performance of the first group of batteries
[0023]
[0024] Table 2 Comparison of rust at 70°C
[0025]
[0026]
[0027] Example 2
[0028] Alkali manganese positive electrode material with steel shell anti-rust additive: 100 parts electrolytic manganese dioxide, 0.15 parts homemade synthetic Mg8Ba4Ca 11 O 23 / SiO2 additive, 6 parts of electrolyte, 0.5 parts of carbomer sodium polyacrylate, 0.2 parts of zinc stearate;
[0029] Alkali manganese negative electrode material with steel shell anti-rust additive: taken from the workshop.
[0030] The preparation method of the alkaline manganese battery with added steel shell antirust additive is consistent with the preparation method of the alkaline manganese battery without added steel shell antirust additive, both of which use the company's existing production line, and the prepared alkaline manganese battery is battery 2-1.
[0031] Control group:
[0032] Except that no rust inhibitor was added to the steel shell, the other formulas and preparation methods of Battery 1 were the same. The alkaline manganese battery prepared in the control group was Battery 2-0.
[0033] The performance of the two is shown in Tables 3 and 4.
[0034] Table 3. Comparison of discharge performance of the second group of batteries
[0035]
[0036] Table 4 Comparison of rust at 70°C storage
[0037] 70 degree storage time Battery 2-0 Battery 2-1 7 days 4 sections of rust (24 sections in total) 0 rust (total 24) 12 days 24 sections of rust (24 sections in total) 0 rust (total 24) 25 days / 3 sections of rust (24 sections in total) 50 days / 24 sections of rust (24 sections in total)
[0038] Example 3
[0039] Alkali manganese positive electrode material with steel shell anti-rust additive: 100 parts electrolytic manganese dioxide, 0.4 parts self-made synthetic Mg8Ba4Ca 11 O 23 / SiO2 additive, 6 parts of electrolyte, 0.5 parts of carbomer sodium polyacrylate, 0.2 parts of zinc stearate;
[0040] Alkali manganese negative electrode material with steel shell anti-rust additive: taken from the workshop.
[0041] The preparation method of the alkaline manganese battery with added steel shell antirust additive is consistent with the preparation method of the alkaline manganese battery without added steel shell antirust additive, both of which use the company's existing production line, and the prepared alkaline manganese battery is battery 3-1.
[0042] Control group:
[0043] Except that no rust inhibitor was added to the steel shell, the other formulas and preparation methods of Battery 1 were the same. The alkaline manganese battery prepared in the control group was Battery 3-0.
[0044] The performance of the two is shown in Tables 5 and 6.
[0045] Table 5. Comparison of discharge performance of the third group of batteries
[0046]
[0047] Table 6 Comparison of rust at 70°C
[0048] 70 degree storage time Battery 3-0 Battery 3-1 7 days 4 sections of rust (24 sections in total) 0 rust (total 24) 12 days 24 sections of rust (24 sections in total) 0 rust (total 24) 25 days / 1 section of rust (24 sections in total) 50 days / 24 sections of rust (24 sections in total)
[0049] From the data in the table above, it can be found that when Mg8Ba4Ca 11 O 23 / The content of SiO2 is between 0.03% and 0.4%. The comprehensive discharge performance and steel shell rust performance are best when the content is 0.15%. After high-temperature storage, all discharge performances are improved. When the content is lower than 0.03%, there is no obvious effect on the discharge performance; when the content is greater than 0.4%, it has an inhibitory effect on the discharge performance.
[0050] The above test results show that for Mg8Ba4Ca 11 O 23 / SiO2 additives, as the amount added increases, the protection of the steel shell after high-temperature storage increases, and the battery's large current discharge performance is significantly improved. However, as the amount added increases excessively, the positive electrode manganese dioxide content will decrease, and the discharge performance will decrease instead. Therefore, when the content is 0.05%-0.3%, it can be the additive ratio for the positive electrode of alkaline manganese batteries, which can improve the battery's discharge performance.
Claims
1. An anti-rust additive for steel shell of alkaline manganese battery, characterized in that: The steel shell antirust additive is Mg a Ca b O c H d / SiO2, the Mg a Ba b Ca c O d Preparation method of SiO2: First, a certain amount of MgO, BaO, CaO and SiO2 are mixed evenly, heated to 100 degrees and kept warm for 8 hours, then taken out and mixed evenly; then heated to 200 degrees and kept warm for 8 hours, then taken out and mixed evenly to obtain MgO / SiO2. a Ba b Ca c O d / SiO2 wherein a is 1-3, b is 2-5, c is 2-5, and d is 10-20.
2. The anti-rust additive for steel shell of alkaline manganese battery according to claim 1, characterized in that: The mass ratio of MgO, BaO, CaO and SiO2 is 1-3:2-5:2-5:10-20.
3. An application of the anti-rust additive for steel shell of alkaline manganese battery as claimed in claims 1 to 2, characterized in that: The steel shell antirust additive is used to prepare the positive electrode of the alkaline manganese battery, and its formula is: 100 parts of electrolytic manganese dioxide, 0.05-0.3 parts of homemade synthetic Mg a Ba b Ca c O d Additives: 2-7 parts electrolyte, 0.1-1 parts binder, 0.1-1 parts zinc stearate.
4. The anti-rust additive for steel shell of alkaline manganese battery as claimed in claim 3, characterized in that: The adhesive is carbomer sodium polyacrylate.
5. The anti-rust additive for steel case of alkaline manganese battery according to claim 4, characterized in that: The electrolyte is a 25%-40% KOH solution.