Preparation method and application of microneedle patch
By preparing microneedle patches and using materials such as photoinitiators, methacrylated hyaluronic acid, and platelet-rich fibrin, the problem of traditional dressings being difficult to penetrate necrotic tissue is solved, and more stable and controllable drug release is achieved , promotes the healing of pressure injury wounds and provides new treatment methods.
Patent Information
- Application Number
- CN202411168161.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-10-18
AI Technical Summary
When treating pressure injuries with existing technology, traditional dressings have difficulty penetrating necrotic tissue or hyperkeratotic skin layers, limiting drug delivery and cell migration, resulting in longer healing times and poor therapeutic effects on irregularly shaped wounds.
Using the preparation method of microneedle patch, a photoinitiator, methacrylated hyaluronic acid, platelet-rich fibrin and polyethylene glycol diacrylate are mixed, and the microneedle patch is prepared through mold curing, with controllable The growth factor release rate and good biocompatibility make it suitable for deep wound treatment.
It achieves more stable and controllable drug release, extends the use time of microneedles, improves treatment effect and patient compliance, promotes the healing of pressure injury wounds, and has broad clinical application prospects.
Smart Images

Figure CN118787591A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of biomedical technology, and in particular to a preparation method and application of a microneedle patch. Background Art
[0002] Pressure injury (PI) is a common skin injury, mainly caused by localized damage to the skin and / or soft tissue under bony prominences and instruments due to intense and / or prolonged pressure or pressure combined with shear force. Although a lot of resources have been invested in the prevention and treatment of pressure injuries, its incidence remains high, especially with the increase in predisposing factors such as an aging population, obesity, diabetes, and cardiovascular disease.
[0003] Pressure injuries not only have a negative impact on the patient's overall health (physiological, psychological, functional and social aspects), but also bring serious economic burdens. Severe pressure injuries are often accompanied by tissue necrosis and even develop into refractory wounds, causing great pain to patients.
[0004] At present, the treatment methods for pressure injuries include body position management, wound cleaning / debridement, surgical removal of necrotic tissue, negative pressure wound therapy, appropriate dressing application, moist wound healing, and improved nutrient metabolism. However, in many cases, the healing time of pressure injuries is still long. To solve the above problems, people are constantly exploring the development of new treatment methods and dressings. Dressings not only provide a physical barrier at the wound site, but also provide a temporary transient additional cell matrix so that cells can migrate and accelerate the healing process. In addition, different biological agents, such as drugs, growth factors (GF), cells, etc., can be loaded into dressings to enhance the healing process. Advanced moist dressings have made some progress in improving the healing rate, but their overall average healing rate is still not high. Traditional dressings cannot effectively penetrate necrotic tissue or hyperkeratotic skin layers, thereby limiting drug delivery and cell migration. Existing wound dressings are usually film-like structures, which are difficult to cover and treat irregularly shaped wounds, and may also cause the wound to not heal completely.
[0005] Therefore, there is still a lack of more effective pressure injury treatment products in the prior art. Summary of the invention
[0006] The purpose of the present invention is to provide a preparation method and application of a microneedle patch, which can effectively treat pressure injuries.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing a microneedle patch, comprising the following steps:
[0009] mixing a photoinitiator solution, methacrylated hyaluronic acid, platelet-rich fibrin (PRF) and polyethylene glycol diacrylate to obtain a microneedle solution;
[0010] The microneedle solution is added into the mold and solidified to obtain a microneedle patch.
[0011] Preferably, the photoinitiator contains lithium phenyl (2,4,6-trimethylbenzoyl) phosphate (LAP) or 2-hydroxy-4′-(2-hydroxyethoxy)-2-methylpropiophenone (I2959);
[0012] The concentration of the photoinitiator solution is 2-3 mg / ml.
[0013] Preferably, the final concentration of methacrylated hyaluronic acid in the microneedle solution is 20 to 40 mg / ml.
[0014] Preferably, the final concentration of platelet-rich fibrin in the microneedle solution is 3 to 8 mg / ml;
[0015] And / or, the platelet-rich fibrin is in the form of a lyophilized powder.
[0016] Preferably, the final concentration of polyethylene glycol diacrylate in the microneedle solution is 1.5-2.5%.
[0017] Preferably, the mold is a polydimethylsiloxane (PDMS) mold;
[0018] The microneedle specifications preset in the mold are:
[0019] The circular base has a diameter of 400 to 500 μm, a height of 500 to 700 μm, and a tip spacing of 800 to 1000 μm.
[0020] Preferably, the step of adding the microneedle solution into the mold comprises the following steps:
[0021] S1, adding the microneedle solution into the mold, centrifuging and heating and concentrating in sequence;
[0022] S2, after heating and concentrating, repeat the steps in S1 2 to 4 times;
[0023] The centrifugal speed is 3000-5000 rpm, and the centrifugal time is 5-15 min.
[0024] Preferably, the curing is carried out by ultraviolet irradiation, and the curing time is 5 to 20 seconds;
[0025] After the solidification, the steps of adding a base solution and drying to obtain a base are also included;
[0026] The base solution contains one or more of polyvinyl alcohol, polyamide, polyethylene, polypropylene, polystyrene, acrylonitrile-butadiene-styrene copolymer, polyethylene terephthalate, polyethylene naphthalate, polyurethane, polyimide, polyetheretherketone, methacrylated hyaluronic acid or polyphenylene sulfide.
[0027] The present invention also provides a microneedle patch prepared by the preparation method described in the claim.
[0028] The present invention also provides the use of the microneedle patch in preparing a product for treating pressure injuries.
[0029] Beneficial effects of the present invention:
[0030] The microneedle patch obtained by the preparation method provided by the present invention can achieve the effect of slowing down the swelling of microneedles. The slowing down of the swelling rate can make the release rate of growth factors more controllable and stable, ensure the continuous and effective drug concentration, and improve the stability and reliability of the treatment effect. At the same time, it can extend the effective use time of microneedles, reduce the replacement frequency, improve the compliance and comfort of patients, and thus reduce the cost of treatment.
[0031] The microneedle patch prepared by the present invention can stimulate the regeneration and healing of tissues around the wound and improve the treatment effect. The microneedle patch has a stable structure, is easy to carry and use, and has good biocompatibility. It can achieve deeper pressure injury wound treatment and promote wound healing. It has a wide range of clinical application prospects and provides a new means for the treatment of patients with pressure injuries. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a schematic diagram of the preparation process of the microneedle patch of the present invention;
[0033] Figure 2 The diagram is a result of the morphology observation of the microneedle patch of the present invention, wherein: the left picture is an overall photo of the HAMA microneedle patch prepared by the present invention; the middle picture is a multi-focus picture of the microneedle patch of the present invention under an ultra-depth-of-field microscope; the right picture is a microneedle height distribution diagram obtained by three-dimensional imaging technology.
[0034] Figure 3 This is a diagram of VEGF release;
[0035] Figure 4 This is the result diagram of the swelling of the microneedle patch;
[0036] Figure 5 Observation results for promoting the healing of pressure injury wounds. DETAILED DESCRIPTION
[0037] The present invention provides a method for preparing a microneedle patch, comprising the following steps:
[0038] mixing a photoinitiator solution, methacrylated hyaluronic acid, platelet-rich fibrin and polyethylene glycol diacrylate to obtain a microneedle solution;
[0039] The microneedle solution is added into the mold and solidified to obtain a microneedle patch.
[0040] In the present invention, preferably, the photoinitiator is LAP; the concentration of the photoinitiator solution is 2-3 g / ml; preferably, the final concentration of methacrylated hyaluronic acid in the microneedle solution is 20-40 mg / ml; preferably, the final concentration of PRF in the microneedle solution is 3-8 mg / ml; and / or, the dosage form of PRF is a lyophilized powder; preferably, the final concentration of polyethylene glycol diacrylate in the microneedle solution is 1.5-2.5%; preferably, the mold is a PDMS mold; the preset microneedle specifications in the mold are: a circular base diameter of 400-500 μm, a height of 500-700 μm, and a needle tip spacing of 800-1000 μm.
[0041] In the present invention, the step of adding the microneedle solution into the mold preferably comprises the following steps:
[0042] S1, adding the microneedle solution into the mold, centrifuging and heating and concentrating in sequence;
[0043] S2, after heating and concentrating, repeat the steps in S1 2 to 4 times; preferably, the centrifugal speed is 3000 to 5000 rpm, and the centrifugal time is 5 to 15 minutes; the curing adopts ultraviolet light irradiation, and the curing time is 5 to 20 seconds; after the curing, it also includes the steps of adding a substrate solution and drying to obtain a substrate; the substrate solution contains one or more of polyvinyl alcohol, polyamide, polyethylene, polypropylene, polystyrene, acrylonitrile-butadiene-styrene copolymer, polyethylene terephthalate, polyethylene naphthalate, polyurethane, polyimide, polyetheretherketone or polyphenylene sulfide.
[0044] The present invention also provides a microneedle patch prepared by the preparation method described in the claim.
[0045] The present invention also provides the use of the microneedle patch in preparing a product for treating pressure injuries.
[0046] In the present invention, the application method of the microneedle patch comprises the following steps:
[0047] Clean the wound: Clean and disinfect the pressure injury wound to ensure that the wound surface is dry;
[0048] Apply the microneedle patch: Apply the microneedle patch to the pressure injury wound, press gently to allow the microneedles to penetrate the wound surface, and ensure that the conical needle structure of the microneedle contacts the wound bed to enhance adhesion;
[0049] Retention time: The microneedle patch is left on the wound surface to gradually release the growth factors in platelet-rich fibrin to promote wound healing. It should be replaced after 2 to 4 days.
[0050] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0051] Example 1
[0052] Preparation of PRF powder:
[0053] Collect autologous blood samples: Collect a certain amount of blood samples from the orbit, abdominal aorta or other suitable parts of SD rats, transfer the blood samples to centrifuge tubes (4 ml per tube) without adding anticoagulants.
[0054] Separation of PRF: Within 1 minute after collection, the whole blood sample was centrifuged in a refrigerated centrifuge (4°C, 400g centrifugation for 10 minutes), and the sample was left to stand until it was separated into three layers: a transparent serum layer, a platelet-rich fibrin layer, and a red blood cell coagulation layer. The upper layer was discarded, the sediment layer containing red blood cells was removed, and finally the fibrin gel in the middle layer was extracted. The PRF layer was taken out and placed in a sterile centrifuge tube and frozen in a -80°C refrigerator. Then, freeze-dried PRF was prepared by freeze drying in a freeze dryer, and ground into PRF powder.
[0055] Preparation of HAMA:
[0056] 2.0 g HA (hyaluronic acid) (Mw 400-800 kDa) was added to 200 ml deionized water and stirred overnight until the HA solution was completely dissolved.
[0057] 2 ml of methacrylamide (MA) was added dropwise to the prepared HA solution, and the reaction was carried out under ice bath conditions, while the pH was kept at 8-9 during the reaction. After stirring overnight, the system was diluted with 2000 ml of PBS and dialyzed with a dialysis membrane (Mw = 3.5 kMa) for 3 days. Finally, the purified product was collected by freeze drying.
[0058] Preparation of microneedle patch:
[0059] The photoinitiator LAP was weighed and dissolved in deionized water to a concentration of 2.5 mg / ml. HAMA was weighed and dissolved in LAP to a final concentration of 30 mg / ml. 5 mg / ml of freeze-dried PRF powder was added under stirring. PEGDA (polyethylene glycol diacrylate) was added at a final concentration of 2% to obtain a microneedle solution.
[0060] The MN master was prepared using 3D printing technology so that the specifications of the MN, including the height, width, and length of the MN, could be freely adjusted. The circular base diameter of each needle was 450 μm, the height was 600 μm, and the tip spacing of the needle was 900 μm. Polydimethylsiloxane (PDMS) was placed on the 3D printed MNs master to make a master mold, which was then cured in an oven at 60 ° C for 8 h, and finally the master mold was completed by carefully peeling off the 3D printed MNs.
[0061] 300 μL of microneedle solution was added into the PDMS mold and centrifuged (4000 rpm, 10 min). The excess solution outside the needle body was scraped off and the solution was concentrated in an oven for 2.5 h. The microneedle solution was added again and centrifuged. The mixture was concentrated by heating and repeated 3 times. The microneedles were irradiated with an ultraviolet lamp (365 nm, 7 w) for 10 s to solidify. Then 15% PVA (polyvinyl alcohol) solution was added as the microneedle substrate and dried at 36 °C. The mold was then demolded to obtain a complete PRF-HAMA.
[0062] Example 2
[0063] The difference from Example 1 is that the preparation method of the microneedle patch is:
[0064] The photoinitiator LAP was weighed and dissolved in deionized water to a concentration of 2 mg / ml. HAMA was weighed and dissolved in LAP to a final concentration of 20 mg / ml. 3 mg / ml of freeze-dried PRF powder was added under stirring. PEGDA (polyethylene glycol diacrylate) was added to a final concentration of 2% to obtain a microneedle solution.
[0065] The MN master was prepared using 3D printing technology so that the specifications of the MN, including the height, width, and length of the MN, could be freely adjusted. The circular base diameter of each needle was 450 μm, the height was 600 μm, and the tip spacing of the needle was 900 μm. Polydimethylsiloxane (PDMS) was placed on the 3D printed MNs master to make a master mold, which was then cured in an oven at 60 ° C for 8 h, and finally the master mold was completed by carefully peeling off the 3D printed MNs.
[0066] 300 μL of microneedle solution was added into the PDMS mold and centrifuged (4000 rpm, 10 min). The excess solution outside the needle body was scraped off and the solution was concentrated in an oven for 2 h. The microneedle solution was added again and centrifuged. The mixture was concentrated by heating and repeated 3 times. The microneedles were irradiated with an ultraviolet lamp (365 nm, 7 w) for 10 s to solidify. Then 15% PVA (polyvinyl alcohol) solution was added as the microneedle substrate and dried at 35 °C. Finally, the mold was removed to obtain a complete PRF-HAMA.
[0067] Example 3
[0068] The difference from Example 1 is that the preparation method of the microneedle patch is:
[0069] The photoinitiator LAP was weighed and dissolved in deionized water to a concentration of 3 mg / ml, HAMA was weighed and dissolved in LAP to make a final concentration of 40 mg / ml, and 8 mg / ml of freeze-dried PRF powder was added under stirring, and PEGDA (polyethylene glycol diacrylate) was added to a final concentration of 2% to obtain a microneedle solution.
[0070] The MN master was prepared using 3D printing technology so that the specifications of the MN, including the height, width, and length of the MN, could be freely adjusted. The circular base diameter of each needle was 450 μm, the height was 600 μm, and the tip spacing of the needle was 900 μm. Polydimethylsiloxane (PDMS) was placed on the 3D printed MNs master to make a master mold, which was then cured in an oven at 60 ° C for 8 h, and finally the master mold was completed by carefully peeling off the 3D printed MNs.
[0071] 300 μL of microneedle solution was added into the PDMS mold and centrifuged (4000 rpm, 10 min). The excess solution outside the needle body was scraped off and the solution was concentrated in an oven for 3 h. The microneedle solution was added again and centrifuged. The mixture was concentrated by heating and repeated 3 times. The microneedles were irradiated with an ultraviolet lamp (365 nm, 7 w) for 10 s to solidify. Then 15% PVA (polyvinyl alcohol) solution was added as the microneedle substrate and dried at 37 ° C. Finally, the mold was removed to obtain a complete PRF-HAMA.
[0072] Comparative Example 1
[0073] The difference from Example 1 is that the preparation method of the microneedle patch is:
[0074] The photoinitiator LAP was weighed and dissolved in deionized water to a concentration of 2.5 mg / ml, HAMA was weighed and dissolved in LAP to a final concentration of 30 mg / ml, and 5 mg / ml of freeze-dried PRF powder was added under stirring to obtain a microneedle solution.
[0075] The MN master was prepared using 3D printing technology so that the specifications of the MN, including the height, width, and length of the MN, could be freely adjusted. The circular base diameter of each needle was 450 μm, the height was 600 μm, and the tip spacing of the needle was 900 μm. Polydimethylsiloxane (PDMS) was placed on the 3D printed MNs master to make a master mold, which was then cured in an oven at 60 ° C for 8 h, and finally the master mold was completed by carefully peeling off the 3D printed MNs.
[0076] 300 μL of microneedle solution was added into the PDMS mold and centrifuged (4000 rpm, 10 min). The excess solution outside the needle body was scraped off and the solution was concentrated in an oven for 2-3 h. The microneedle solution was added again and centrifuged. The microneedles were concentrated by heating and repeated 3 times. The microneedles were irradiated with ultraviolet light (365 nm, 7 w) for 10 s and then solidified. Then 15% PVA (polyvinyl alcohol) solution was added as the microneedle substrate and dried at 35°C-37°C. Finally, the mold was demolded to obtain a complete PRF-HAMA.
[0077] Comparative Example 2
[0078] The difference from Example 1 is that the preparation method of the microneedle patch is:
[0079] The photoinitiator LAP was weighed and dissolved in deionized water to a concentration of 2.5 mg / ml. HAMA was weighed and dissolved in LAP to a final concentration of 30 mg / ml. 5 mg / ml of freeze-dried PRF powder was added under stirring. PEGDA (polyethylene glycol diacrylate) was added at a final concentration of 1% to obtain a microneedle solution.
[0080] The MN master was prepared using 3D printing technology so that the specifications of the MN, including the height, width, and length of the MN, could be freely adjusted. The circular base diameter of each needle was 450 μm, the height was 600 μm, and the tip spacing of the needle was 900 μm. Polydimethylsiloxane (PDMS) was placed on the 3D printed MNs master to make a master mold, which was then cured in an oven at 60 ° C for 8 h, and finally the master mold was completed by carefully peeling off the 3D printed MNs.
[0081] 300 μL of microneedle solution was added into the PDMS mold and centrifuged (4000 rpm, 10 min). The excess solution outside the needle body was scraped off and the solution was concentrated in an oven for 2-3 h. The microneedle solution was added again and centrifuged. The microneedles were concentrated by heating and repeated 3 times. The microneedles were irradiated with ultraviolet light (365 nm, 7 w) for 10 s and then solidified. Then 15% PVA (polyvinyl alcohol) solution was added as the microneedle substrate and dried at 35°C-37°C. Finally, the mold was demolded to obtain a complete PRF-HAMA.
[0082] Comparative Example 3
[0083] The difference from Example 1 is that the preparation method of the microneedle patch is:
[0084] The photoinitiator LAP was weighed and dissolved in deionized water to a concentration of 2.5 mg / ml. HAMA was weighed and dissolved in LAP to a final concentration of 30 mg / ml. 5 mg / ml of freeze-dried PRF powder was added under stirring. PEGDA (polyethylene glycol diacrylate) was added at a final concentration of 3% to obtain a microneedle solution.
[0085] The MN master was prepared using 3D printing technology so that the specifications of the MN, including the height, width, and length of the MN, could be freely adjusted. The circular base diameter of each needle was 450 μm, the height was 600 μm, and the tip spacing of the needle was 900 μm. Polydimethylsiloxane (PDMS) was placed on the 3D printed MNs master to make a master mold, which was then cured in an oven at 60 ° C for 8 h, and finally the master mold was completed by carefully peeling off the 3D printed MNs.
[0086] 300 μL of microneedle solution was added into the PDMS mold and centrifuged (4000 rpm, 10 min). The excess solution outside the needle body was scraped off and the solution was concentrated in an oven for 2-3 h. The microneedle solution was added again and centrifuged. The microneedles were concentrated by heating and repeated 3 times. The microneedles were irradiated with ultraviolet light (365 nm, 7 w) for 10 s and then solidified. Then 15% PVA (polyvinyl alcohol) solution was added as the microneedle substrate and dried at 35°C-37°C. Finally, the mold was demolded to obtain a complete PRF-HAMA.
[0087] Experimental Example 1: Morphology Observation
[0088] The microneedle patch prepared in Example 1 was photographed by an ordinary camera and an ultra-depth microscope to show the overall and local structure and height distribution of the microneedles. Figure 2 shown.
[0089] The picture on the left is an overall photo of the HAMA microneedle patch prepared by the present invention, and the picture shows that the patch is round and transparent, and the microneedle structure is neatly arranged on the surface.
[0090] The middle picture is a multi-focus picture of the microneedle patch of the present invention under an ultra-depth microscope. The arrangement and shape of the microneedles can be clearly seen in the picture, where each microneedle presents a slender cone structure with a thicker bottom and gradually tapering at the top. The height of the microneedle is about 590μm and the base is about 450μm.
[0091] The picture on the right is a microneedle height distribution map obtained through three-dimensional imaging technology. The colors in the picture represent the height of the microneedles from blue to red. It can be seen from the picture that the height of each microneedle is evenly distributed, with red at the top and blue at the bottom.
[0092] Experimental Example 2 Drug Release Efficiency Detection
[0093] Experimental method: HAMA-PRF microneedle patches prepared in Example 1 under the same conditions and 10 mg freeze-dried PRF were placed in 6-well plates containing PBS, 5 mL PBS was added to each well, and the cells were incubated in a 37 ° C constant temperature incubator to simulate the in vivo environment, and samples were taken at different time points (1 hour, 4 hours, 24 hours, 48 hours, and 72 hours). Take 1 mL of sample at each time point and add fresh PBS to maintain the total volume. According to the ELISA kit instructions, standard solutions of 10 pg / ml, 20 pg / ml, 40 pg / ml, 80 pg / ml, 160 pg / ml, and 320 pg / ml were used to construct a standard curve; the collected samples were added to a 96-well plate and operated according to the ELISA kit operating steps, including adding detection antibodies, enzyme-labeled secondary antibodies, colorimetric substrates, and stop solutions. The optical density (OD value) was read using an ELISA reader, and the concentration of VEGF in the sample was calculated according to the standard curve.
[0094] The experimental results show that the VEGF concentration released by the HAMA-PRF microneedle patch provided by the present invention is always slightly higher than that of freeze-dried PRF during the entire incubation process, and the VEGF release of both increases rapidly in the initial stage (1 hour to 24 hours) and tends to be stable in the later stage (48 hours to 72 hours).
[0095] Experimental Example 3 Swelling Record
[0096] Experimental method: The microneedles prepared in Example 1 and Comparative Examples 1 to 3 were used as samples, and the initial weight of the microneedles was weighed. Then 3 ml of PBS was added to the prepared microneedle samples, and the samples were taken out at different time points (10 min, 40 min, 1 h, 2 h, 16 h, and 24 h). After the surface moisture was absorbed with filter paper, the mass of the microneedles was immediately weighed (record the wet weight). Swelling was calculated according to the formula: Swelling = (wet weight - dry weight) / dry weight,
[0097] The experimental results show that the product prepared in Example 1 provided by the present invention can achieve the lowest swelling rate.
[0098] Experimental Example 4: Efficacy Verification
[0099] Experimental methods: Select eligible SPF-grade healthy adult male SD rats weighing 200-250g. After one week of adaptive feeding, the experimental operation was carried out. After inhalation anesthesia with gas (isoflurane), the back skin was depilated and disinfected, and a circular magnet with a diameter of 12mm and a thickness of 1mm was implanted under the skin, and disinfected after the operation. After the rats recovered from anesthesia for 24 hours, the ischemia / reperfusion (I / R) cycle was started. A circular magnet with a diameter of 12mm, a thickness of 3mm, and a magnetic flux density of 2000 Gauss was placed on the implanted magnet to form a 2-hour ischemia cycle, followed by reperfusion for 30 minutes. Five cycles were performed per day, and 11.5 hours of reperfusion were allowed at the end of each day. After 15 I / R cycles (3 days), it was observed that the wound on the back of the rats after acupuncture was black and hardened, without bleeding, and the wound performance was consistent with stage III PI. Six SD rat models of pressure injury were established. After successful modeling, debridement was performed and then the rats were randomly divided into 2 groups (n=3): ① blank control group: no intervention; ② PRF-HAMA microneedle patch group: the microneedle patch prepared in Example 1 was used and adhered to the pressure injury wound after pressing. The experimental group was intervened every 2 days and photographed and recorded until the end of the experiment. Observation indicators: Wound healing rate (the observation time nodes were the day after successful modeling and the 1st, 3rd, 6th and 9th days thereafter, and image analysis software (ImageJ) was used for analysis; wound healing rate = (D0-D x ) Wound area / D0 wound area×100%
[0100] The experimental results showed that the healing rate of the microneedle group was higher than that of the blank group from the first day to the ninth day, indicating that the microneedles provided by the present invention can promote the healing of pressure injury wounds.
[0101] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a microneedle patch, characterized in that: The following steps are involved: mixing a photoinitiator solution, methacrylated hyaluronic acid, platelet-rich fibrin and polyethylene glycol diacrylate to obtain a microneedle solution; The microneedle solution is added into the mold and solidified to obtain a microneedle patch.
2. The preparation method according to claim 1, characterized in that: The photoinitiator contains phenyl (2,4,6-trimethylbenzoyl) lithium phosphate or 2-hydroxy-4′-(2-hydroxyethoxy)-2-methylpropiophenone; The concentration of the photoinitiator solution is 2-3 mg / ml.
3. The preparation method according to claim 1, characterized in that: The final concentration of methacrylated hyaluronic acid in the microneedle solution is 20-40 mg / ml.
4. The preparation method according to claim 1, characterized in that: The final concentration of platelet-rich fibrin in the microneedle solution is 3 to 8 mg / ml; And / or, the platelet-rich fibrin is in the form of a lyophilized powder.
5. The preparation method according to claim 1, characterized in that: The final concentration of polyethylene glycol diacrylate in the microneedle solution is 1.5-2.5%.
6. The preparation method according to claim 1, characterized in that: The mold is a polydimethylsiloxane mold; The microneedle specifications preset in the mold are: The circular base has a diameter of 400 to 500 μm, a height of 500 to 700 μm, and a tip spacing of 800 to 1000 μm.
7. The preparation method according to claim 6, characterized in that: The step of adding the microneedle solution into the mold comprises the following steps: S1, adding the microneedle solution into the mold, centrifuging and heating and concentrating in sequence; S2, after heating and concentrating, repeat the steps in S1 2 to 4 times; The centrifugal speed is 3000-5000 rpm, and the centrifugal time is 5-15 min.
8. The preparation method according to claim 7, characterized in that: The curing is carried out by ultraviolet irradiation, and the curing time is 5 to 20 seconds; After the solidification, the steps of adding a base solution and drying to obtain a base are also included; The base solution contains one or more of polyvinyl alcohol, polyamide, polyethylene, polypropylene, polystyrene, acrylonitrile-butadiene-styrene copolymer, polyethylene terephthalate, polyethylene naphthalate, polyurethane, polyimide, polyetheretherketone, methacrylated hyaluronic acid or polyphenylene sulfide.
9. A microneedle patch prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the microneedle patch according to claim 9 in preparing a product for treating pressure injuries.