Bimetal catalyst as well as preparation method and application thereof
The current problem was solved by converting 2,3,5,6-tetrachloropyridine into 2,3-dichloropyridine and 2,3,5-trichloropyridine in a hydrodechlorination reaction using a palladium-containing bimetallic catalyst. The problem of complicated synthesis steps and high cost in the technology has been solved, and efficient and low-cost industrial production has been achieved.
Patent Information
- Application Number
- CN202410426202.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-14
- Filing Date
- 2024-04-10
- Publication Date
- 2024-10-18
AI Technical Summary
The existing synthesis methods of 2,3-dichloropyridine and 2,3,5-trichloropyridine have problems such as complicated steps, expensive raw materials, high cost, low product yield, and unsuitable for industrial production.
Using a palladium carbon catalyst containing silver, nickel, zinc, copper, chromium, manganese, cobalt, iron or zirconium, nano activated carbon is prepared through hydrothermal carbonization reaction, and a bimetallic catalyst is obtained through impregnation and calcination for use in hydrodechlorination The selectivity of 2,3,5,6-tetrachloropyridine is improved during the reaction and converted into 2,3-dichloropyridine and 2,3,5-trichloropyridine.
High selective conversion rate and product yield of 2,3-dichloropyridine and 2,3,5-trichloropyridine are achieved. The process is simple and low-cost, suitable for industrial production, and the stability and activity of the catalyst are maintained.
Smart Images

Figure BDA0004784700630000091 
Figure BDA0004784700630000092 
Figure BDA0004784700630000101
Abstract
Description
Technical Field
[0001] The invention belongs to the field of chemical technology, and specifically relates to a bimetallic catalyst and a preparation method and application thereof. The bimetallic catalyst is a palladium-carbon catalyst containing silver, nickel, zinc, copper, chromium, manganese, cobalt, iron or zirconium. Background Art
[0002] 2,3-Dichloropyridine and 2,3,5-trichloropyridine are very important chemical intermediates and are widely used in pesticides, medicines and other fields.
[0003] 2,3-Dichloropyridine is an important substance for the synthesis of the new insecticide chlorantraniliprole. At present, there are several methods for the synthesis of 2,3-dichloropyridine: 2,3,6-trichloropyridine reduction method, 2-chloropyridine synthesis method, 3-chloropyridine synthesis method and synthesis method using nicotinamide as raw materials. Among them, the raw materials of the 2,3,6-trichloropyridine reduction method are not easy to obtain, the reaction conditions have high requirements on equipment, and the selectivity is not high; the target product of the 2-chloropyridine synthesis method is difficult to separate, the yield is not high, and it does not have the value of industrial production; the raw materials and reagents used in the 3-chloropyridine synthesis method are too expensive, the yield is low, and there is no advantage; the synthesis method using nicotinamide as raw material, the raw materials are obtained by Hofmann degradation, chlorination, diazotization and Sandmeyer reaction, this synthesis route has many steps, complex process, difficult to control and low yield, and the product quality is not high.
[0004] 2,3,5-Trichloropyridine reacts with alkali metal hydroxide to prepare 3,5-dichloro-2-pyridinol, which is an important raw material for synthesizing a series of pesticides such as insecticides and herbicides such as oxadiazine. 2,3,5-Trichloropyridine can also be further subjected to fluorination reaction to synthesize 2,3-difluoro-5-chloropyridine, which is the basic raw material for synthesizing the herbicide clodinafop-butyl. At present, there are not many reports on the synthesis methods of 2,3,5-trichloropyridine, mainly the following: (1) US4127575 and GB1215387A respectively disclose the synthesis of 2,3,5-trichloropyridine using trichlorohydrazine pyridine and 3,5-dichloro-2-pyridone as raw materials. These two methods have fewer reaction steps and relatively ideal yields, but both have disadvantages such as expensive and difficult to obtain raw materials; (2) Patent 201410669523.5 discloses the reaction of 2-chloropyridine with water or alcohols under base catalysis. 2-Alkoxypyridine is generated, and 2-alkoxypyridine reacts with a chlorinating agent in the presence of a base to generate 3,5-dichloro-2-alkoxypyridine, which is then chlorinated to obtain 2,3,5-trichloropyridine. This synthesis method is complicated and produces a lot of industrial "three wastes", making it unsuitable for industrial production. (3) U.S. Patent No. 4245098 discloses a technology for synthesizing 2,3,5-trichloropyridine by a catalytic cyclization method, which mainly includes using trichloroacetaldehyde and acrylonitrile as raw materials to prepare 2,3,5-trichloropyridine under the action of a catalyst. The synthesis process is complicated, the reaction conditions are harsh, and it is difficult to control. In addition, a large amount of metal salts are used, which will pollute the environment. At the same time, the product yield is not ideal. (4) The preparation method of 2,3,5-trichloropyridine disclosed in CN105887128A is to use an acidic solution as a reaction medium and pentachloropyridine as a raw material to generate 2,3,4,5-tetrachloropyridine and 2,3,5-trichloropyridine through electrolysis reaction, and then separate and purify them. The preparation method of 2,3,5-trichloropyridine disclosed in CN108358835A is to use water as a solvent, sodium carbonate as an acid binding agent, and butanol as a catalyst auxiliary agent to react 2,3,4,5-tetrachloropyridine with hydrazine hydrate to generate trichloropyridine hydrazine group, and then directly oxidize it with hydrogen peroxide under the action of alkaline substances and phase transfer catalysts to obtain 2,3,5-trichloropyridine.
[0005] Patents in this regard only involve the preparation of one product, and the process is complicated and the effect is poor. Therefore, it is necessary to develop a synthetic process that is simple, environmentally friendly, low-cost, and has a high product yield and high purity. Summary of the invention
[0006] Problem that the invention aims to solve
[0007] The present invention aims to provide a bimetallic catalyst and a preparation method and application thereof. The bimetallic catalyst is a palladium-carbon catalyst containing silver, nickel, zinc, copper, chromium, manganese, cobalt, iron or zirconium. The catalyst can improve the raw material conversion rate and product selectivity of selectively hydrodechlorinating 2,3,5,6-tetrachloropyridine to prepare 2,3-dichloropyridine and 2,3,5-trichloropyridine, and the catalyst has excellent stability and can still maintain high activity after multiple cycles. The preparation method of the catalyst and the method for preparing 2,3-dichloropyridine and 2,3,5-trichloropyridine using the catalyst have simple process, low cost, simple post-treatment process, low cost, and are suitable for industrial production.
[0008] Solutions for solving problems
[0009] In order to solve the above problems, the present invention provides a method for preparing a bimetallic catalyst, which comprises the following steps:
[0010] (1) using a sugar aqueous solution as a raw material to carry out a hydrothermal carbonization reaction, cooling, filtering, and drying to obtain nano-activated carbon;
[0011] (2) impregnating the pretreated activated carbon in an alcohol or / and aqueous solution of palladium chloride, and drying after the impregnation to obtain catalyst 1;
[0012] (3) impregnating the catalyst 1 in an alcohol or / and aqueous solution of an auxiliary agent, calcining and drying after the impregnation is completed;
[0013] Wherein, the auxiliary agent is silver nitrate, nickel nitrate, zinc chloride, copper chloride, chromium chloride, manganese chloride, cobalt chloride, ferric chloride or zirconium chloride.
[0014] Preferably, the auxiliary agent in step (1) is nickel nitrate.
[0015] Preferably, the nano activated carbon in step (1) is spherical according to SEM characterization. Ordinary activated carbon is amorphous according to SEM characterization.
[0016] Preferably, the specific surface area of the nano activated carbon in step (1) is 500-3000m 2 / g. In a specific embodiment, the specific surface area of the nano-activated carbon can be 600m 2 / g、700m 2 / g、800m 2 / g、900m 2 / g、1000m 2 / g、1100m 2 / g、1200m 2 / g、1300m 2 / g、1400m 2 / g、1500m2 / g、1600m 2 / g、1700m 2 / g、1800m 2 / g、1900m 2 / g, 2000m 2 / g, 2200m 2 / g, 2400m 2 / g, 2600m 2 / g、2800m 2 / g or 3000m 2 / g, etc.
[0017] Preferably, the average pore size of the nano activated carbon in step (1) is 1.0-10 nm. In a specific embodiment, the average pore size of the nano activated carbon can be 1.5 nm, 2.0 nm, 2.5 nm, 3.0 nm, 3.5 nm, 4.0 nm, 4.5 nm, 5.0 nm, 5.5 nm, 6.0 nm, 6.5 nm, 7.0 nm, 7.5 nm, 8.0 nm, 8.5 nm, 9.0 nm, 9.5 nm or 10 nm, etc.
[0018] Preferably, the pore volume of the nano-activated carbon in step (1) is 0.5-3.0 cm 3 / g. In a specific embodiment, the pore volume of the nano-activated carbon can be 0.75cm 3 / g, 1.0cm 3 / g, 1.25cm 3 / g, 1.5cm 3 / g, 1.75cm 3 / g, 2.0cm 3 / g, 2.25cm 3 / g, 2.50cm 3 / g, 2.75cm 3 / g or 3.0cm 3 / g etc.
[0019] Preferably, the mass specific capacity of the nano activated carbon in step (1) is 100-450F / g. In a specific embodiment, the mass specific capacity of the nano activated carbon can be 150F / g, 200F / g, 250F / g, 300F / g, 350F / g, 400F / g or 450F / g, etc.
[0020] Preferably, the sugar in step (1) is one or more of glucose, fructose, sucrose or xylose.
[0021] Preferably, the concentration of the aqueous solution of sugar in step (1) is 0.2-0.6 mol / L. In a specific embodiment, the concentration of the aqueous solution of sugar is 0.25 mol / L, 0.3 mol / L, 0.35 mol / L, 0.4 mol / L, 0.45 mol / L, 0.5 mol / L, 0.55 mol / L or 0.6 mol / L, etc.
[0022] Preferably, the temperature of the hydrothermal carbonization reaction in step (1) is 150°C-250°C, for example, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C or 250°C, etc.
[0023] Preferably, the time of the hydrothermal carbonization reaction in step (1) is 8 h to 20 h, for example, 9 h, 10 h, 11 h, 12 h, 13 h, 14 h, 15 h, 16 h, 17 h, 18 h, 19 h or 20 h, etc.
[0024] Preferably, the drying temperature in step (1) is 40-80°C, such as 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C.
[0025] Preferably, the drying time in step (1) is 2-12 h, for example, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h or 12 h, etc.
[0026] Preferably, the mass ratio of palladium in the palladium chloride to the nano activated carbon in step (2) is 2% to 10%:1, for example, 3%:1, 4%:1, 5%:1, 6%:1, 7%:1, 8%:1, 9%:1 or 10%:1, etc.
[0027] Preferably, the alcohol in step (2) is ethanol, methanol, isopropanol or tert-butanol;
[0028] Preferably, the concentration of the alcohol aqueous solution in step (2) is 60wt%-80wt%, for example, 60wt%, 65wt%, 70wt%, 75wt% or 80wt%.
[0029] Preferably, the immersion time in step (2) is 6-24 h, for example 6 h, 8 h, 10 h, 12 h, 14 h, 15 h, 16 h, 18 h, 20 h, 22 h or 24 h, etc.
[0030] Preferably, the drying temperature in step (2) is 30-50°C, such as 30°C, 35°C, 40°C, 45°C or 50°C.
[0031] Preferably, the drying time in step (2) is 6-12 h, for example, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h or 12 h, etc.
[0032] Preferably, the molar ratio of the metal in the auxiliary agent in step (3) to the palladium in the palladium chloride in step (2) is 0.01-0.1:1, preferably 0.05-0.1:1, more preferably 0.07:1; for example, 0.01:1, 0.02:1, 0.03:1, 0.04:1, 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1 or 0.1:1, etc.
[0033] Preferably, the immersion time in step (3) is 6-24 h, for example 6 h, 8 h, 10 h, 12 h, 14 h, 15 h, 16 h, 18 h, 20 h, 22 h or 24 h, etc.
[0034] Preferably, the calcination temperature in step (3) is 300-400°C, for example, 300°C, 320°C, 340°C, 350°C, 360°C, 380°C or 400°C.
[0035] Preferably, the calcination time in step (3) is 2-4 h, such as 2 h, 2.5 h, 3 h, 3.5 h or 4 h.
[0036] Preferably, the drying temperature in step (3) is 30-50°C, such as 30°C, 35°C, 40°C, 45°C or 50°C.
[0037] Preferably, the drying time in step (3) is 6-12 h, for example, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h or 12 h.
[0038] In another aspect, the present invention provides a bimetallic catalyst obtained by the above preparation method.
[0039] In another aspect, the present invention provides use of the bimetallic catalyst in a dechlorination hydrogenation reaction.
[0040] Preferably, the raw material for the dechlorination hydrogenation reaction is an aromatic ring or heteroaromatic ring compound substituted with chlorine atoms.
[0041] More preferably, the dechlorination hydrogenation reaction is a reaction of preparing 2,3,5-trichloropyridine and 2,3-dichloropyridine from 2,3,5,6-tetrachloropyridine.
[0042] On the other hand, the present invention provides a method for co-producing 2,3,5-trichloropyridine and 2,3-dichloropyridine, which comprises the following steps: in the presence of an organic solvent and an acid binding agent, using 2,3,5,6-tetrachloropyridine as a raw material and hydrogen as a hydrogen source, reacting under the catalysis of the aforementioned bimetallic catalyst to obtain 2,3,5-trichloropyridine and 2,3-dichloropyridine.
[0043] Preferably, the acid binding agent is selected from one or more of an inorganic base, an organic base, a phosphate or a carboxylate.
[0044] Preferably, the inorganic base is one or more of alkali metal hydroxides, alkali metal oxides, alkali metal carbonates, alkali metal bicarbonates, alkaline earth metal carbonates, alkaline earth metal bicarbonates, alkaline earth metal oxides, alkaline earth metal hydroxides, ammonium carbonate, ammonium bicarbonate or acid salts, preferably alkali metal carbonates and alkaline earth metal oxides.
[0045] Furthermore, the inorganic base is selected from one or more of sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, ammonium bicarbonate, magnesium oxide, magnesium hydroxide, calcium oxide, and calcium hydroxide, preferably sodium carbonate or magnesium oxide, and more preferably magnesium oxide.
[0046] The organic base is selected from one or more of pyridine, alkylpyridine or organic amine.
[0047] Furthermore, the alkyl pyridine is selected from one or more of 2-methyl pyridine, 3-methyl pyridine or 4-methyl pyridine.
[0048] Furthermore, the organic amine is selected from one or more of aliphatic amines, alicyclic amines or aromatic amines.
[0049] Furthermore, the organic amine is selected from one or more of methylamine, ethylamine, propylamine, dimethylamine, ethylenediamine, diethylamine or triethylamine.
[0050] Preferably, the phosphate is selected from one or more of dihydrogen phosphate, hydrogen phosphate or orthophosphate.
[0051] Furthermore, the phosphate is selected from one or more of sodium dihydrogen phosphate, potassium dihydrogen phosphate, potassium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, ammonium diphosphate, and triammonium phosphate.
[0052] Preferably, the carboxylate is selected from one or more of formates, acetates, triacrylates and tetrasuccinates.
[0053] Furthermore, the carboxylate is selected from one or more of ammonium formate, sodium formate, potassium formate, ammonium acetate and sodium acetate.
[0054] Preferably, the molar ratio of the acid binding agent to the 2,3,5,6-tetrachloropyridine is 0.2: 1-3: 1. In a specific embodiment, the molar ratio of the acid binding agent to the 2,3,5,6-tetrachloropyridine can be 0.4: 1, 0.6: 1, 0.8: 1, 1.0: 1, 1.2: 1, 1.4: 1, 1.6: 1, 1.8: 1, 2.0: 1, 2.2: 1, 2.4: 1, 2.6: 1, 2.8: 1 or 3.0: 1, etc.
[0055] Preferably, the mass ratio of the 2,3,5,6-tetrachloropyridine to the bimetallic catalyst is 1:0.001-1:0.01. In a specific embodiment, the mass ratio of the 2,3,5,6-tetrachloropyridine to the bimetallic catalyst is 1:0.002, 1:0.003, 1:0.004, 1:0.005, 1:0.006, 1:0.007, 1:0.008, 1:0.009 or 1:0.01, etc.
[0056] Preferably, the organic solvent is selected from one or more of benzene ring-containing compounds, furan compounds, ester solvents, alcohol solvents, nitrile solvents or alkane solvents.
[0057] Furthermore, the organic solvent is selected from: C6-C 12 benzene ring-containing compounds, such as toluene, xylene, trimethylbenzene, p-xylene, etc.; C4-C8 furan compounds, such as tetrahydrofuran; alkane carboxylic acid esters, especially esters of C1-C8 alkane carboxylic acids and C1-C8 alkanols, such as ethyl acetate, propyl acetate, butyl acetate, butyl propionate, etc.; C1-C8 alcohols, such as methanol, ethanol, propanol, isopropanol, etc.; C2-C4 nitriles, such as acetonitrile and propionitrile; C6-C 10 Alkanes, such as n-hexane, cyclohexane, etc.
[0058] Preferably, the mass ratio of the organic solvent to the 2,3,5,6-tetrachloropyridine is 1:1-10:1. In a specific embodiment, the mass ratio of the organic solvent to the 2,3,5,6-tetrachloropyridine may be in the range of 1:1 to 10:1. In certain specific embodiments, the mass ratio of the organic solvent to the 2,3,5,6-tetrachloropyridine may be 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1 or 10:1, etc. In a specific embodiment, the mass ratio of the organic solvent to the 2,3,5,6-tetrachloropyridine is 4 to 1.
[0059] Preferably, the pressure of the hydrogen is 0.1-3 MPa. In a specific embodiment, the pressure of the hydrogen can be 0.2 MPa, 0.3 MPa, 0.4 MPa, 0.5 MPa, 0.6 MPa, 0.7 MPa, 0.8 MPa, 0.9 MPa, 1.0 MPa, 1.2 MPa, 1.4 MPa, 1.5 MPa, 1.6 MPa, 1.8 MPa, 2.0 MPa, 2.2 MPa, 2.4 MPa, 2.5 MPa, 2.6 MPa, 2.8 MPa or 3.0 MPa, etc.
[0060] Preferably, the reaction temperature is 20-100°C, for example, at 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C or 100°C.
[0061] Preferably, the reaction time is not particularly limited, as long as the hydrogenation catalytic reaction is substantially completed. "Substantially completed" means that the conversion rate of the compound of formula (I) is greater than or equal to 80%. Preferably, the reaction time of the method of the present invention can be in the range of 2 hours to 14 hours, such as 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 12 hours or 14 hours, etc.
[0062] Preferably, the reaction further comprises a post-processing step, and the post-processing step comprises steps such as filtration, distillation and rectification.
[0063] Furthermore, the distillation is carried out under normal pressure, and the distillation temperature is 40°C to 100°C.
[0064] Furthermore, the distillation is carried out under a vacuum degree of ≤-0.07 MPa, a distillation temperature of 100°C to 150°C, and a reflux ratio of 5 to 20:1.
[0065] Specifically in the embodiment, 2,3,5,6-tetrachloropyridine and a catalyst are first added to the autoclave, and then an organic solvent and an acid binding agent are added; nitrogen is introduced for displacement 3 times, and finally hydrogen is introduced for displacement; after the displacement is completed, the hydrogen pressure in the autoclave is maintained between 0.1-3.0 MPa, and the temperature is controlled to be maintained within 20-100° C., stirring is started, and the reaction time is 2-14 hours; after the reaction is completed, the temperature is naturally cooled to room temperature, the residual gas in the autoclave is discharged, and nitrogen is introduced for purging; the reaction liquid is filtered to separate the catalyst, the filtrate is subjected to atmospheric distillation to separate the solvent, and then 2,3-dichloropyridine and 2,3,5-trichloropyridine are separated by rectification.
[0066] Compared with the prior art, the present invention has the following advantages:
[0067] 1. The present invention adopts 2,3,4,5-tetrachloropyridine to prepare 2,3-dichloropyridine and 2,3,5-trichloropyridine, uses hydrogen as a hydrogen source, and selectively dechlorinates to obtain 2,3-dichloropyridine and 2,3,5-trichloropyridine under the action of a catalyst and an acid binding agent. The raw materials can be completely converted, and the yields of the two products are as high as more than 96%;
[0068] 2. 2,3,5,6-tetrachloropyridine is a byproduct in the chlorination process of pyridine and has low utilization value. The present invention uses 2,3,5,6-tetrachloropyridine as a raw material to prepare 2,3-dichloropyridine and 2,3,5-trichloropyridine with higher value, and has a simple process, good performance, and great industrial value;
[0069] 3. The catalyst of the present invention uses Pd as an active component, and the reaction performance is further improved through the synergistic effect between metals, while the amount of catalyst used can be reduced and the service life of the catalyst can be extended, thereby reducing the production cost;
[0070] 4. The addition of alkali in the reaction system of the present invention effectively solves the corrosion of the reactor by HCl generated during the reaction and the damage to the catalyst. The reaction process conditions are relatively mild, the reaction is thorough, and no excessive three wastes are generated. The method is economical and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0071] Figure 1 :SEM image of nano activated carbon
[0072] Figure 2 :SEM image of ordinary activated carbon DETAILED DESCRIPTION
[0073] The present invention is further explained and illustrated by means of test examples and embodiments below.
[0074] Example 1 Preparation of Nano-Activated Carbon
[0075] Add 34g sucrose to a glass, add 400ml deionized water to dissolve, stir until the solution is clear at room temperature, transfer to a 500ml hydrothermal kettle, and perform hydrothermal carbonization reaction at 180℃ for 12h to obtain the product. Cool naturally, filter, wash repeatedly with alcohol and water, and dry the solid at 60℃ for 6h to obtain nano-activated carbon. See the attached SEM image of nano-activated carbon. Figure 1 The prepared nano-activated carbon was spherical and had a specific surface area of 935 m 2 / g, average pore diameter is 3.28nm; pore volume is 1.43cm 3 / g, and the mass specific capacity is 400.5F / g.
[0076] Example 2 Preparation of Pd-Ni / C Catalyst
[0077] 32g of palladium chloride was dissolved in 1000ml of ethanol solution with a mass concentration of 70% to obtain an ethanol solution of palladium chloride; 150mL of palladium solution (1eq) was added to 96g of the nano-activated carbon carrier prepared in Example 1, and impregnated for 12h. After the impregnation, it was dried at 60°C for 4h under a nitrogen atmosphere to obtain a primary catalyst; 3.9g of nickel nitrate hexahydrate (0.05eq) was weighed, 10g of deionized water was added to dissolve it, and then it was added dropwise to the primary catalyst, impregnated for 12h, dried at 60°C for 4h under a nitrogen atmosphere, and then placed in a tubular furnace, purged with nitrogen, and calcined under a nitrogen protective atmosphere, the calcination temperature was 300°C, and the calcination time was 3h. After the calcination was completed, it was naturally cooled to room temperature, and 58g of water was added to obtain a Pd-Ni / C catalyst with a water content of 60wt%, which was stored for standby use.
[0078] Example 3 Catalytic Hydrodechlorination
[0079] A method for preparing 2,3-dichloropyridine and 2,3,5-trichloropyridine by using 2,3,5,6-tetrachloropyridine, comprising the following steps:
[0080] (1) A 20 L autoclave was charged with 1 kg (216.9 g / mol, 1 eq) of 2,3,5,6-tetrachloropyridine as a raw material, 4 kg of methanol as a solvent, 50 g (in terms of Pd, 106.4 g / mol, 0.1 eq) of the Pd-Ni / C catalyst (water content 60 wt%) prepared in Example 2, and 185.7 g (40.3 g / mol, 1 eq) of magnesium oxide. The autoclave was replaced with nitrogen three times, and finally hydrogen was introduced to 1 MPa. The temperature was raised to 40° C. and the reaction was carried out for 8 h. Hydrogen was continuously introduced during the process to ensure a reaction pressure of 1 MPa.
[0081] (2) After the reaction is completed, the mixture is naturally cooled to room temperature, hydrogen is removed, nitrogen is replaced, and the catalyst and reaction liquid are separated by filtration.
[0082] (3) The catalyst is separated by filtration and recovered for later use.
[0083] (4) The reaction liquid was tested by liquid chromatography, wherein the raw material conversion rate was 100%. The reaction liquid was subjected to atmospheric distillation at 70°C to separate the solvent methanol; then 2,3-dichloropyridine and 2,3,5-trichloropyridine were obtained by rectification, wherein the rectification temperature was 115°C, the vacuum degree was -0.08MPa, and the reflux ratio was 10:1. The product purities of the obtained 2,3-dichloropyridine and 2,3,5-trichloropyridine were both ≥99%.
[0084] Example 4
[0085] According to the method of Example 2, different bimetallic catalysts can be prepared, including Pd-Zn / C, Pd-Fe / C, Pd-Co / C, etc.
[0086] Using the nano activated carbon of Example 1 as a carrier, Pd / C was prepared according to the preparation method of the primary catalyst in Example 2.
[0087] Using the common activated carbon of Example 1 as a carrier, Pd / C ’ .
[0088] According to the method of Example 3, the above Pd-Zn / C, Pd-Fe / C, Pd-Co / C, Pd / C and Pd / C ’ The catalysts were used for the reaction of 2,3,5,6-tetrachloropyridine to prepare 2,3-dichloropyridine and 2,3,5-trichloropyridine. The reaction results are shown in the following table.
[0089]
[0090] Example 5
[0091] According to the method of Example 2, by changing the molar amount of the auxiliary agent nickel nitrate, bimetallic catalysts with different Pd-Ni ratios can be prepared, wherein the molar ratio of Ni to Pd is 0.01:1, 0.03:1, 0.05:1, 0.07:1 and 0.1:1.
[0092] According to the method of Example 3, the above catalyst was used for the reaction of preparing 2,3-dichloropyridine and 2,3,5-trichloropyridine from 2,3,5,6-tetrachloropyridine. The reaction results are shown in the following table.
[0093]
[0094] Example 6
[0095] According to the method of Example 3, ammonium bicarbonate, potassium bicarbonate, calcium hydroxide, calcium carbonate, sodium carbonate and sodium acetate were selected as acid binding agents, and the reaction results are shown in the following table.
[0096]
[0097] In addition to the above embodiments, the present invention may also have other implementation modes. Any technical solution formed by equivalent replacement or equivalent transformation falls within the protection scope required by the present invention.
Claims
1. A method for preparing a bimetallic catalyst, comprising the following steps: (1) using a sugar aqueous solution as a raw material to carry out a hydrothermal carbonization reaction, cooling, filtering, and drying to obtain nano-activated carbon; (2) impregnating the pretreated activated carbon in an alcohol or / and aqueous solution of palladium chloride, and drying after the impregnation to obtain catalyst 1; (3) impregnating the catalyst 1 in an alcohol or / and aqueous solution of an auxiliary agent, calcining and drying after the impregnation is completed; Wherein, the auxiliary agent is silver nitrate, nickel nitrate, zinc chloride, copper chloride, chromium chloride, manganese chloride, cobalt chloride, ferric chloride or zirconium chloride.
2. The preparation method according to claim 1, characterized in that: The specific surface area of the nano activated carbon is 500-3000m 2 / g; The average pore size of the nano activated carbon is 1.0-10nm; The pore volume of the nano activated carbon is 0.5-3.0cm 3 / g; The mass specific capacity of the nano activated carbon is 100-450F / g.
3. The preparation method according to claim 1 or 2, characterized in that: Step (1) further comprises at least one of the following conditions: The sugar is one or more of glucose, fructose, sucrose or xylose; The concentration of the sugar aqueous solution is 0.2-0.6 mol / L; The temperature of the hydrothermal carbonization reaction is 150-250°C; The hydrothermal carbonization reaction time is 8-20h; The drying temperature is 40-80°C; The drying time is 2-12 hours.
4. The preparation method according to any one of claims 1 to 3, characterized in that Step (2) further comprises at least one of the following conditions: The mass ratio of palladium in the palladium chloride to the nano activated carbon is 2% to 10% to 1; The alcohol is ethanol, methanol, isopropanol or tert-butanol; The concentration of the alcohol aqueous solution is 60wt%-80wt%; The immersion time is 6-24h; The drying temperature is 30-50°C; The drying time is 6-12 hours.
5. The preparation method according to any one of claims 1 to 4, characterized in that: Step (3) further comprises at least one of the following conditions: The molar ratio of the metal in the auxiliary agent to the palladium in the palladium chloride in step (2) is 0.01-0.1:1, preferably 0.05-0.1:1, more preferably 0.07:1; The immersion time is 6-24h; The calcination temperature is 300-400°C; The calcination time is 2-4h; The drying temperature is 30-50°C; The drying time is 6-12 hours.
6. A bimetallic catalyst obtained by the preparation method according to any one of claims 1 to 5.
7. Use of the bimetallic catalyst obtained by the preparation method according to any one of claims 1 to 5 or the bimetallic catalyst according to claim 6 in a dechlorination hydrogenation reaction; preferably, the raw material of the dechlorination hydrogenation reaction is an aromatic ring or heteroaromatic ring compound substituted by a chlorine atom; more preferably, the dechlorination hydrogenation reaction is a reaction for preparing 2,3,5-trichloropyridine and 2,3-dichloropyridine from 2,3,5,6-tetrachloropyridine.
8. A method for co-producing 2,3,5-trichloropyridine and 2,3-dichloropyridine, comprising the following steps: In the presence of an organic solvent and an acid-binding agent, 2,3,5,6-tetrachloropyridine is used as a raw material and hydrogen is used as a hydrogen source. The reaction is carried out under the catalysis of the bimetallic catalyst obtained by the preparation method according to any one of claims 1 to 5 or the bimetallic catalyst according to claim 6 to obtain 2,3,5-trichloropyridine and 2,3-dichloropyridine.
9. The preparation method according to claim 8, characterized in that: The acid binding agent is selected from one or more of inorganic bases, organic bases, phosphates or carboxylates.
10. The preparation method according to claim 9, characterized in that: The inorganic base is one or more of alkali metal carbonates, alkali metal bicarbonates, alkali metal oxides, alkaline earth metal carbonates, alkaline earth metal bicarbonates, alkaline earth metal oxides, alkaline earth metal hydroxides, ammonium carbonate or ammonium bicarbonate, preferably alkali metal carbonates, alkaline earth metal oxides, more preferably sodium carbonate or magnesium oxide, and most preferably magnesium oxide.
11. The preparation method according to claim 9, characterized in that: The organic base is selected from one or more of pyridine, alkylpyridine or organic amine.
12. The preparation method according to claim 9, characterized in that: The phosphate is selected from one or more of dihydrogen phosphate, hydrogen phosphate or orthophosphate.
13. The preparation method according to claim 9, characterized in that: The carboxylate is selected from one or more of formates, acetates, triacrylates and tetrasuccinates.
14. The preparation method according to claim 8, characterized in that: The molar ratio of the acid binding agent to 2,3,5,6-trichloropyridine is 0.5 to 2:
1.
15. The preparation method according to claim 8 or 9, characterized in that: The preparation method further comprises at least one of the following conditions: The mass ratio of the 2,3,5,6-tetrachloropyridine to the bimetallic catalyst is 1:0.001-1:0.01; The molar ratio of the acid binding agent to the 2,3,5,6-tetrachloropyridine is 0.2:1-3:1; The organic solvent is a benzene ring-containing compound, ester or alcohol, preferably C6-C 12 One or more of a benzene ring-containing compound, an alkane carboxylic acid alkane alcohol ester or a C1-C8 alcohol; The mass ratio of the organic solvent to the 2,3,5,6-tetrachloropyridine is 1:1-10:1; The pressure of the hydrogen is 0.1-3MPa; The reaction temperature is 20-100°C.
Citation Information
Patent Citations
Preparation method for 2,3-dichloropyridine
CN107056688A
Application of Pd-C nano-composite material to oxidative catalysis of organic matter
CN108554404A
Preparation method for 2,3-dichloropyridine
CN109280026A
Catalyst and uses in hydrodechlorination of 2,3,6-trichloropyridine
CN110961110A
Catalyst for synthesis of 2, 3-dichloropyridine and preparation method thereof
CN114192140A
Cited By
Dechlorination method of 2, 3, 5, 6-tetrachloropyridine
CN117820207A
Amber core synthesis catalyst, preparation method thereof and synthesis method of amber core
CN119158595A