Method for preparing iron phosphate by recycling waste

CN118790964APending Publication Date: 2024-10-18GUIZHOU PHOSPHATING NEW MATERIAL TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411050630.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

[0003]本发明的目的在于提供一种废料再利用制备磷酸铁的方法,以解决现有的磷酸铁废料处理方式造成原料极大浪费,导致生产电池级磷酸铁的投入成本升高的问题

Benefits of technology

[0003]本发明的目的在于提供一种废料再利用制备磷酸铁的方法,以解决现有的磷酸铁废料处理方式造成原料极大浪费,导致生产电池级磷酸铁的投入成本升高的问题。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118790964A_ABST
    Figure CN118790964A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of utilization of battery-grade iron phosphate waste materials, and particularly discloses a method for preparing iron phosphate by recycling waste materials. The method comprises the following nine steps: dissolving the anhydrous iron phosphate waste into a diluted sulfuric acid solution, filtering for the first time, calculating, adjusting the specific content of iron and phosphorus, adjusting the pH value, filtering for the second time, washing, curing, filtering for the third time, and calcining and crushing, so as to obtain the anhydrous iron phosphate with low impurity content and high specific surface area. According to the scheme, the material loss in the manufacturing process of the battery-grade iron phosphate is reduced, the great waste of raw materials is avoided, the input cost for producing the battery-grade iron phosphate is reduced, the unqualified iron phosphate waste is converted into the high-quality anhydrous iron phosphate at lower cost, and the average dissolution rate reaches 98% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of battery-grade iron phosphate waste utilization, and in particular to a method for preparing iron phosphate by recycling waste. Background Art

[0002] In order to ensure that the battery has a higher energy density and longer service life, and to improve the cycle stability and reliability of the battery, the current requirements for the impurity content of battery-grade iron phosphate are very high. In the production process of battery-grade iron phosphate, multiple links such as the raw material processing stage, the production reaction stage, the product post-processing stage, the detection and screening stage, etc. will produce waste materials with impurity content that does not meet the standards. For these waste materials with high impurity content, the existing treatment method is to directly stack them in the warehouse, resulting in a waste of floor space, or directly use them for phosphate fertilizer production. These treatment methods cause a great waste of raw materials for preparing battery-grade iron phosphate, resulting in a significant increase in the investment cost of producing battery-grade iron phosphate. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing iron phosphate by recycling waste materials, so as to solve the problem that the existing method of treating waste iron phosphate causes great waste of raw materials and leads to increased investment cost for producing battery-grade iron phosphate.

[0004] In order to solve the above problems, the technical solutions provided are as follows:

[0005] A method for preparing ferric phosphate by recycling waste materials comprises the following steps:

[0006] S1: Dissolving and first filtering: using dilute sulfuric acid to dissolve unqualified anhydrous iron phosphate waste, filtering out insoluble matter to obtain filter cake and filtrate;

[0007] S2: Calculation: Dry the filter cake in S1 at a temperature of 100-120°C, weigh the filter cake, and calculate the dissolution rate of the anhydrous ferric phosphate waste;

[0008] S3: Adjusting the iron-phosphorus ratio: adding phosphoric acid or refined ferrous sulfate to the filtrate in S1 to adjust the iron-phosphorus ratio in the solution to between 0.9 and 1;

[0009] S4: Adjusting pH: The pH of the filtrate is adjusted to between 1.9 and 2.1 with 8% ammonia water to obtain a reaction slurry;

[0010] S5: Second filtration: filtering the reaction slurry to obtain a filter cake and a filtrate;

[0011] S6: washing: washing the filter cake in step S5 with desalted water for multiple times until the conductivity is lower than 150 μs / cm;

[0012] S7: Ripening: After slurrying the washed filter cake with water, add 1% by mass phosphoric acid and ripen for 3 hours to obtain dihydrate iron phosphate slurry;

[0013] S8: third filtration: filtering the white ferric phosphate dihydrate slurry in step S7, and drying the filtered filter cake at a temperature of 90-100° C. to obtain ferric phosphate dihydrate;

[0014] S9: Calcination and crushing: Calcine and crush the dihydrate ferric phosphate to obtain anhydrous ferric phosphate with low impurity content.

[0015] The beneficial effects of the above technical scheme are: using sulfuric acid to dissolve iron phosphate waste and then reproducing anhydrous iron phosphate with low impurity content and high specific surface area, reducing material loss in the manufacturing process of battery-grade iron phosphate, avoiding huge waste of raw materials, and reducing the investment cost of producing battery-grade iron phosphate. This scheme converts unqualified iron phosphate waste into high-quality anhydrous iron phosphate at a relatively low cost, and the dissolution rate reaches an average of more than 98%.

[0016] Preferred solution 1: As a further optimization of the basic solution, in step S1, 55 parts of concentrated sulfuric acid are added to 700 parts of desalted water and stirred evenly to obtain a dilute sulfuric acid solution, and 100 parts of anhydrous iron phosphate waste are added to the diluted solution to dissolve.

[0017] Preferred solution 2: As a further optimization of preferred solution 1, in step S1, 65 parts of concentrated sulfuric acid are added to 700 parts of desalted water and stirred evenly to obtain a dilute sulfuric acid solution, and 100 parts of anhydrous iron phosphate waste are added to the diluted solution to dissolve.

[0018] Preferred solution three: As a further optimization of preferred solution two, in step S1, 85 parts of concentrated sulfuric acid are added to 700 parts of desalted water and stirred evenly to obtain a dilute sulfuric acid solution, and 100 parts of anhydrous iron phosphate waste are added to the diluted solution to dissolve.

[0019] Preferred solution 4: As a further optimization of preferred solution 3, in step S1, 95 parts of concentrated sulfuric acid are added to 700 parts of desalted water and stirred evenly to obtain a dilute sulfuric acid solution, and 100 parts of anhydrous iron phosphate waste are added to the diluted solution to dissolve.

[0020] Preferred solution five: As a further optimization of preferred solution four, in step S1, 180 parts of concentrated sulfuric acid are added to 2100 parts of desalted water and stirred evenly to obtain a dilute sulfuric acid solution, and 300 parts of anhydrous iron phosphate waste are added to the diluted solution to dissolve. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The figure is a flow chart of an embodiment of the present invention. DETAILED DESCRIPTION

[0022] The following is further described in detail through specific implementation methods:

[0023] The embodiment is basically as shown in the attached Figure 1 As shown:

[0024] Example 1

[0025] A method for preparing ferric phosphate by recycling waste materials comprises the following steps:

[0026] S1: Dissolve and filter for the first time: Take 50g of concentrated sulfuric acid and add it to 700g of desalted water and stir it to obtain a diluted solution. Take 100g of anhydrous iron phosphate waste and add it to the diluted solution to dissolve. Dissolve for 30 minutes. After no obvious white material is seen in the system, continue to dissolve for 20 minutes, filter, and obtain a filter cake and a filtrate. The filter cake is an insoluble impurity, and the filtrate is an iron-phosphorus mixed solution with a low content of metal impurities;

[0027] S2: Calculation: Dry the filter cake in S1 at 110°C, weigh the filter cake, and calculate the dissolution rate of the anhydrous ferric phosphate waste;

[0028] S3: Adjusting the iron-phosphorus ratio: adding phosphoric acid or refined ferrous sulfate (refined ferrous sulfate is obtained by removing impurities from ferrous sulfate heptahydrate, a byproduct of titanium dioxide) to the filtrate in S1 to adjust the iron-phosphorus ratio in the solution to between 0.9 and 1;

[0029] S4: Adjusting pH: The pH of the filtrate is adjusted to between 1.95 with 8% ammonia water to obtain a reaction slurry;

[0030] S5: Second filtration: filtering the reaction slurry to obtain a filter cake and a filtrate;

[0031] S6: washing: washing the filter cake in step S5 with desalted water for multiple times until the conductivity is lower than 150 μs / cm;

[0032] S7: Ripening: After the washed filter cake is slurried with water, 1% by mass phosphoric acid is added and ripened for 3 hours to obtain a white iron phosphate dihydrate slurry;

[0033] S8: third filtration: filtering the white ferric phosphate dihydrate slurry in step S7, and drying the filtered filter cake at a temperature of 92° C. to obtain ferric phosphate dihydrate;

[0034] S9: Calcination and crushing: Calcine and crush the dihydrate ferric phosphate to obtain anhydrous ferric phosphate with low impurity content.

[0035] Example 2

[0036] The difference between Example 2 and Example 1 is that in step S1, 55 g of concentrated sulfuric acid is added to 700 g of desalted water and stirred evenly to obtain a diluted solution, and 100 g of anhydrous iron phosphate waste is added to the diluted solution to dissolve.

[0037] Example 3

[0038] The difference between Example 3 and Example 1 is that: in step S1, 65 g of concentrated sulfuric acid is added to 700 g of desalted water and stirred evenly to obtain a diluted solution, and 100 g of anhydrous iron phosphate waste is added to the diluted solution to dissolve.

[0039] Example 4

[0040] The difference between Example 4 and Example 1 is that in step S1, 85 g of concentrated sulfuric acid is added to 700 g of desalted water and stirred evenly to obtain a diluted solution, and 100 g of anhydrous iron phosphate waste is added to the diluted solution to dissolve.

[0041] Example 5

[0042] The difference between Example 5 and Example 1 is that in step S1, 95 g of concentrated sulfuric acid is added to 700 g of desalted water and stirred evenly to obtain a diluted solution, and 100 g of anhydrous iron phosphate waste is added to the diluted solution to dissolve.

[0043] Example 6

[0044] The difference between Example 6 and Example 1 is that in step S1, 180 g of concentrated sulfuric acid is added to 2100 g of desalted water and stirred evenly to obtain a diluted solution, and 300 g of anhydrous iron phosphate waste is added to the diluted solution to dissolve.

[0045] The dissolution rates of anhydrous iron phosphate waste calculated in Examples 1-6 are shown in Table 1 below;

[0046] Table 1 Dissolution rate of anhydrous iron phosphate waste

[0047]

[0048] It can be seen from the data in Table 1 above that, except for Example 1, the dissolution rate of the anhydrous ferric phosphate waste material is above 98% on average, and the highest dissolution rate is 98.86% in Example 5. It can be seen that the recovery rate of the anhydrous ferric phosphate waste material is as high as above 98%.

[0049] The contents of various elements in the anhydrous ferric phosphate prepared in Examples 1-6 were calculated by spectral analysis and are shown in Table 2 below;

[0050] Table 2 Content of each element in anhydrous ferric phosphate

[0051]

[0052]

[0053] From the data of the content of each element in the anhydrous iron phosphate in Table 2 above, it can be seen that the impurity S element in the anhydrous iron phosphate after being treated by Examples 1-6 is greatly reduced, the impurity Mg, Na, K, Ca, Cd, and Cu elements are almost removed, and the content of the remaining impurity elements is also reduced. The anhydrous iron phosphate with low impurity content and high specific surface area successfully converts the iron phosphate waste with unqualified impurity content into high-quality anhydrous iron phosphate. Reduce material loss in the manufacturing process of battery-grade iron phosphate, avoid causing great waste of raw materials, and reduce the investment cost of producing battery-grade iron phosphate.

[0054] The above is only an embodiment of the present invention, and the common knowledge such as the known specific structure and characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, several deformations and improvements can be made without departing from the structure of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A method for preparing ferric phosphate by recycling waste materials, characterized in that: The following steps are involved: S1: Dissolving and first filtering: using dilute sulfuric acid to dissolve unqualified anhydrous iron phosphate waste, filtering out insoluble matter to obtain filter cake and filtrate; S2: Calculation: Dry the filter cake in S1 at a temperature of 100-120°C, weigh the filter cake, and calculate the dissolution rate of the anhydrous ferric phosphate waste; S3: Adjusting the iron-phosphorus ratio: adding phosphoric acid or refined ferrous sulfate to the filtrate in S1 to adjust the iron-phosphorus ratio in the solution to between 0.9 and 1; S4: Adjusting pH: The pH of the filtrate is adjusted to between 1.9 and 2.1 with 8% ammonia water to obtain a reaction slurry; S5: Second filtration: filtering the reaction slurry to obtain a filter cake and a filtrate; S6: washing: washing the filter cake in step S5 with desalted water for multiple times until the conductivity is lower than 150 μs / cm; S7: Ripening: After slurrying the washed filter cake with water, add 1% by mass phosphoric acid and ripen for 3 hours to obtain dihydrate iron phosphate slurry; S8: third filtration: filtering the white ferric phosphate dihydrate slurry in step S7, and drying the filtered filter cake at a temperature of 90-100° C. to obtain ferric phosphate dihydrate; S9: Calcination and crushing: Calcine and crush the dihydrate ferric phosphate to obtain anhydrous ferric phosphate with low impurity content.

2. The method for preparing ferric phosphate by recycling waste materials according to claim 1, characterized in that: In the step S1, 55 parts of concentrated sulfuric acid are added into 700 parts of desalted water and stirred to obtain a dilute sulfuric acid solution, and 100 parts of anhydrous iron phosphate waste are added into the diluted solution to dissolve.

3. The method for preparing ferric phosphate by recycling waste materials according to claim 1, characterized in that: In the step S1, 65 parts of concentrated sulfuric acid are added into 700 parts of desalted water and stirred evenly to obtain a diluted solution, and 100 parts of anhydrous iron phosphate waste are added into the diluted solution to dissolve.

4. The method for preparing ferric phosphate by recycling waste materials according to claim 1, characterized in that: In step S1, 85 parts of concentrated sulfuric acid are added into 700 parts of desalted water and stirred evenly to obtain a diluted solution, and 100 parts of anhydrous iron phosphate waste are added into the diluted solution to dissolve.

5. The method for preparing ferric phosphate by recycling waste materials according to claim 1, characterized in that: In the step S1, 95 parts of concentrated sulfuric acid are added into 700 parts of desalted water and stirred evenly to obtain a diluted solution, and 100 parts of anhydrous iron phosphate waste are added into the diluted solution to dissolve.

6. The method for preparing ferric phosphate by recycling waste materials according to claim 1, characterized in that: In the step S1, 180 parts of concentrated sulfuric acid are added into 2100 parts of desalted water and stirred to obtain a diluted solution, and 300 parts of anhydrous iron phosphate waste are added into the diluted solution to dissolve.

Citation Information

Patent Citations

  • Method for regenerating iron phosphate waste

    CN110683528A