Tetrahedral-site-doped cobalt-free lithium-rich manganese-based oxide positive electrode material and preparation method and application thereof
By introducing boron ions into the cobalt-free lithium-rich manganese-based oxide cathode material to form a tetrahedral doping structure, the problem of poor lattice oxygen stability of the material under high pressure is solved, the cycle stability and capacity retention rate of the battery are improved, and It reduces production costs and has commercial application prospects.
Patent Information
- Application Number
- CN202410956663.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-18
AI Technical Summary
Existing lithium-rich manganese-based oxide cathode materials have poor lattice oxygen stability under high pressure, resulting in irreversible oxygen release and unstable material structure, affecting battery cycle life and capacity retention, and industrial preparation methods lead to uneven particle size distribution and inconsistent performance. good.
Through high-temperature calcination by the molten salt method, boron ions are introduced into the cobalt-free lithium-rich layered oxide cathode material to form a tetrahedral site doping structure, forming a strong B-O bond, improving the redox stability of oxygen ions, and through simple processing Stable tetrahedral site-doped cobalt-free lithium-rich manganese-based oxide cathode materials are prepared through steps and easily controllable conditions.
It significantly improves the material's cycle stability and capacity retention rate, ensuring the long-term stability of the battery in high-capacity cycles, and does not contain precious metal cobalt. It has the advantages of low cost and environmental friendliness, and has great commercial prospects.
Smart Images

Figure CN118791008A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium-ion batteries, and more specifically, relates to a tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material and a preparation method and application thereof. Background Art
[0002] With the continuous updating of electronic products and the continuous development of electric vehicles, lithium-ion batteries need better comprehensive performance, such as higher energy density, better safety performance, lower cost and environmental friendliness. However, the specific capacity of current commercial cathode materials such as lithium iron phosphate (LFP), lithium cobalt oxide (LCO) and ternary nickel cobalt manganese oxide (NCM) is generally not as good as that of the negative electrode. This is one of the main reasons why the capacity of lithium-ion batteries has been difficult to increase, and it obviously cannot meet the development needs. Lithium-rich manganese-based oxide cathode materials have excellent specific capacity (greater than 250mAh g -1 ) is expected to solve this problem. However, an important defect of the current lithium-rich manganese-based oxide positive electrode materials is the poor stability of lattice oxygen under high pressure. The lattice oxygen will be over-oxidized and cause irreversible oxygen release, resulting in an unstable material structure, which ultimately affects the battery cycle life and leads to a serious disadvantage of low capacity retention rate. In addition, the current industrial preparation method for lithium-rich manganese-based oxide positive electrode materials is mainly a high-temperature solid-phase method, but the material produced by this method has an uneven particle size distribution, and is mostly impure phase with irregular morphology, which affects the quality of the material and the stability of its performance, resulting in poor electrochemical performance. It can be seen that the defects of the material itself and the synthesis method have seriously hindered the commercialization of lithium-rich manganese-based oxide positive electrode materials. Summary of the invention
[0003] In order to solve the deficiencies and shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a method for preparing a tetrahedral doped cobalt-free lithium-rich oxide positive electrode material. The method mainly uses a molten salt method for high-temperature calcination, introduces boron ions in the tetrahedral position of the cobalt-free lithium-rich layered oxide positive electrode material for structural fine-tuning, and the incorporated boron ions can introduce new electronic states in the crystal, provide additional electrons for the nearest neighbor oxygen atoms, form a strong BO bond, effectively prevent excessive oxidation of oxygen anions, and increase the redox stability of oxygen ions, which makes the material structure more stable and ensures that the battery can be cycled for a long time with high capacity. The preparation method overcomes the shortcomings of fast capacity decay and poor cycle stability of cobalt-free lithium-rich layered oxide positive electrode materials, and the processing steps are simple, the conditions are easy to control, and the repeatability is good. At the same time, the material does not contain precious metal cobalt elements, has low cost of ownership, has environmentally friendly advantages, and has great commercial prospects.
[0004] Another object of the present invention is to provide a tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material prepared by the above method.
[0005] Another object of the present invention is to provide an application of the above-mentioned tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material.
[0006] The purpose of the present invention is achieved through the following technical solutions:
[0007] A method for preparing a tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material comprises the following specific steps:
[0008] S1. The transition metal precursor, lithium salt, sodium salt, potassium salt and boron compound are mixed, heated to 800-1000°C for heat treatment, cooled with the furnace, washed, impurities filtered, dried at 150-200°C, and ground to obtain a powder;
[0009] S2. The powder is heated to 200-500° C. and sintered to obtain a tetrahedral boron-doped cobalt-free lithium-rich manganese-based oxide positive electrode material, wherein the chemical formula of the cobalt-free lithium-rich oxide positive electrode material is Li 1.2 Mn 0.6 Ni 0.2 B x O2,0 <x≤0.02。
[0010] Preferably, the transition metal precursor in step S1 is a transition metal carbonate precursor or a transition metal hydroxide precursor.
[0011] More preferably, the transition metal carbonate precursor is TMCO3; the transition metal hydroxide precursor is TM(OH)2, TM=Mn or Ni.
[0012] Preferably, in step S1, the lithium salt is one or more of lithium carbonate, lithium hydroxide, lithium nitrate or lithium acetate; the sodium salt is sodium chloride, and the potassium salt is potassium chloride; and the boron compound is boric acid, sodium borate or ammonium borate.
[0013] Preferably, in step S1, the molar ratio of the transition metal ions in the transition metal precursor to the lithium ions in the lithium salt is 1:(1.2-1.6), the total molar ratio of the sodium ions and potassium ions in the sodium salt and potassium salt to the transition metal ions in the transition metal precursor and the lithium ions in the lithium salt is (3-5):1, and the molar ratio of the boron ions in the boron compound to the transition metal ions in the transition metal precursor is (0.1-2.5):100.
[0014] Preferably, the heating rate in step S1 is 1-4°C / min, the heat treatment time is 8-20h; and the drying time is 6-12h.
[0015] Preferably, the sintering temperature rise rate in step S2 is 3-5° C. / min, and the sintering time is 3-5 h.
[0016] A tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material is prepared by the above method.
[0017] The application of the tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material in the field of lithium-ion batteries.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1. The method of tetrahedral doping modification of the cobalt-free lithium-rich manganese-based oxide positive electrode material of the present invention using a boron-containing compound overcomes the shortcomings of fast capacity decay and poor cycle stability of the cobalt-free lithium-rich layered oxide positive electrode material, and has simple processing steps, easy controllable conditions, good repeatability, and at the same time, the material does not contain precious metal cobalt, has low cost of ownership, has environmentally friendly advantages, and has great commercial prospects.
[0020] 2. The main phase of the tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material of the present invention is to use boron-containing compounds to fine-tune the structure of the cobalt-free lithium-rich manganese-based oxide positive electrode material, successfully introduce boron ions into the crystal structure, provide additional electrons for the nearest neighbor oxygen atoms, form a strong BO bond, effectively prevent excessive oxidation of oxygen anions, and increase the redox stability of oxygen ions, which makes the material structure more stable and ensures that the battery can be cycled for a long time with high capacity.
[0021] 3. The tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material of the present invention overcomes the shortcomings of the previous materials such as short cycle life and fast capacity decay. When the voltage window is 2.0-4.8V and the current density is 200mAg -1 The discharge capacity of this type of cathode material is up to 232.31 mAh g -1 After 300 cycles, the discharge capacity is still as high as 210.66 mAh g -1 The retention rate reaches more than 80%, and the highest capacity retention rate is 90.7%. The introduction of B ions greatly improves the cycle stability of cobalt-free lithium-rich manganese-based oxide positive electrode materials and can be used in the field of lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 is Li in Example 1 1.2 Mn 0.6 Ni 0.2 B 0.004 X-ray diffraction pattern of O2 powder.
[0023] Figure 2 is Li in Example 1 1.2 Mn 0.6 Ni 0.2 B0.004 SEM photo of O2 powder.
[0024] Figure 3 is Li of Example 1 1.2 Mn 0.6 Ni 0.2 B 0.004 XPS graph of boron element in O2 powder.
[0025] Figure 4 Li for Application Example 1 1.2 Mn 0.6 Ni 0.2 B 0.004 When O2 powder is used as positive electrode, the current is 20mA g -1 The first charge and discharge curve at .
[0026] Figure 5 Li for Application Example 1 1.2 Mn 0.6 Ni 0.2 B 0.004 O2 powder as positive electrode at room temperature 200mA g -1 Capacity stability curve.
[0027] Figure 6 For Li in Application Example 2 1.2 Mn 0.6 Ni 0.2 B 0.02 O2 powder as positive electrode at room temperature 20mAg -1 The first charge and discharge curve at .
[0028] Figure 7 For Li in Application Example 2 1.2 Mn 0.6 Ni 0.2 B 0.02 O2 powder as positive electrode at room temperature 200mAg -1 Capacity stability curve.
[0029] Figure 8 For Li in Application Example 3 1.2 Mn 0.6 Ni 0.2 B 0.0008 O2 powder as positive electrode at room temperature 20mA g -1 The first charge and discharge curve at .
[0030] Fig. 9 For Li in Application Example 3 1.2 Mn 0.6 Ni 0.2 B 0.0008 O2 powder as positive electrode at room temperature 200mA g -1Capacity stability curve. DETAILED DESCRIPTION
[0031] The content of the present invention is further described below in conjunction with specific examples, but it should not be construed as limiting the present invention. If not specifically indicated, the technical means used in the examples are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0032] Example 1
[0033] 1. Weigh 1g of transition metal carbonate precursor (Mn 0.75 Ni 0.25 CO3), 0.5022g lithium salt (Li2CO3), 0.0022g sodium borate (B4Na2O7), 3.8602g potassium salt (KCl) and 2.0174g sodium salt (NaCl), grind them thoroughly and put them into a crucible; place them in a box-type muffle furnace at 850℃ for 12h, cool them with the furnace, wash and filter them to obtain block material A;
[0034] 2. Dry the bulk material A in a box-type blast oven at 180°C for 8 hours, and grind it to obtain powder B;
[0035] 3. Powder B was placed in a crucible and placed in a box-type muffle furnace at 400°C for 3 hours, cooled with the furnace, and ground again to obtain Li 1.2 Mn 0.6 Ni 0.2 B 0.004 O2 powder is a tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material.
[0036] Figure 1 In this embodiment, Li 1.2 Mn 0.6 Ni 0.2 B 0.004 X-ray diffraction pattern of O2 powder. Figure 1 It can be seen that Li 1.2 Mn 0.6 Ni 0.2 B 0.004 O2 powder has a typical O3-type lithium-rich oxide spatial structure and is a mixed phase of Li2MnO3 and ternary layered materials. Figure 2 In this embodiment, Li 1.2 Mn 0.6 Ni 0.2 B 0.004 SEM photo of O2 powder. Figure 2 It can be seen that Li 1.2 Mn 0.6 Ni 0.2 B 0.004O2 powder is assembled micron spheres. Figure 3 For the Li of Example 1 1.2 Mn 0.6 Ni 0.2 B 0.004 XPS graph of boron in O2 powder. Figure 3 It can be seen that element B has been successfully incorporated into the crystal structure of the material.
[0037] Application Example 1
[0038] The button cell was used for testing. The Li 1.2 Mn 0.6 Ni 0.2 B 0.004 O2 powder, conductive carbon black (Super P), and binder polyvinylidene fluoride (PVDF) were uniformly mixed in a mass ratio of 8:1:1 and coated on aluminum foil. Finally, the electrodes were cut into circular electrodes with a diameter of 14 mm. The metal lithium sheet was used as the counter electrode. 1 mol·L -1 LiPF6 / EC+EMC (EC:EMC volume ratio 3:7) is used as electrolyte, polypropylene material is used as separator, battery test system is Xinwei, charge and discharge voltage window is 2.0~4.8V, charge and discharge current density is 20mAg -1 , 200mAg -1 , the material exhibits good electrochemical performance when used as the positive electrode of lithium-ion batteries. Figure 4 Li in Application Example 1 1.2 Mn 0.6 Ni 0.2 B 0.004 O2 powder as positive electrode at room temperature 20mAg -1 The first charge and discharge curve at . Figure 4 It can be seen that at 20mAg -1 The first discharge capacity at the charge and discharge current density is 285.8 mAh g -1 . Figure 5 Li in Application Example 1 1.2 Mn 0.6 Ni 0.2 B 0.004 O2 powder as positive electrode at room temperature 200mA g -1 The capacity stability curve shows that the discharge capacity can reach 232.31 mAh g -1 After 300 cycles, the discharge capacity is still as high as 210.66 mAh g -1 The capacity retention rate is 90.7%, indicating that the introduction of B ions can greatly improve the cycle stability of cobalt-free lithium-rich manganese-based oxide positive electrode materials.
[0039] Example 2
[0040] The difference between Example 1 and Example 1 is that the mass of sodium borate in step 1 is 0.0108 g, and Li 1.2 Mn 0.6 Ni 0.2 B 0.02 O2 powder is a tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material.
[0041] Application Example 2
[0042] The electrode in this application example is the Li 1.2 Mn 0.6 Ni 0.2 B 0.02 Made from O2 powder. Figure 6 For Li in Application Example 2 1.2 Mn 0.6 Ni 0.2 B 0.02 O2 powder as positive electrode at room temperature 20mA g -1 The first charge and discharge curve at . Figure 6 It can be seen that at 20mAg -1 The first discharge capacity is 271.27 mAh g -1 . Figure 7 For Li in Application Example 2 1.2 Mn 0.6 Ni 0.2 B 0.02 O2 powder as positive electrode at room temperature 200mA g -1 The capacity stability curve shows that the maximum discharge capacity is 191.82 mAh g -1 After 300 cycles, the capacity retention rate was 80.9%, indicating that this doping amount can still improve the cycle stability of the material, but this is at the expense of capacity.
[0043] Example 3
[0044] The difference between Example 1 and Example 1 is that the mass of sodium borate in step 1 is 0.0004 g, and Li 1.2 Mn 0.6 Ni 0.2 B 0.0008 O2 powder is a tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material.
[0045] Application Example 3
[0046] The pole piece in this application example is the Li 1.2 Mn 0.6 Ni 0.2 B 0.0008 Made from O2 powder. Figure 8 For Li in Application Example 3 1.2Mn 0.6 Ni 0.2 B 0.0008 O2 powder as positive electrode at room temperature 20mAg -1 The first charge and discharge curve at . Figure 8 It can be seen that at 20mAg -1 The first discharge capacity at the charge and discharge current density is 297.96 mAh g -1 . Fig. 9 For Li in Application Example 3 1.2 Mn 0.6 Ni 0.2 B 0.0008 O2 powder as positive electrode at room temperature 200mA g -1 The capacity stability curve shows that the maximum discharge capacity is 247.99 mAh g -1 After 100 cycles, the capacity retention rate was 75.5%, indicating that the doping amount was not sufficient to bring good results.
[0047] It can be seen that the tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material of the present invention has a voltage window of 2.0-4.8V and a current density of 200mAg -1 The discharge capacity is up to 232.31 mAh g -1 After 300 cycles, the capacity is still as high as 210.66 mAh g -1 The retention rate reaches more than 80%, and the highest capacity retention rate is 90.7%. The introduction of B ions greatly improves the cycle stability of cobalt-free lithium-rich manganese-based oxide positive electrode materials, overcoming the shortcomings of previous materials such as short cycle life and fast capacity decay, and can be used in the field of lithium-ion batteries.
[0048] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material, characterized in that: The specific steps include: S1. The transition metal precursor, lithium salt, sodium salt, potassium salt and boron compound are mixed, heated to 800-1000°C for heat treatment, cooled with the furnace, washed, impurities filtered, dried at 150-200°C, and ground to obtain a powder; S2. The powder is heated to 200-500° C. and sintered to obtain a tetrahedral boron-doped cobalt-free lithium-rich manganese-based oxide positive electrode material, wherein the chemical formula of the cobalt-free lithium-rich oxide positive electrode material is Li 1.2 Mn 0.6 Ni 0.2 B x O2,0 <x≤0.02。 2. The method for preparing the tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material according to claim 1, characterized in that: The transition metal precursor in step S1 is a transition metal carbonate precursor or a transition metal hydroxide precursor.
3. The method for preparing the tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material according to claim 2, characterized in that: The transition metal carbonate precursor is TMCO3; the transition metal hydroxide precursor is TM(OH)2, TM=Mn or Ni.
4. The method for preparing the tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material according to claim 1, characterized in that: In step S1, the lithium salt is one or more of lithium carbonate, lithium hydroxide, lithium nitrate or lithium acetate; the sodium salt is sodium chloride, and the potassium salt is potassium chloride; the boron compound is boric acid, sodium borate or ammonium borate.
5. The method for preparing the tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material according to claim 1, characterized in that: In step S1, the molar ratio of the transition metal ions in the transition metal precursor to the lithium ions in the lithium salt is 1:(1.2-1.6), the total molar ratio of the sodium ions and potassium ions in the sodium salt and potassium salt to the transition metal ions in the transition metal precursor and the lithium ions in the lithium salt is (3-5):1, and the molar ratio of the boron ions in the boron compound to the transition metal ions in the transition metal precursor is (0.1-2.5):
100.
6. The method for preparing the tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material according to claim 1, characterized in that: In step S1, the heating rate is 1-4°C / min, the heat treatment time is 8-20h, and the drying time is 6-12h.
7. The method for preparing the tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material according to claim 1, characterized in that: The sintering temperature rise rate in step S2 is 3-5°C / min, and the sintering time is 3-5h.
8. A tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material, characterized in that: The cobalt-free lithium-rich manganese-based oxide positive electrode material is prepared by the method according to any one of claims 1-7.
9. Application of the tetrahedral doped cobalt-free lithium-rich manganese-based oxide positive electrode material according to claim 8 in the field of lithium-ion batteries.
Citation Information
Patent Citations
Surface layer gradient doped lithium-rich layered oxide positive electrode material as well as preparation method and application thereof
CN111326730A
Tantalum and zirconium co-doped cobalt-free single crystal lithium-rich manganese-based positive electrode material and preparation method thereof
CN116623295A
Surface modified cobalt-free lithium-rich oxide positive electrode material as well as preparation method and application thereof
CN117976897A