Modified polyurethane, preparation method thereof and application of modified polyurethane as meniscus substitute material
Through modified polyurethane materials and 3D printing technology, the problems of the lubrication mechanism and cartilage wear of meniscal substitutes in the body have been solved, and a meniscus substitute with high hydrophilicity and excellent mechanical properties has been achieved, slowing down the progression of osteoarthritis.
Patent Information
- Application Number
- CN202310381628.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-04-11
AI Technical Summary
Existing meniscal substitutes are difficult to simulate the lubrication mechanism in the body, resulting in cartilage wear problems during long-term implantation, and shape mismatch and load transfer disorder after transplantation exacerbate the progression of osteoarthritis.
Using modified polyurethane materials, through the introduction of zwitterionic and hydrogen bonding structural design, combined with 3D printing technology, meniscal substitutes with high hydrophilicity and excellent mechanical properties are prepared to achieve shape matching and lubricated surfaces to reduce cartilage wear.
The meniscus substitute implanted in the body has good lubrication and mechanical properties, reduces cartilage wear, delays the progression of osteoarthritis, and has a simple preparation process and is suitable for personalized customization.
Smart Images

Figure CN118791697A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of biomedical materials, and more specifically to the preparation of modified polyurethane and its application in 3D printing as a meniscus substitute material. Background Art
[0002] Due to its unique vascularization characteristics, the self-repair ability of the meniscus is limited. So far, meniscectomy is still the most commonly used method for clinical treatment of severe meniscus injuries. However, removal of the meniscus may lead to stress concentration and load transfer disorder in the knee joint, thereby accelerating the progression of osteoarthritis (OA), while allogeneic meniscus transplantation has problems such as insufficient graft source, immune rejection and risk of disease transmission. Therefore, there is an urgent need to develop an artificial meniscus substitute to reconstruct the function of the meniscus, reduce cartilage wear, and avoid the development of osteoarthritis after meniscectomy.
[0003] Polyurethane is a well-recognized biomedical material that has been widely used as a replacement for internal human tissues and organs due to its high degree of freedom in molecular design. Among various polyurethanes, polycarbonate polyurethanes show excellent resistance to oxidative degradation and hydrolytic stability, and are expected to be used as meniscus substitutes for long-term implantation. Generally, polyurethanes have low hydrophilicity, which can cause problems with cartilage wear when used as implants. Some studies have confirmed that the introduction of zwitterions into polyurethane systems can significantly improve the hydrophilicity and lubricity of polyurethanes.
[0004] Emerging 3D printing technologies, such as fused deposition modeling (FDM), are expected to achieve precise printing with high shape fidelity, which can effectively solve the microstructural design and personalized customization of meniscus, thereby reducing problems such as shape mismatch and load transfer that may occur after transplantation. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and solve the problem that the current meniscus substitutes are difficult to simulate the lubrication mechanism in the body and face the problem of cartilage wear during long-term implantation. A modified polyurethane and a method for preparing a 3D printed meniscus are proposed, which have a simple formula and an easy preparation method.
[0006] The technical purpose of the present invention is achieved through the following technical solutions.
[0007] A modified polyurethane and a preparation method thereof are carried out according to the following steps:
[0008] Step 1, uniformly dispersing zwitterionic diol, polyhexamethylene carbonate diol, and diisocyanate in an organic solvent, adding a catalyst for prepolymerization, wherein the mass ratio of polyhexamethylene carbonate diol, zwitterionic diol, and diisocyanate is 1:(0.1-0.3):(0.5-0.8), the prepolymerization temperature is 70-90 degrees Celsius, and the time is 1-3 hours;
[0009] In step 1, the mass ratio of polyhexamethylene carbonate diol, zwitterionic diol and diisocyanate is 1:(0.1-0.2):(0.5-0.6).
[0010] In step 1, the diisocyanate is a hexamethylene diisocyanate hard segment.
[0011] In step 1, the number average molecular weight of polyhexamethylene carbonate diol is 1k-3k.
[0012] In step 1, the molecular formula of the zwitterionic diol is shown below
[0013] The preparation was carried out as follows: N-methyldiethanolamine (5.96 g, 50 mmol), 1,3-propane sultone (6.70 g, 55 mmol) and dichloromethane (200 mL) were added to a 500 mL round-bottom flask. The mixture was stirred in an oil bath at 40 ° C for 24 hours at 400 rpm under a nitrogen atmosphere. The reactant solution was rotated to about 25 mL using a rotary evaporator. The remaining solution was precipitated with acetone at a ratio of 1:20 and then washed three times with acetone to obtain a white powder. Finally, the product was dried in a vacuum oven and weighed; Reference: Liu Q, Wang X, Chiu A, et al. Azwitterionic polyurethane nanoporous device with low foreign-body response for islet encapsulation [J]. Advanced Materials, 2021, 33 (39): 2102852.
[0014] In step 1, polyhexamethylene carbonate diol (solid) and zwitterionic diol (solid) are added to a three-necked flask, a mechanical stirring device is assembled, and the interface is simply sealed with plastic wrap and then placed in a 120°C oil bath for vacuum drying for 1 hour to remove moisture from the raw materials and avoid violent polymerization during the prepolymerization stage.
[0015] In step 1, the catalyst is a commonly used catalyst in the polyurethane field, such as stannous 2-ethylhexanoate, and its amount is adjusted according to the amount of the reactants and is evenly added dropwise.
[0016] In step 1, the organic solvent is a commonly used reaction solvent in the polyurethane field, and the type and / or amount thereof is adjusted according to the amount of reactants, such as dimethyl sulfoxide, dimethylformamide or dimethylacetamide.
[0017] In step 1, the prepolymerization temperature is 70-80 degrees Celsius and the time is 1-2 hours.
[0018] Step 2, after prepolymerization, the temperature of the reaction system is lowered to 40-50 degrees Celsius, a chain extender adipic acid dihydrazide (ADH) is added dropwise to the reaction system and the reaction is carried out at a temperature of 1: (0.3-0.5) during the entire reaction process starting from the prepolymerization.
[0019] In step 2, the same solvent as in step 1 is selected to evenly disperse the chain extender adipic acid dihydrazide, and then added dropwise to the reaction system in batches to carry out a chain extension reaction (the amount added in each batch is substantially equal), during which the "pole climbing" phenomenon is observed.
[0020] In step 2, the inert protective atmosphere is nitrogen, helium or argon.
[0021] In step 2, the reaction temperature is 40-50 degrees Celsius and the reaction time is 6-12 hours.
[0022] In step 2, the mass ratio of polyhexamethylene carbonate diol to adipic acid dihydrazide is 1:(0.3-0.4).
[0023] In step 2, after the reaction is completed, the reactants are added to ether at a volume ratio of 1:20 for precipitation, the solid product obtained by precipitation is filtered, and washed three times with ether and pure water in sequence, and then placed in a vacuum drying oven for drying, and finally a dry white product is obtained, which is the modified polyurethane of the present invention, and is named PCU-MeSB.
[0024] The modified polyurethane of the present invention is used as a meniscus substitute material. The modified polyurethane is 3D printed by a biological 3D printer, and the prepared modified polyurethane (PCU-MeSB) material is added to the high-temperature barrel of the printer, and the temperature is raised to 180-220°C, and the temperature is kept for a period of time, such as 10-20 minutes, and the printing parameters are set to perform continuous printing. The extruded microfibers are deposited on a printing platform at 35-45°C; after the printing is completed, the printed product is immersed in a PBS buffer solution until the swelling equilibrium is reached to obtain a 3D printed PCU-MeSB scaffold with a specific shape.
[0025] In the technical solution of the present invention, the printing mode is a linear filling mode, the printing speed is 6-10 mm / s, and the wire output speed is 0.05-0.15 mm / s.
[0026] In the technical solution of the present invention, CAD / CAM software is used to design a 3D printing model, the rabbit meniscus model is obtained by reconstructing Micro-CT data, and the design system architecture is constructed by a layer-by-layer stacking method.
[0027] The present invention starts with the design of hydrogen bond structure, and adopts the combination of polyhexamethylene carbonate diol soft segment, hexamethylene diisocyanate hard segment and adipic acid dihydrazide chain extender to obtain supramolecular polyurethane (PCU) with high symmetry and high rigidity to ensure sufficient structural support in the subsequent printing process. On this basis, zwitterionic diol (MeSB-diol) was synthesized and introduced into the polyurethane system to synthesize zwitterionic polyurethane (PCU-MeSB). On the one hand, the introduced zwitterionic side groups will help to regulate the intermolecular hydrogen bonding interaction and the movement of the polymer chain in the hard segment, so that it has appropriate processing temperature, printability and toughness; on the other hand, the hydration of zwitterionic groups can improve the hydrophilicity of PCU and provide a lubricating surface. Through FDM 3D printing technology, PCU-MeSB meniscus substitutes with specific properties can be easily and directly prepared without any other post-processing (such as coating and filling with hydrogel). The invention has a simple formula and an easy preparation method. Appropriate soft and hard segments and chain extenders are selected to construct a polyurethane framework with excellent mechanical properties. On this basis, a zwitterionic chain extender is synthesized and introduced to improve its hydrophilicity and biocompatibility to solve the problem of cartilage wear caused by high-rigidity polyurethane. The modified polyurethane is added to the high-temperature barrel of the 3D printer, heated to 180-220°C for fused deposition molding 3D printing, and a 3D printed meniscus scaffold is obtained; the 3D printed meniscus scaffold is placed in a phosphate buffered saline solution and soaked until swelling equilibrium is obtained to obtain a 3D printed meniscus substitute for in vivo implantation. The method can achieve excellent mechanical properties through hydrogen bond structure design, introduce zwitterionic chain extenders to alleviate cartilage wear problems, and 3D print to obtain a size-matched meniscus scaffold, which has great application prospects as a meniscus substitute. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is the synthesis route of the present invention, wherein a is the synthesis route of zwitterionic diol MeSB-diol, and b is the synthesis route of PCU and PCU-MeSB polyurethane.
[0029] Figure 2These are photos of 3D printed PCU and PCU-MeSB in the present invention, where a is a photo of a single filament and b is a display of PCU-MeSB multi-layer square grids, meniscus, cylinders, and snowflake shapes.
[0030] Figure 3 3D printed structures of PCU and PCU-MeSB in the present invention are tensile stress-strain curves.
[0031] Figure 4 It is a bar chart of the test results of the mechanical properties Young's modulus, tensile strength, elongation at break and toughness corresponding to the PCU-MeSB of the 3D printed structure in the present invention.
[0032] Figure 5 It is a 1000-cycle tensile loading-unloading curve diagram of the PCU-MeSB of the 3D printed structure in the present invention.
[0033] Figure 6 It is the final stress and dissipated energy curve of the PCU-MeSB of the 3D printed structure in the present invention corresponding to the first and every 100 cycles of tensile loading-unloading.
[0034] Figure 7 It is a 1000-cycle compression loading-unloading curve diagram of the PCU-MeSB of the 3D printed structure in the present invention.
[0035] Figure 8 It is the final stress and dissipated energy curve of the PCU-MeSB of the 3D printed structure in the present invention corresponding to the first and every 100 cycles of compression loading-unloading.
[0036] Fig. 9 It is a bar graph of the tear energy test results of PCU and PCU-MeSB of the 3D printed structure in the present invention.
[0037] Fig.10 It is a friction coefficient test curve diagram of PCU and PCU-MeSB of the 3D printed structure in the present invention.
[0038] Fig.11 The 3D printed meniscus substitute of the present invention is implanted in the rabbit model and the gross observation diagram, wherein a is the implantation process of the 3D printed meniscus substitute in the rabbit model in the animal experiment, (i) is the incision of skin tissue and fascia tissue, (ii) is the cutting of the medial collateral ligament and the opening of the knee joint capsule, (iii) is the meniscectomy, (iv) is the stent implantation, (v) is the suturing of the medial collateral ligament and the closing of the knee joint capsule, (vi) is the suturing of skin tissue and fascia tissue, and b is the gross observation diagram of the femoral condyle (FC), tibial plateau (TP) and meniscus substitute at 4 and 12 weeks after surgery, and the scale is 5 mm.
[0039] Fig.12 These are the staining pictures of the femoral condyle (FC) and tibial plateau (TP) 4 and 12 weeks after implantation of the 3D printed meniscus substitute in the present invention in a rabbit model, wherein hematoxylin-eosin is the H&E staining picture, and safranin O-fast green is the SOFG staining picture.
[0040] Fig.13 This is a bar graph (1) showing the results of evaluating the degree of cartilage degeneration using the Osteoarthritis Research Institute International (OARSI) score in the present invention.
[0041] Fig.14 This is a bar graph (2) showing the results of evaluating the degree of cartilage degeneration using the Osteoarthritis Research Institute International (OARSI) score in the present invention. DETAILED DESCRIPTION
[0042] The technical solution of the present invention is further described below through specific embodiments.
[0043] Example 1
[0044] Step 1, N-methyldiethanolamine (5.96g, 50mmol), 1,3-propane sultone (6.70g, 55mmol) and dichloromethane (200mL) were added to a 500mL round-bottom flask. The mixture was stirred in an oil bath at 40°C for 24 hours at 400rpm under a nitrogen atmosphere. Then, the reactant solution was rotated to about 25mL using a rotary evaporator. The remaining solution was precipitated with acetone at a ratio of 1:20, and then washed three times with acetone to obtain a white powder. Finally, the product was dried in a vacuum oven and weighed. Weigh 1g of polyhexamethylene carbonate diol (Mn~2000) and 0.121g of MeSB-diol, add them to a 100mL three-necked flask, assemble a mechanical stirring device and simply seal the interface with plastic wrap, then place it in a 120°C oil bath pot for vacuum drying for 1 hour to remove moisture from the raw materials and avoid violent polymerization during the prepolymerization stage. After the temperature was lowered to 80°C, 0.504g of hexamethylene diisocyanate (HDI) was weighed in a 10mL centrifuge tube, and 6mL of dimethyl sulfoxide (DMSO) solvent and a few drops of 2-ethylhexanoic acid stannous catalyst were added thereto in turn. After mixing evenly, the mixture was added dropwise to a three-necked flask for prepolymerization for 1 hour. The temperature was lowered to 40°C, 0.369g of adipic acid dihydrazide (ADH) chain extender was weighed and dissolved in 20mL of DMSO solvent, and added dropwise to a three-necked flask twice for chain extension, and the "pole climbing" phenomenon was observed during the period. After that, the mixture was stirred overnight at 40°C, and the reaction was always carried out under a nitrogen atmosphere during the entire reaction process starting from the prepolymerization. After that, the reactants were added to ether in a ratio of 1:20 for precipitation, and the solid product obtained by precipitation was filtered, and washed with ether and pure water three times in turn, and then placed in a vacuum drying oven for drying, and finally a dry white product was obtained, which was named PCU-MeSB. A polyurethane control group with the same soft and hard segment contents was prepared by the same method and named PCU.
[0045] Example 2
[0046] Step 1, N-methyldiethanolamine (5.96g, 50mmol), 1,3-propane sultone (6.70g, 55mmol) and dichloromethane (200mL) were added to a 500mL round-bottom flask. The mixture was stirred at 400rpm in an oil bath at 40°C for 24 hours under a nitrogen atmosphere. Then, the reactant solution was rotated to about 25mL using a rotary evaporator. The remaining solution was precipitated with acetone at a ratio of 1:20, and then washed three times with acetone to obtain a white powder. Finally, the product was dried in a vacuum oven and weighed. Weigh 1g of polyhexamethylene carbonate diol (Mn~2000) and 0.121g of MeSB-diol, add them to a 100mL three-necked flask, assemble a mechanical stirring device and simply seal the interface with plastic wrap, then place it in a 120°C oil bath pot for vacuum drying for 1 hour to remove moisture from the raw materials and avoid violent polymerization during the prepolymerization stage. After the temperature was lowered to 80°C, 0.504g of hexamethylene diisocyanate (HDI) was weighed in a 10mL centrifuge tube, and 6mL of dimethyl sulfoxide (DMSO) solvent and a few drops of 2-ethylhexanoic acid stannous catalyst were added thereto in turn. After mixing evenly, the mixture was added dropwise to a three-necked flask for prepolymerization for 1 hour. The temperature was lowered to 40°C, 0.369g of adipic acid dihydrazide (ADH) chain extender was weighed and dissolved in 20mL of DMSO solvent, and added dropwise to a three-necked flask twice for chain extension, and the "pole climbing" phenomenon was observed during the period. After that, the mixture was stirred overnight at 40°C, and the reaction was always carried out under a nitrogen atmosphere during the entire reaction process starting from the prepolymerization. After that, the reactants were added to ether in a ratio of 1:20 for precipitation, and the solid product obtained by precipitation was filtered, and washed with ether and pure water three times in turn, and then placed in a vacuum drying oven for drying, and finally a dry white product was obtained, which was named PCU-MeSB. A polyurethane control group with the same soft and hard segment contents was prepared by the same method and named PCU.
[0047] Example 3
[0048] Step 1, N-methyldiethanolamine (5.96g, 50mmol), 1,3-propane sultone (6.70g, 55mmol) and dichloromethane (200mL) were added to a 500mL round-bottom flask. The mixture was stirred at 400rpm in an oil bath at 40°C for 24 hours under a nitrogen atmosphere. Then, the reactant solution was rotated to about 25mL using a rotary evaporator. The remaining solution was precipitated with acetone at a ratio of 1:20, and then washed three times with acetone to obtain a white powder. Finally, the product was dried in a vacuum oven and weighed. Weigh 1g of polyhexamethylene carbonate diol (Mn~2000) and 0.121g of MeSB-diol, add them to a 100mL three-necked flask, assemble a mechanical stirring device and simply seal the interface with plastic wrap, then place it in a 120°C oil bath pot for vacuum drying for 1 hour to remove moisture from the raw materials and avoid violent polymerization during the prepolymerization stage. After the temperature was lowered to 80°C, 0.504g of hexamethylene diisocyanate (HDI) was weighed in a 10mL centrifuge tube, and 6mL of dimethyl sulfoxide (DMSO) solvent and a few drops of 2-ethylhexanoic acid stannous catalyst were added thereto in turn. After mixing evenly, the mixture was added dropwise to a three-necked flask for prepolymerization for 1 hour. The temperature was lowered to 40°C, 0.369g of adipic acid dihydrazide (ADH) chain extender was weighed and dissolved in 20mL of DMSO solvent, and added dropwise to a three-necked flask twice for chain extension, and the "pole climbing" phenomenon was observed during the period. After that, the mixture was stirred overnight at 40°C, and the reaction was always carried out under a nitrogen atmosphere during the entire reaction process starting from the prepolymerization. After that, the reactants were added to ether in a ratio of 1:20 for precipitation, and the solid product obtained by precipitation was filtered, and washed with ether and pure water three times in turn, and then placed in a vacuum drying oven for drying, and finally a dry white product was obtained, which was named PCU-MeSB. A polyurethane control group with the same soft and hard segment contents was prepared by the same method and named PCU.
[0049] When performing 3D printing, refer to 3D printing of lubricative stiff supramolecular polymer hydrogels for meniscus replacement, Biomater. Sci., 2021, 9, 5116–5126.
[0050] Mechanical properties test of 3D printed scaffolds (PCU and PCU-MeSB) for meniscus replacement: The prepared 3D printed scaffolds (PCU and PCU-MeSB) for meniscus replacement were tested using an electronic universal testing machine (Instron, USA): rectangular tensile specimens (length: 20 mm, width: 5 mm, thickness: 0.5 mm) and cylindrical compression specimens (diameter: 7 mm; height: 2 mm), tensile tests were performed at a strain rate of 50 mm / min, compression tests were performed at a strain rate of 10 mm / min, the maximum strain of the cyclic tensile loading-unloading experiment was fixed to 30%, the strain rate was 50 mm / min, the maximum strain of the cyclic compression loading-unloading experiment was fixed to 30%, the strain rate was 10 mm / min (i.e., the maximum strain of all cycles was fixed to 30%), and the tear test was performed using trouser-shaped specimens at a strain rate of 50 mm / min. For the tear test, the trouser-shaped PCU and PCU-MeSB printed specimens were used, the two legs were fixed on the tensile machine fixture, and the tension was performed at a loading rate of 50 mm / min. The tearing energy of the specimen is calculated as follows:
[0051]
[0052] Where F is the average load during the steady tearing process in N, and d is the thickness of the sample in mm.
[0053] (1) Figure 3 and Figure 4 The tensile mechanical properties of the printed structure were characterized. The 3D printed PCU-MeSB exhibited a tensile strength of 4.56±0.78MPa, a Young's modulus of 14.92±2.82MPa, an elongation at break of 694.01±209.61%, and a tensile strength of 23.48±10.02MJ·m -3 In contrast, the 3D printed PCU exhibited relatively poor mechanical properties (tensile strength of 1.38 ± 0.83 MPa, Young's modulus of 13.74 ± 5.38 MPa, elongation at break of 144.01 ± 87.35%, and toughness of 1.23 ± 0.92 MJ·m) due to the uneven filaments formed during the printing process and the large number of defects. -3 ), thus intuitively illustrating the comprehensive mechanical properties of the 3D printed PCU-MeSB structure, which can better meet the load-bearing requirements.
[0054] (2) Figure 5 —8, in order to further evaluate the fatigue resistance of 3D printed PCU-MeSB, 1000 cycles of cyclic tension and compression loading-unloading tests were performed without rest between two consecutive cycles. Figure 6 and 8 The dissipated energy is Figure 5 and7 The area enclosed by the corresponding stress-strain curve and the coordinate axes in the cyclic tensile and compressive loading-unloading process. During the cyclic tensile and compressive loading-unloading process, the ultimate stress and dissipated energy at 30% strain first decreased and then gradually stabilized. In addition, the stress-strain curve of 3D printed PCU-MeSB has good repeatability with the increase of the number of cycles. In the cyclic tensile test, the 3D printed PCU-MeSB achieved a maximum stress of 4.71MPa and a maximum energy of 588.72kJ·m in the first cycle. -3 The maximum dissipated energy of the steel sheet is 4.04 MPa and the dissipated energy is 174.38 kJ·m after 1000 cycles. -3 The above results indicate that part of the irreversible deformation occurred during the initial stretching process, in which energy dissipation dominated. In addition, similar results were observed in the cyclic compression test. The ultimate stress and dissipated energy of the 3D printed PCU-MeSB reached 8.00 MPa and 266.97 kJ·m after 1000 cycles, respectively. -3 . It is important to note that after 1000 cycles, the ultimate stress of 3D printed PCU-MeSB exceeds the initial stress value, which may be due to the volatilization of zwitterionic adsorbed water in PCU-MeSB during constant compression, resulting in stress increase. It is well known that a significant stress-strain hysteresis curve helps dissipate energy and resist changing loads; while low hysteresis and good fatigue resistance are more suitable for meniscus implants. (To illustrate that the printed PCU-MeSB exhibits excellent fatigue resistance).
[0055] (3) Poor tear resistance may limit the application of meniscus implants in vivo, because once cracks are formed during the implantation process, the implant will tear rapidly, eventually leading to the failure of the meniscus replacement implantation surgery. Fig. 9 As shown in Figure 2, the tearing energy of PCU-MeSB is as high as 12.51±1.57 kJ·m -2 , about PCU (1.81±0.2 kJ·m -2 ), indicating that the printed PCU-MeSB exhibits excellent tear resistance, indicating that the printed PCU-MeSB structure can withstand tearing and maintain its integrity after implantation.
[0056] Lubrication performance test of 3D printed brackets (PCU and PCU-MeSB) for meniscus replacement: The lubrication performance of 3D printed PCU-MeSB was tested by using the TRB ball-disc tribometer (CSM Tribometer). A stainless steel ball with a diameter of 6 mm was used as the friction pair. The sliding distance during the test was 10 mm and the test frequency was 1 Hz. The test temperature was 25 ° C, the test time was 300 s, the lubricant was water, and the friction coefficient was calculated by the system's own software.
[0057] Before the in vivo implantation experiments, the lubrication properties of the 3D printed PCU-MeSB were characterized by in vitro friction tests. Fig.10 As shown in the figure, the printed PCU-MeSB (COF = 0.13 ± 0.01) exhibits better lubricity than the printed PCU (COF = 0.39 ± 0.03), indicating that the printed PCU-MeSB has certain surface lubricity, indicating that the printed PCU-MeSB implants may have better cartilage protection in vivo. It should be noted that the COF of the printed PCU-MeSB is similar to the COF of porcine articular cartilage (0.11).
[0058] Animal experiment of 3D printed scaffolds (PCU and PCU-MeSB) implanted in rabbit model for meniscus replacement:
[0059] All procedures of animal experiments were performed in accordance with the guidelines of the Animal Experiment Management Committee of the Chinese Government. Animal experiments were approved by the Animal Ethics Committee of Tianjin Academy of Medical Sciences. Twenty-six male rabbits weighing 2.5-3.0 kg were used for experiments for 4 and 12 weeks. The experimental animals were randomly divided into 4 groups: sham operation group (2 rabbits at each time point), meniscectomy group (3 rabbits at each time point), PCU group (4 rabbits at each time point), and PCU-MeSB group (4 rabbits at each time point). Meniscus implants soaked in 75% ethanol were sterilized with ultraviolet light for 1 hour before surgery, and all surgeries were performed under sterile conditions. General anesthesia was given by injection of 10% chloral hydrate (3.5 mL / kg) into the rabbit ear vein before surgery, and local anesthesia was given by xylazine hydrochloride (0.2 mL / kg) during surgery. Then, the rabbits were fixed on the operating table, the leg hair was shaved, and disinfected with iodine. Then, the medial meniscus of both knees of the rabbits was completely removed. First, the skin tissue and fascia tissue were cut to form a 2-cm incision. Then the medial collateral ligament was cut to expose the posterior horn of the medial meniscus. Subsequently, the joint capsule tissue was opened, and the posterior and anterior horns of the meniscus were dissected along the junction of the medial meniscus and the tibial plateau with a pointed scalpel, and then the entire meniscus was removed. Next, the meniscus substitute of appropriate size was selected for implantation by gross observation during the operation. The PCU and PCU-MeSB meniscus implants were transplanted into the knee joint, and the anterior horn of the implant was sutured to the medial collateral ligament, and the posterior horn of the implant was sutured to the joint capsule tissue to fix the meniscus horizontally to the initial position of the medial meniscus of the knee joint. In comparison, only the meniscus was exposed as the sham operation group, and only the meniscectomy was performed as the meniscectomy group. After that, non-absorbable surgical sutures were used to connect the medial collateral ligament and close the joint capsule, suture the fascia tissue and skin tissue, and the surgical leg was cleaned with an alcohol cotton pad. Finally, all rabbits were injected with penicillin three days after surgery to prevent infection. After surgery, the rabbits were returned to the cage to ensure that all rabbits were free to move. Over the next period of time, the knee joint conditions and activities of the rabbits were observed and recorded. All rabbits were euthanized, and their femurs, tibiae, and meniscal implants were collected at 4 and 12 weeks after surgery. The femoral condyles (FCs), tibial plateaus (TPs), and meniscal substitutes of all rabbits were photographed and evaluated. The tissues were fixed in 4% paraformaldehyde for 3 days, and the corresponding distal femurs and proximal tibiae were decalcified in ethylenediaminetetraacetic acid (EDTA) solution (10%) for 28 days. Afterwards, all tissues were dehydrated using graded ethanol and embedded in paraffin. Finally, the obtained tissue sections were stained with hematoxylin-eosin (H&E) and safranin-fast green (SOFG) (thickness ~10μm). The above tissue sections were observed and photographed using an EVOS M500 inverted fluorescence microscope. The group with only exposed rabbit meniscus was set as the sham operation group, the group with only meniscectomy was set as the meniscectomy group, and the 3D printed meniscus scaffold (PCU and PCU-MeSB) group was the experimental group. Fig.12 As shown in Figure 2, the 3D printed meniscus scaffold (PCU-MeSB) group was significantly better than the other groups. According to the osteoarthritis research society international (OARSI) osteoarticular cartilage histopathological evaluation system, 4 researchers blindly reviewed and independently evaluated the cartilage degeneration of FC and TP. The higher the score, the worse the cartilage condition. Fig.13 As shown in Figure 14, the 3D printed meniscus scaffold (PCU-MeSB) group is significantly better than the other groups. Therefore, the PCU-MeSB of the present invention is used as a meniscus substitute material.
[0060] By adjusting the process parameters according to the content of the present invention, the preparation of modified polyurethane and 3D printed meniscus can be achieved. After testing, they all show performance basically consistent with the present invention. The above is an exemplary description of the present invention. It should be noted that without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be done by other technicians in this field without spending creative labor falls within the scope of protection of the present invention.
Claims
1. A modified polyurethane, It is characterized in that Follow the steps below: Step 1, uniformly dispersing zwitterionic diol, polyhexamethylene carbonate diol, and diisocyanate in an organic solvent, adding a catalyst for prepolymerization, wherein the mass ratio of polyhexamethylene carbonate diol, zwitterionic diol, and diisocyanate is 1: (0.1-0.3): (0.5-0.8), the prepolymerization temperature is 70-90 degrees Celsius, and the time is 1-3 hours; the molecular formula of zwitterionic diol is as follows: Step 2, after prepolymerization, the temperature of the reaction system is lowered to 40-50 degrees Celsius, and a chain extender adipic acid dihydrazide is added dropwise to the reaction system and kept warm for reaction to obtain a modified polyurethane; during the entire reaction process starting from the prepolymerization, the reaction is always carried out under an inert protective atmosphere, wherein the mass ratio of polyhexamethylene carbonate diol to adipic acid dihydrazide is 1:(0.3-0.5).
2. A modified polyurethane according to claim 1, It is characterized in that In step 1, the mass ratio of polyhexamethylene carbonate diol, zwitterionic diol and diisocyanate is 1:(0.1-0.2):(0.5-0.6); the diisocyanate is hexamethylene diisocyanate hard segment, and the number average molecular weight of polyhexamethylene carbonate diol is 1k-3k; the catalyst is stannous 2-ethylhexanoate, the organic solvent is dimethyl sulfoxide, dimethylformamide or dimethylacetamide, the prepolymerization temperature is 70-80 degrees Celsius, and the time is 1-2 hours.
3. A modified polyurethane according to claim 1, It is characterized in that In step 2, the same solvent as in step 1 is selected to evenly disperse the chain extender adipic acid dihydrazide, and then added dropwise to the reaction system in batches to carry out a chain extension reaction (the amount added in each batch is basically equal), and whether the "pole climbing" phenomenon occurs during the reaction; the inert protective atmosphere is nitrogen, helium or argon; the reaction temperature is 40-50 degrees Celsius, and the reaction time is 6-12 hours; the mass ratio of polyhexamethylene carbonate diol to adipic acid dihydrazide is 1:(0.3-0.4).
4. A method for preparing a modified polyurethane, It is characterized in that Follow the steps below: Step 1, uniformly dispersing zwitterionic diol, polyhexamethylene carbonate diol, and diisocyanate in an organic solvent, adding a catalyst for prepolymerization, wherein the mass ratio of polyhexamethylene carbonate diol, zwitterionic diol, and diisocyanate is 1: (0.1-0.3): (0.5-0.8), the prepolymerization temperature is 70-90 degrees Celsius, and the time is 1-3 hours; the molecular formula of zwitterionic diol is as follows: Step 2, after prepolymerization, the temperature of the reaction system is lowered to 40-50 degrees Celsius, and a chain extender adipic acid dihydrazide is added dropwise to the reaction system and kept warm for reaction to obtain a modified polyurethane; during the entire reaction process starting from the prepolymerization, the reaction is always carried out under an inert protective atmosphere, wherein the mass ratio of polyhexamethylene carbonate diol to adipic acid dihydrazide is 1:(0.3-0.5).
5. A method for preparing a modified polyurethane according to claim 4, It is characterized in that In step 1, the mass ratio of polyhexamethylene carbonate diol, zwitterionic diol and diisocyanate is 1:(0.1-0.2):(0.5-0.6); the diisocyanate is hexamethylene diisocyanate hard segment, and the number average molecular weight of polyhexamethylene carbonate diol is 1k-3k; the catalyst is stannous 2-ethylhexanoate, the organic solvent is dimethyl sulfoxide, dimethylformamide or dimethylacetamide, the prepolymerization temperature is 70-80 degrees Celsius, and the time is 1-2 hours.
6. A method for preparing a modified polyurethane according to claim 4, It is characterized in that In step 2, the inert protective atmosphere is nitrogen, helium or argon; the reaction temperature is 40-50 degrees Celsius, and the reaction time is 6-12 hours; the mass ratio of polyhexamethylene carbonate diol and adipic acid dihydrazide is 1:(0.3-0.4), and the same solvent as in step 1 is selected to evenly disperse the chain extender adipic acid dihydrazide, and then added dropwise to the reaction system in batches to carry out a chain extension reaction (the amount added in each batch is basically equal), and whether the "pole climbing" phenomenon occurs during the process is observed.
7. Use of a modified polyurethane as claimed in any one of claims 1 to 3 in the preparation of meniscus substitute materials.
8. Use of the modified polyurethane according to claim 7 in preparing a meniscus substitute material, It is characterized in that The modified polyurethane is 3D printed by a biological 3D printer, the modified polyurethane material is added to the high-temperature barrel of the printer, the temperature is raised to 180-220°C, and the temperature is kept for a period of time, such as 10-20 minutes, and the printing parameters are set for continuous printing; the extruded microfibers are deposited on a printing platform at 35-45°C; after the printing is completed, the printed product is immersed in a PBS buffer solution until swelling equilibrium is reached to obtain a 3D printed PCU-MeSB scaffold with a specific shape.
9. Use of the modified polyurethane according to claim 8 in preparing a meniscus substitute material, It is characterized in that The printing mode is linear filling mode, the printing speed is 6-10mm / s, and the wire output speed is 0.05-0.15mm / s; the design system architecture is constructed by layer-by-layer stacking method.
10. Use of the modified polyurethane according to claim 7 in preparing a meniscus substitute material, It is characterized in that The Young's modulus of the 3D printed structure for meniscus replacement is 14.92±2.82MPa; the compression modulus is 22.08±4.31MPa; and the toughness is 23.48±10.02MJ / m 3 .
Citation Information
Patent Citations
Zwitterionic polyester diol and preparation method thereof
CN104262597A
Preparation method of zwitterionic waterborne polyurethane
CN104371085A
A method for preparing a super-tough polyurethane crosslinked network
CN114933723A
Preparation method and application of high-performance polyurethane
CN115636919A