Special high-toughness easy-to-form hot work die steel for additive manufacturing and manufacturing method thereof

By optimizing the alloy composition and heat treatment process in the mold steel, the problems of uneven temperature distribution and insufficient toughness in traditional mold manufacturing are solved, high-quality forming and damage repair of large-sized complex structural parts are achieved, the life of the mold is extended and the cost is reduced. cost.

CN118792591APending Publication Date: 2024-10-18SUZHOU JUNJING METAL TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411181506.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

There are problems with uneven temperature distribution, cracking and metallurgical defects in traditional mold manufacturing. Especially during the forming and damage repair process of large-scale complex structural parts in the additive manufacturing process, the toughness of traditional hot work mold steel is insufficient, resulting in a high risk of cracking. And the cost is higher.

Method used

Hot work die steel with alloy composition C0.03-0.3%, Ni 15-21%, Mo 4-8%, Co 6-10%, Ti 0.5-2% is used, and repaired by selective laser melting and laser cladding Technology, combined with a three-stage heat treatment process, improves the toughness and strength of the material.

Benefits of technology

It achieves high-quality forming of large-sized complex structural parts and precise repair of damaged parts, extends the service life of the mold, reduces costs, and improves the toughness and strength of the material, making it suitable for high-temperature service environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118792591A_ABST
    Figure CN118792591A_ABST
Patent Text Reader

Abstract

The invention provides special high-toughness easy-to-form hot work die steel for additive manufacturing, the alloy components of the hot work die steel comprise the following elements in percentage by mass: 0.03-0.3% of C, 15-21% of Ni, 4-8% of Mo, 6-10% of Co, 0.5-2% of Ti and the balance of Fe and inevitable impurity elements, the impurity elements comprise less than or equal to 0.015% of P and less than or equal to 0.003% of S; wherein the sum of the mass percentages of Ni and Mo is not greater than 25%; the ratio of the mass percent of Co to the sum of the mass percent of Ni and Mo is not less than 0.35. Meanwhile, the invention further discloses an additive manufacturing method of the high-toughness easy-to-form hot work die steel, according to the method, a sedimentary state hot work die or a failure-repaired sedimentary state hot work die is obtained through selective laser melting forming, then heat treatment is matched to improve the strength and toughness of the sedimentary state hot work die, and the high-toughness easy-to-form hot work die steel is obtained. According to the method, additive manufacturing of the large-size hot-working die part with the complex shape and inner cavity structure can be achieved, and the damaged hot-working die part can be repaired in a high-quality mode through a laser cladding method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of metal additive manufacturing, and in particular relates to a high-toughness and easy-to-form hot-working die steel specially used for additive manufacturing and a manufacturing method thereof. Background Art

[0002] A mold is a metal mold that is used to repeatedly produce the same product through stamping, forging, casting, etc. Large, integrated, complex structural parts with high integration are playing an increasingly important role in the manufacturing of new energy vehicles, and molds, as the "mother of industry", are crucial to the manufacturing of these complex structural parts.

[0003] The drilling and inlaying methods commonly used in traditional mold manufacturing to process cooling channels in the mold cannot achieve the forming of molds with complex inner cavities. This traditional processing method can only introduce linear temperature control sites, and cannot achieve efficient control of mold temperature, resulting in uneven mold temperature distribution, which in turn introduces local cracking and metallurgical defects in the casting, and there are problems such as long mold opening cycle, low production capacity, and short mold life. Different from the spot cooling temperature control of traditional machined molds, by utilizing the near-net forming and high processing accuracy advantages of selective laser melting technology in additive manufacturing, conformal temperature control channels with complex shapes can be embedded inside the mold, thereby significantly improving the temperature control accuracy and efficiency of the mold, greatly improving the yield rate of alloy castings, and speeding up the production cycle of castings.

[0004] The mold gate and other parts are subjected to stronger heat and force during service, which is prone to local excessive wear or cracking. Spot repair of damaged parts of the mold after service can greatly increase the overall service life of the mold, which has very important economic value. When repairing parts through common repair technologies such as thermal spraying, spray welding, electroplating, and surface coating, there are often problems such as small repair size, limited repairable parts, and poor bonding strength between the repair layer and the component matrix. The laser cladding technology in additive manufacturing technology can be used to repair failed parts with high quality. It has the advantages of good metallurgical bonding, high forming accuracy, and a wide range of applications. It can achieve fast, accurate, and high-quality repair of damaged parts of large molds.

[0005] The above-mentioned metal additive manufacturing processes all have ultra-high temperature gradients and ultra-high cooling rates. Metal powders will produce large solidification shrinkage stresses during the rapid melting-solidification process. At the same time, the cold and hot shrinkage between different deposition layers will also cause large thermal stresses inside the formed parts. The above two types of stress are extremely sensitive to the C content in the alloy, and the C content of traditional hot working die steel (H13 steel, patent CN 105886933A, patent CN 109136765 A, patent CN 110172641 A) is usually above 0.3% by mass. Therefore, the additive manufacturing processability of traditional hot working die steel is poor, especially in the process of forming large-sized hot working dies with complex shapes and inner cavity structures through selective laser melting technology and repairing damaged parts through laser cladding. There is a great risk of cracking. At the same time, since the cost of hot working dies formed by additive manufacturing is significantly higher than that of traditional processing methods, it is necessary to optimize the performance of hot working die steel to extend its service life, so as to ensure the economic applicability of hot working dies for additive manufacturing. It should be pointed out that toughness is a very important performance indicator of hot working dies and is closely related to their life. Hot working dies are subjected to complex stresses such as impact and vibration during service. Heavy-loaded dies often suffer from various forms of damage such as cracking and chipping due to insufficient toughness.

[0006] Therefore, it is very necessary to design a high-toughness and easy-to-form hot working die steel specifically for additive manufacturing. Summary of the invention

[0007] The technical problem to be solved by the present invention is that in view of the deficiencies of the above-mentioned prior art, a high-toughness and easy-to-form hot working die steel specially used for additive manufacturing and a manufacturing method thereof are provided. The method realizes the manufacture of high-toughness and easy-to-form hot working die steel, that is, solves the problem of a large risk of cracking in the process of forming large-sized hot working dies with complex shapes and internal cavity structures by selective laser melting technology and repairing damaged parts by laser cladding, and can realize high-quality laser cladding repair.

[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is: a high-toughness and easy-to-form hot working die steel specially used for additive manufacturing, characterized in that the alloy composition of the hot working die steel is composed of the following elements in mass percentage: C 0.03-0.3%, Ni 15-21%, Mo 4-8%, Co 6-10%, Ti 0.5-2%, and the balance is Fe and unavoidable impurity elements, and P ≤ 0.015% and S ≤ 0.003% among the impurity elements;

[0009] Wherein, the sum of the mass percentages of Ni and Mo is not greater than 25%;

[0010] The ratio of the mass percentage of Co to the sum of the mass percentages of Ni and Mo is not less than 0.35.

[0011] Preferably, C 0.1-0.2%.

[0012] Preferably, the sum of the mass percentages of Ni and Co is not less than 25%.

[0013] Preferably, the weight of the hot working die steel can reach 280 kg and the size can reach 350×350×350 mm.

[0014] At the same time, the present invention also provides an additive manufacturing method for the high-toughness and easy-to-form hot working die steel specially used for additive manufacturing, comprising the following steps:

[0015] Step 1: Selectively laser melt the powder of the hot working die steel to obtain a deposited hot working die, wherein the laser power of the selective laser melting is 300-380 W, the scanning speed is 0.7-1 m / s, the scanning spacing is 0.07-0.12 mm, the powder layer thickness is 0.03-0.08 mm, and the substrate preheating temperature is not less than 120 ° C;

[0016] Alternatively, the damaged parts of the failed hot working die are evaluated and removed by machining, and then a three-dimensional model of the area to be repaired is established and laser cladding repair is performed, wherein the laser power is 1600-2000W, the laser spot size is 3mm, the powder feeding amount is 5-15g / min, the laser scanning speed is 4-8mm / s, and the multi-pass overlap rate is 20-60%. After the repair is completed, the cladding area is further fine-machined to obtain a repaired deposited hot working die;

[0017] Step 2: heat-treating the deposited hot working mold or the repaired deposited hot working mold obtained in step 1 to improve its strength and toughness, and obtaining high-toughness and easy-to-form hot working die steel; the heat treatment is specifically as follows: first, the deposited hot working mold or the repaired deposited hot working mold is kept at 900-1000°C for 0.5-3h, and cooled to room temperature by oil cooling; then, it is kept at 620-720°C for 0.5-2h, and cooled to room temperature by air cooling; finally, it is kept at 450-480°C for 5-8h, and cooled to room temperature by furnace cooling.

[0018] Preferably, in the selective laser melting forming process of the hot working die steel powder in step one, the laser power is 350 W, the scanning speed is 0.9 m / s, the scanning spacing is 0.1 mm, the powder layer thickness is 0.05 mm, the substrate preheating temperature is 200°C, and the density of the deposited parts is not less than 99.5%.

[0019] Preferably, during the laser cladding repair of the failed hot working mold in step one, the laser power is 1800 W, the laser spot size is 3 mm, the powder feeding amount is 8 g / min, the laser scanning speed is 6 mm / s, the multi-pass overlap rate is 40%, and the porosity of the cladding layer is less than 2%.

[0020] Preferably, the deposited hot working mold or the repaired deposited hot working mold is first kept at 980-1000°C for 0.5-1h, and cooled to room temperature by oil cooling; then kept at 640-660°C for 0.5-1h, and cooled to room temperature by air cooling; finally kept at 450-460°C for 7-8h, and cooled to room temperature by furnace cooling.

[0021] Compared with the prior art, the present invention has the following advantages:

[0022] 1. The C in the alloy of the hot working die steel of the present invention is one of the most effective strengthening elements in steel materials. In the hot working die steel of the present invention, C can be combined with Ti and Mo elements to form MC and M2C carbides, thereby improving the hardness and strength of the material. However, a large number of experiments in the present invention have confirmed that when the mass percentage of C is higher than 0.3%, the risk of cracking of metal components during additive manufacturing will increase sharply, which is related to the greater brittleness of high-C martensite. Therefore, the C content of the hot working die steel in the present invention is controlled below 0.3% by mass, so that while achieving carbide strengthening of the matrix, ultra-low C lath martensite with good toughness is obtained, thereby ensuring the excellent additive manufacturing processability of the alloy.

[0023] The Ni element in the alloy can effectively reduce the C equivalent of the material, thereby improving the welding performance and additive manufacturing processability of the alloy, and then inhibiting the cracking problem caused by excessive thermal stress in the additive manufacturing process of the parts. In addition, Ni can form Ni3 (Mo, Ti) precipitation phase with Mo and Ti, thereby improving the strength of the alloy. Therefore, the addition of Ni is very necessary. Experimental verification shows that when the content of Ni is above 15% by mass, the above two effects can be better achieved. On the other hand, Ni is a strong austenite stabilizing element, which will greatly reduce the martensitic transformation temperature of the alloy. When the Ni content is too high, the parts will retain some residual austenite after quenching. These residual austenites are prone to coarsening during subsequent heat treatment, thereby deteriorating the strength and hardness of the material. Therefore, it is necessary to control the content of Ni in the alloy within the range of 15-22% by mass.

[0024] The Mo element in the alloy has a high solute distribution coefficient in the non-equilibrium solidification process, and the additive manufacturing process is an extremely non-equilibrium solidification process. Therefore, the Mo element in the additive component will form a serious element segregation between the primary dendrite arms of the matrix, and the overall distribution is in a network, which improves the stability of the austenite in the corresponding area. The present invention utilizes this characteristic of the Mo element and realizes the network distribution of the reverse transformation austenite by regulating the heat treatment system, thereby improving the toughness of the material. At the same time, when the temperature is kept at 450-480°C, the Mo element dissolved in the matrix will combine with Ni and C to form fine and dispersed Ni3Mo and Mo2C precipitation phases, which significantly improves the strength of the alloy. However, the Mo content will also affect the structure of the material after quenching. In order to obtain a fully martensitic structure after quenching, the Mo content is controlled within the range of 4-8% by mass according to the Schaeffler phase diagram, and further satisfies the mass percentage of (Ni+Mo) ≤25%.

[0025] The Co element in the alloy does not participate in the formation of the precipitate phase in the special steel for additive manufacturing of the present invention, but it will improve the nucleation efficiency of the Ni3 (Ti, Mo) precipitate phase during the heat treatment process, thereby promoting its distribution in the form of fine dispersed precipitates, which is helpful to improve the strength of the material. In addition, since the addition of elements such as C, Ni, and Mo will reduce the martensitic start transformation temperature (Ms point) of the material, if the Ms point is too low, a large amount of residual austenite will exist in the deposited material and it is difficult to eliminate it by heat treatment, thereby reducing the strength of the material. The addition of Co can increase the Ms point of the alloy. A mass fraction of 1% Co can increase the Ms point of the alloy by 10°C. In order to make the alloy have a higher Ms point, so as to obtain a full martensitic structure after quenching, after testing, the Co content in the present invention is controlled at 6-10% by mass percentage, and at the same time satisfies Co / (Ni+Mo)≥0.35, which has the best effect on the performance improvement of hot working die steel.

[0026] As a strong carbide-forming element, Ti in the alloy can combine with C to precipitate fine and dispersed MC-type carbides with good high-temperature stability through a suitable heat treatment process. The carbide is not easy to coarsen during service, and can effectively improve the strength and tempering resistance of the material. At the same time, Ti will also form a Ni3Ti precipitation phase with Ni in the matrix, further improving the strength of the material. Similar to the Mo element, the Ti element will also produce a network segregation during the additive manufacturing process, thereby improving the austenite stability in the corresponding area, and then inducing reverse transformation of austenite to be distributed in a network during the tempering process. It should be noted that if the Ti content is too high, it will increase the crack sensitivity of the steel, increase the brittle fracture tendency of the steel, and reduce the toughness of the material. Therefore, the Ti content in the present invention is controlled within the range of 0.5-2% by mass.

[0027] Based on the requirements of laser additive manufacturing process and laser cladding repair of hot working dies with large size, large weight, complex shape and inner cavity structure, the present invention not only considers the influence of alloy composition design on the performance of hot working die steel, but also considers the influence of additive manufacturing process, combines the previous theoretical analysis of alloy composition and some experiments, and obtains deposited samples with lower hardness and higher toughness by regulating alloy composition and additive manufacturing process, so as to ensure that large-size and heavy hot working dies will not crack due to excessive residual stress during additive manufacturing or laser cladding repair. On this basis, the mechanical properties are regulated by a three-stage heat treatment system to ensure its service performance as a hot working die: the first step is to obtain a full martensitic structure through high-temperature heat treatment, the second step is to introduce a network-distributed reverse transformation austenite through medium-temperature heat treatment, and the third step is to introduce a dispersed distribution of fine intermetallic compounds and carbide precipitation phases through low-temperature heat treatment. The first two heat treatments in the three-stage heat treatment system in the present invention are to obtain a network-distributed reverse transformation austenite, thereby improving the toughness of the alloy; the last heat treatment is to strengthen the precipitation of the phase, thereby improving the strength and hardness of the alloy. It is a well-known method to improve the performance of alloy heat treatment, but the alloy composition and alloy dosage have an important influence on the selection of heat treatment process. After theoretical analysis combined with experimental analysis, the specific process of heat treatment of the present invention is finally obtained: first, the deposited hot working mold or the repaired deposited hot working mold is kept at 900-1000℃ for 0.5-3h, and cooled to room temperature by oil cooling; then kept at 620-720℃ for 0.5-2h, and cooled to room temperature by air cooling; finally kept at 450-480℃ for 5-8h, and cooled to room temperature by furnace cooling. After three-stage heat treatment, the hardness of the material is ≥44HRC, the yield strength is ≥1380MPa, and the impact energy of the V-notch sample is ≥51J. At the same time, long-term heat treatment ensures that the material has high high-temperature organizational stability and excellent anti-tempering stability. After keeping at 600℃ for 100h, the Rockwell hardness is not less than 40HRC, which is very suitable for the long-term high-temperature service environment of the hot working mold.

[0028] 2. The deposited alloy material with low hardness and high toughness obtained by the present invention is an easy-to-form and high-toughness hot working die steel with additive manufacturing, which solves the problems of easy cracking of traditional hot working die steel during the additive manufacturing forming process and insufficient toughness during service. It provides high-performance materials for defect-free forming of large hot working dies and high-quality laser cladding repair of damaged parts of hot working dies. The size of the formable parts reaches 350×350×350mm, the weight of the formable parts reaches 280kg, and the formed parts have excellent performance, which are the best in the current field.

[0029] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 Solidification path of the hot working die steel in Example 1 obtained based on thermodynamic calculations.

[0031] Figure 2 SEM photograph of the original powder of hot working die steel in Example 1 of the present invention.

[0032] Figure 3 Optical micrographs of deposited samples obtained using different process parameters in Example 1 of the present invention.

[0033] Figure 4 Optical micrographs of the cladding layers obtained using different process parameters in Example 2 of the present invention.

[0034] Figure 5 Schematic diagram of the heat treatment process of the hot working die steel specially used for additive manufacturing of the present invention.

[0035] Figure 6 XRD diffraction patterns of the hot working die steel in the deposited state (a) and the HT-5 heat-treated state (b) in Example 4 of the present invention.

[0036] Figure 7 EBSD phase distribution diagram of HT-5 heat-treated mold steel (a) and conventional mold steel (b) as a comparative material in Example 4 of the present invention, wherein red represents martensite and green represents austenite.

[0037] Figure 8 TEM image and element distribution diagram at the same position of HT-5 heat-treated hot working die steel in Example 4 of the present invention.

[0038] Fig. 9 Engineering stress-strain curve of HT-5 heat-treated hot working die steel in Example 4 of the present invention.

[0039] Fig.10 Hardness changes of the heat-treated sample block and Dievar and H13 steels in Example 5 of the present invention when kept at 600°C.

[0040] Fig.11 The martensite-austenite transformation temperature of the heat-treated sample block in Example 5 of the present invention is tested at different heating rates.

[0041] Fig.12 A physical picture of an additively manufactured hot working die part made using the hot working die steel material of the present invention in Example 6 of the present invention.

[0042] Fig.13 Actual picture of the additively manufactured hot working die part made of traditional hot working die steel H13 in Example 6 of the present invention.

[0043] Fig.14Actual picture of a large-sized additively manufactured hot working die part made using the hot working die steel material of the present invention in Example 7 of the present invention.

[0044] Fig.15 A photo of the damaged mold part in Example 8 of the present invention (left) and a photo of the mold part after repair by laser cladding (right).

[0045] Fig.16 A physical picture of an additively manufactured hot working die part made of the hot working die steel material of the present invention in Comparative Example 4. DETAILED DESCRIPTION

[0046] Example 1

[0047] This embodiment provides a hot working die steel for additive manufacturing obtained based on thermodynamic calculations, and its alloy composition is shown in Table 1. Figure 1 The solidification path of the hot working die steel in Example 1 obtained based on thermodynamic calculations reflects the change in phase volume fraction during the additive manufacturing process.

[0048] Table 1 Chemical composition of initial powder of die steel in Example 1 (mass percentage)

[0049] Ni Co Mo Ti C Fe 15.6 8.7 5.5 1.6 0.06 Bal.

[0050] It is prepared into spherical powder for additive manufacturing through gas atomization powder making technology, and its morphology is as follows Figure 2 As shown in the figure, a sample forming experiment was carried out using a BLT-A320 selective laser melting device. The specific method is as follows: the powder of the hot working die steel was subjected to selective laser melting using a BLT-A320 selective laser melting device to obtain a deposited hot working die sample. The laser power of the selective laser melting was 320-380 W, the scanning speed was 0.8-1 m / s, the scanning spacing was 0.09-0.11 mm, the powder layer thickness was 0.04-0.05 mm, and the substrate preheating temperature was not less than 150 °C. A total of 16 groups of die steel sample tests prepared under different selective laser melting forming parameters were designed. The specific forming parameter tests are shown in Table 2.

[0051] To prevent oxidation of the metal powder after being melted by the laser, the entire forming process is carried out in a closed forming chamber under nitrogen protection. Figure 3The optical microscope photos of 16 groups of deposited samples are shown in Table 2. The density of the mold steel samples prepared by different process parameters is tested by the Archimedes drainage method. The results are shown in Table 2. It can be seen that the density of the samples prepared by the hot working die steel in Example 1 under the selected different selective laser melting forming parameters is above 99.5%, indicating that the mold steel has a large selective laser melting forming process window and is suitable for additive manufacturing. When the laser power, scanning speed, scanning spacing, powder layer thickness, and preheating temperature are 350W, 0.90m / s, 0.10mm, 0.05mm, and 200℃, respectively, the density of the formed sample is the highest, reaching 99.96%.

[0052] Table 2 Density of mold steel samples prepared under different selective laser melting forming parameters in Example 1

[0053]

[0054] Example 2

[0055] The present embodiment provides a method for manufacturing a deposited hot working die steel sample block, which comprises: using the hot working die steel powder in Table 3 to manufacture a deposited sample block by laser cladding, selecting different laser cladding parameters to prepare the deposited sample block, and designing a total of 12 groups of different laser cladding parameters, as shown in Table 4.

[0056] Table 3 Chemical composition of initial powder of die steel in Example 2 (mass percentage)

[0057] Ni Co Mo Ti C Fe 16.8 9.7 7.9 1.3 0.14 Bal.

[0058] Table 4 Porosity of cladding layer under different laser cladding parameters in Example 2

[0059]

[0060]

[0061] Figure 4 It is a light microscopic photograph of the deposited sample, which has no obvious metallurgical defects. The porosity of the sample made by each process parameter is statistically analyzed through the light microscopic photograph, and the results are shown in Table 4. It can be seen that the porosity of the cladding layer formed by the hot working die steel in Example 2 under the selected laser cladding forming parameters is less than 2%, indicating that the die steel has a large laser cladding forming process window and is suitable for additive manufacturing. Among them, when the laser power, scanning speed, powder feeding amount, and overlap rate are 1800W, 6mm / s, 8g / min, and 40% respectively, the porosity of the formed cladding layer is the lowest, only 0.65%.

[0062] Example 3

[0063] The optimal selective laser melting forming process in Example 1 was adopted (laser power of 350 W, scanning speed of 0.90 m / s, scanning spacing of 0.10 mm, powder layer thickness of 0.05 mm, substrate preheating temperature of 200 ° C), and powders of six mold steel alloy compositions (as shown in Table 5) were selected to prepare deposited hot working mold specimens, and the Archimedes drainage method was used to test the density of the deposited specimens. The results are shown in Table 5.

[0064] The best laser cladding process in Example 2 was adopted (laser power of 1800 W, scanning speed of 6 mm / s, powder feeding amount of 8 g / min, overlap rate of 40%), and powders of six mold steel alloy compositions (as shown in Table 5) were selected to prepare deposited hot working mold specimens. The porosity of the deposited specimens was statistically analyzed by optical microscope photographs. The results are shown in Table 5.

[0065] Table 5 Chemical composition (mass percentage) of hot working die steel in Example 3 and its

[0066] Density of Selective Laser Melting Samples and Porosity of Laser Cladding Samples

[0067]

[0068] From the data in Table 5, it can be seen that the density of the deposited samples made of each alloy is above 99.5%, and the porosity of the deposited samples made of each alloy is below 0.7%, which shows that the alloy composition is designed to manufacture hot working die steel with excellent additive manufacturing processability.

[0069] Example 4

[0070] This embodiment provides a heat treatment system for the selective laser melting formed sample block of the deposited sample block 5 manufactured in Example 3.

[0071] Table 6 Heat treatment schedule for the selected laser melting sample of Alloy 5 in Example 3

[0072]

[0073]

[0074] This embodiment adopts Figure 5 The three-stage heat treatment process shown in the figure is high temperature quenching, medium temperature tempering and low temperature tempering. The specific parameters are shown in Table 6. First, the intracellular Ac 1 The temperature is kept above 400 °C for a short time and then cooled by oil quenching to eliminate the residual austenite in the deposited structure and obtain a full martensite structure, while retaining the network segregation of solute elements such as Mo and Ti at the cell wall; then, Ac 1 Temperature and intracellular Ac 1Tempering is performed for a short time between the temperature and air cooling, thereby promoting the transformation of the cell wall structure into reverse austenite, and then constructing a network of austenite structures in the material to improve the impact toughness of the material; finally, at the cell wall element segregation Ac 1 Tempering for a long time below temperature and cooling with the furnace can promote the precipitation of the precipitated phase, thereby maximizing the hardness and strength of the material.

[0075] Figure 6 1 and 2 are XRD spectra of the deposited sample block 5 and the HT-5 heat-treated sample block 5. It can be seen that the deposited sample block 5 is a full martensite structure, and the heat-treated sample block 5 is a two-phase structure of martensite and austenite. Figure 7 The EBSD phase distribution diagram of the HT-5 heat-treated sample block, where (a) is the hot working die steel of this embodiment, and (b) is the comparison material traditional maraging steel 18Ni300. Figure 7 (a) with Figure 7 (b) It can be found that the austenite content in the HT-5 heat-treated hot working die steel in this embodiment is much higher than that in the comparative material. At the same time, the austenite in the comparative material is distributed in an island shape, while the austenite in the HT-5 heat-treated hot working die steel in this embodiment is distributed in a network shape. These network-distributed austenites have high toughness and can effectively promote stress homogenization during material deformation, thereby improving the material's plasticity and toughness retention ability. Figure 8 This is the TEM image of the HT-5 heat-treated hot working die steel in this embodiment. It can be found that a large number of Ti-rich and Mo-rich fine and uniform second phases are distributed in the matrix. These second phase particles can effectively hinder the dislocation movement during the deformation process of the material and improve the strength and hardness of the material.

[0076] The heat-treated hot working die steel in this embodiment was subjected to hardness test, tensile test and Charpy V-notch impact toughness test, and the results are shown in Table 7, wherein the comparison material Dievar alloy is a high-quality hot working die steel widely used on the market (its hardness and impact toughness data are quoted from the official website of Sweden ASSAB, and the strength data are from the actual measurement of the inventor), and the comparison material 18Ni300 is a hot working die steel widely studied in the field of additive manufacturing (its data are from the actual measurement of the inventor). Overall, the hardness of the hot working die steel in the present invention is ≥44HRC, which is equivalent to the comparison material; the yield strength is ≥1380MPa, which is equivalent to the comparison material; the impact toughness is ≥51J, which is much better than the comparison material. Among the five heat treatment systems in this embodiment, the HT-5 heat-treated material has the best comprehensive performance, with a hardness of 48HRC, a yield strength of 1431MPa, and an impact toughness of 56J. Fig. 9 This is the room temperature quasi-static uniaxial tensile curve.

[0077] Table 7 Comparison of room temperature mechanical properties of heat-treated hot working die steel in Example 4 and conventional hot working die steel

[0078] Sample No. Hardness (HRC) Yield strength (MPa) Impact toughness(J) HT-1 48 1442 53 HT-2 44 1380 57 HT-3 49 1392 51 HT-4 47 1387 52 HT-5 48 1431 56 Dievar 46 1330 25 18Ni300 44 1403 18

[0079] Example 5

[0080] This example provides an evaluation of the service behavior of the HT-5 heat-treated hot working die steel in Example 4. First, the tempering resistance of the hot working die steel of the present invention at 600°C was tested and compared with the high-quality hot working die steel Dievar and the traditional hot working die steel H13. The results are as follows: Fig.10 As shown. It can be seen that after the hot working die steel in the present invention is kept in a high temperature environment of 600°C for 100 hours, the hardness is still above 40HRC; in contrast, the hardness of the high-quality hot working die steel Dievar and the traditional hot working die steel H13 rapidly decays to about 35HRC after the same heat exposure. This result shows that the hot working die steel specially used for additive manufacturing proposed in the present invention has excellent tempering resistance and will not be excessively softened during high-temperature service. The martensite-austenite phase transition temperature of the hot working die steel of the present invention at different heating rates was then tested by a thermal expansion experiment. The results are shown in Fig.11 As shown. It can be seen that at all tested heating rates, the martensite-austenite phase transition temperature of the hot working die steel of the present invention is above 600°C, which indicates that the hot working die steel proposed in the present invention has good high-temperature structural stability and will not undergo martensite-austenite phase transition during high-temperature service. The above two results both show that the hot working die steel proposed in the present invention has good high-temperature service performance, which is beneficial to the performance maintenance and service life of the hot working die during service in a high-temperature environment.

[0081] Example 6

[0082] This embodiment provides an additive manufacturing method for hot working die steel with a complex structure, the method comprising:

[0083] Step 1: Selectively laser melt the hot working die steel powder of alloy composition 5 in Example 3 to obtain a deposited hot working die part, with a laser power of 350 W, a scanning speed of 0.90 m / s, a scanning spacing of 0.10 mm, a powder layer thickness of 0.05 mm, and a substrate preheating temperature of 200° C. A deposited hot working die part with a complex structure as shown in 12 is obtained, and it can be found that the surface of the formed part is intact without defects such as cracks and holes.

[0084] Step 2: heat-treat the deposited hot working mold parts to obtain parts whose mechanical properties meet the requirements for the use of the parts. The heat treatment process specifically adopts the specific process conditions of HT-5 in Example 4.

[0085] Comparative Example 1

[0086] In this comparative example, the alloy powder of hot working die steel H13 is used to form a deposited hot working die part by the selective laser melting forming method disclosed in Example 6, such as Fig.13 As shown in the dotted red circle in the figure, there is obvious cracking on the surface of the formed part, which almost runs through the entire part, and it cannot meet the use requirements. Therefore, compared with the methods of Example 6 and Comparative Example 1, the hot working die steel proposed in the present invention has excellent additive manufacturing processability and can achieve defect-free additive manufacturing of mold parts.

[0087] Example 7

[0088] This embodiment provides an additive manufacturing method for large-size and heavy-weight hot-working die steel, the method comprising:

[0089] Step 1: Use the hot working die steel powder of the alloy composition of Alloy 5 in Example 3 to perform selective laser melting to obtain a deposited hot working die part. The laser power is 350W, the scanning speed is 0.90m / s, the scanning spacing is 0.10mm, the powder layer thickness is 0.05mm, and the substrate preheating temperature is 200℃. The weight of the obtained deposited hot working die part is as high as 280kg, the size is about 350×350×350mm, and the conformal temperature control water channel is embedded. Fig.14 As shown in the figure, it can be seen that the surface of the large-sized hot working die parts is good without defects such as cracks and holes. This result shows that the hot working die steel proposed in the present invention has excellent additive manufacturing processability and can realize defect-free additive manufacturing of large-sized and heavy molds.

[0090] Step 2: heat-treat the deposited hot working mold parts to obtain parts whose mechanical properties meet the requirements for the use of the parts. The heat treatment process specifically adopts the specific process conditions of HT-5 in Example 4.

[0091] Example 8

[0092] This embodiment provides an additive manufacturing method for a damaged mold part, the method comprising:

[0093] Step 1: Use hot working die steel powder with the alloy composition of Alloy 5 in Example 3 to evaluate the surface of the damaged die parts and remove them by machining. Then, establish a three-dimensional model of the area to be repaired and perform laser cladding repair. The laser cladding process parameters are: laser power of 1800 W, scanning speed of 6 mm / s, powder feeding amount of 8 g / min, and overlap rate of 40%. Fig.15 (a) is a photo of a damaged mold part, showing obvious material loss on its surface after high-temperature service. Fig.15(b) is a photo of a part after laser cladding repair and polishing using Alloy 5 in Example 3. The surface of the repaired part is intact and has no visible defects. This shows that the alloy composition provided by the present invention has excellent additive manufacturing processability and can achieve high-quality laser cladding repair of failed mold parts.

[0094] It should be noted that the alloy composition of the damaged mold part and the repaired hot-working mold steel manufactured by additive manufacturing in the present invention does not have to be consistent.

[0095] Comparative Example 2

[0096] This comparative example provides 4 kinds of comparative materials of hot working die steel, and its alloy composition is shown in Table 8. This is only part of the inventor's many comparative experiments, and does not mean that the inventor has only made these 4 comparative materials (comparative alloys 1-4 respectively). Adopting the best process parameters in Example 1 (laser power is 350W, scanning speed is 0.90m / s, scanning spacing is 0.10mm, powder layer thickness is 0.05mm, substrate preheating temperature is 200℃), using 4 kinds of comparative materials for selective laser melting forming, using Archimedes drainage method to test the density of deposited sample blocks, the results are shown in Table 8, the deposited density of each alloy is below 99%. Adopting the best process parameters in Example 2 (laser power is 1800W, scanning speed is 6mm / s, powder feeding amount is 8g / min, overlap rate is 40%), laser cladding forming is performed on 4 kinds of comparative materials, and the porosity of deposited sample blocks is statistically analyzed by optical microscope photos. The results are shown in Table 8, and the deposited porosity of each alloy is above 2%. The above results show that compared with the hot working die steel specially used for additive manufacturing provided by the present invention, the additive manufacturing processability of the four comparative materials in this comparative example is poor.

[0097] Table 8 Chemical composition (mass percentage) of hot working die steel in comparative example 2 and density (%) of selected laser melting sample and porosity (%) of laser cladding forming sample

[0098] Element Ni Co Mo Ti C Fe Density Porosity Comparison alloy 1 16.5 7.8 5.6 1.5 0.37 Bal. 97.13 3.77 Comparison Alloy 2 14.2 6.8 5.7 1.8 0.21 Bal. 98.32 3.13 Comparison Alloy 3 20.8 4.6 8.8 0.7 0.11 Bal. 98.54 2.88 Comparison Alloy 4 21.2 5.8 8.6 1.2 0.35 Bal. 97.65 3.78

[0099] Comparative Example 3

[0100] This comparative example provides eight selective laser melting forming processes for alloy 5 in Example 3, and the selected additive manufacturing forming parameters are shown in Table 9. Only some comparative experiments on laser melting forming process by the inventors are shown, and the density of the deposited sample block is tested by Archimedes drainage method. The results are shown in Table 9. The deposited density of each alloy is below 99%, among which the density of the sample block prepared by process parameter #4 is only 94.33%. This result shows that the selective laser melting process parameters in this comparative example cannot achieve high-quality forming of the hot working die steel for additive manufacturing of the present invention.

[0101] Table 9 Density of mold steel samples prepared under different selective laser melting forming parameters in comparative example 3

[0102]

[0103]

[0104] Comparative Example 4

[0105] This comparative example provides an additive manufacturing method for hot working die parts, the method comprising:

[0106] Step 1: Use the hot working die steel powder with the alloy composition of Alloy 5 in Example 3 to perform selective laser melting to obtain deposited hot working die parts, with a laser power of 350 W, a scanning speed of 0.90 m / s, a scanning spacing of 0.10 mm, a powder layer thickness of 0.05 mm, and a substrate preheating temperature of 200°C.

[0107] Step 2: The deposited hot working mold parts are heat treated under various conditions. Five heat treatment processes are selected to illustrate that the heat treatment process is crucial to the manufacturing of hot working mold parts. The parameters of the five heat treatment processes are shown in Table 10.

[0108] Table 10 Heat treatment system of laser melting formed samples in selected area of ​​comparative example 4

[0109]

[0110] The heat-treated hot working die steel in this comparative example was subjected to hardness test, tensile test and Charpy V-notch impact toughness test, and the results are shown in Table 11. In general, after heat treatment of the hot working die steel for additive manufacturing provided by the present invention using the heat treatment parameters in this comparative example, the comprehensive performance of the material is poor, especially the impact toughness, which is below 25 J, far lower than the heat-treated performance of the hot working die steel in Example 4, and is not suitable for the long-term high and low temperature cold and hot cycle service performance of the mold.

[0111] Table 11 Comparison of room temperature mechanical properties of heat-treated hot working die steel in comparative example 4 and conventional hot working die steel

[0112] Sample No. Hardness (HRC) Yield strength (MPa) Impact toughness(J) HT-1 56 1252 17 HT-2 52 1420 14 HT-3 53 1334 23 HT-4 38 1189 21 HT-5 41 1431 19

[0113] Comparative Example 5

[0114] This comparative example is an additive manufacturing method for mold parts, and the method comprises:

[0115] Step 1: Use the hot working die steel powder with the alloy composition of Alloy 5 in Example 3 to perform selective laser melting to obtain a deposited hot working die part, with a laser power of 400 W, a scanning speed of 1.0 m / s, a scanning spacing of 0.10 mm, a powder layer thickness of 0.10 mm, and a substrate preheating temperature of 100°C. Fig.16 This is a photo of the hot working die part manufactured by additive manufacturing in this comparative example. As shown by the dotted red circle in the figure, there is obvious cracking on the surface of the formed part, which almost runs through the entire part. This result shows that the selective laser melting process parameters in this comparative example will introduce fatal defects in the formed part and are not suitable for the selective laser melting forming of the hot working die steel of the present invention.

[0116] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A high-toughness and easy-to-form hot-working die steel specially designed for additive manufacturing. It is characterized in that The alloy composition of the hot working die steel is composed of the following elements in mass percentage: C 0.03-0.3%, Ni 15-21%, Mo 4-8%, Co 6-10%, Ti 0.5-2%, and the balance is Fe and unavoidable impurity elements, among which P ≤ 0.015%, S ≤ 0.003%; Wherein, the sum of the mass percentages of Ni and Mo is not greater than 25%; The ratio of the mass percentage of Co to the sum of the mass percentages of Ni and Mo is not less than 0.

35.

2. According to claim 1, a high-toughness and easy-to-form hot-working die steel specially used for additive manufacturing, It is characterized in that C0.1-0.2%。 3. The high-toughness and easy-to-form hot-working die steel specially used for additive manufacturing according to claim 2, It is characterized in that The sum of the mass percentages of Ni and Co is not less than 25%.

4. A high-toughness and easy-to-form hot-working die steel specially used for additive manufacturing according to claim 1 or 2, It is characterized in that The weight of the hot working die steel can reach 280kg and the size can reach 350×350×350mm.

5. An additive manufacturing method for the high-toughness and easy-to-form hot-working die steel specially used for additive manufacturing as claimed in any one of claims 1 to 4, It is characterized in that The following steps are involved: Step 1: Selectively laser melt the powder of the hot working die steel to obtain a deposited hot working die, wherein the laser power of the selective laser melting is 300-380 W, the scanning speed is 0.7-1 m / s, the scanning spacing is 0.07-0.12 mm, the powder layer thickness is 0.03-0.08 mm, and the substrate preheating temperature is not less than 120 ° C; Alternatively, the damaged parts of the failed hot working die are evaluated and removed by machining, and then a three-dimensional model of the area to be repaired is established and laser cladding repair is performed, wherein the laser power is 1600-2000W, the laser spot size is 3mm, the powder feeding amount is 5-15g / min, the laser scanning speed is 4-8mm / s, and the multi-pass overlap rate is 20-60%. After the repair is completed, the cladding area is further fine-machined to obtain a repaired deposited hot working die; Step 2: heat-treating the deposited hot working mold or the repaired deposited hot working mold obtained in step 1 to improve its strength and toughness, and obtaining high-toughness and easy-to-form hot working die steel; the heat treatment is specifically as follows: first, the deposited hot working mold or the repaired deposited hot working mold is kept at 900-1000°C for 0.5-3h, and cooled to room temperature by oil cooling; then, it is kept at 620-720°C for 0.5-2h, and cooled to room temperature by air cooling; finally, it is kept at 450-480°C for 5-8h, and cooled to room temperature by furnace cooling.

6. The additive manufacturing method according to claim 5, It is characterized in that In the selective laser melting process of the hot working die steel powder in step 1, the laser power is 350W, the scanning speed is 0.9m / s, the scanning spacing is 0.1mm, the powder layer thickness is 0.05mm, the substrate preheating temperature is 200°C, and the density of the deposited parts is not less than 99.5%.

7. The additive manufacturing method according to claim 5, It is characterized in that In step 1, when the failed hot working mold is repaired by laser cladding, the laser power is 1800 W, the laser spot size is 3 mm, the powder feeding amount is 8 g / min, the laser scanning speed is 6 mm / s, the multi-pass overlap rate is 40%, and the porosity of the cladding layer is less than 2%.

8. The additive manufacturing method according to claim 5, It is characterized in that The heat treatment in step 2 is specifically as follows: first, the deposited hot working mold or the repaired deposited hot working mold is kept at 980-1000°C for 0.5-1h, and cooled to room temperature by oil cooling; then, it is kept at 640-660°C for 0.5-1h, and cooled to room temperature by air cooling; finally, it is kept at 450-460°C for 7-8h, and cooled to room temperature by furnace cooling.

Citation Information

Cited By

  • High-thermal-conductivity die-casting die additive manufacturing metal powder and preparation method

    CN121109871A

  • Low-crack-sensitivity high-thermal-conductivity die-casting die additive manufacturing metal powder and preparation method

    CN121109872A